A dual-curing hardening coating, its preparation method and application
By using a dual-curing resin system that combines thermosetting and photocuring, the problems of increased brittleness and insufficient weather resistance of surface hardened coatings on polycarbonate materials have been solved, achieving a balance of high hardness, wear resistance and high toughness, and improving the impact performance and adhesion stability of the substrate.
Patent Information
- Application Number
- CN202611176689.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2026-07-09
- Filing Date
- 2026-08-05
- Publication Date
- 2026-11-17
AI Technical Summary
In the prior art, the surface hardening coating of polycarbonate materials can easily lead to increased brittleness when improving hardness and wear resistance, affecting the notched impact performance of the substrate, and has insufficient resistance to yellowing and adhesion stability when used outdoors.
A dual-curing resin system is adopted, which combines thermosetting and photocuring. Components such as polyurethane-modified acrylate, silicone-modified acrylate, polycarbonate polyol and hydroxyl acrylic acid are used to construct a cross-linking network to achieve a balance between high hardness, wear resistance and high toughness.
While ensuring high hardness and wear resistance, it reduces the risk of coating brittleness, improves the impact performance and weather resistance of the substrate, and maintains the adhesion stability of the coating.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polycarbonate curing coating technology, and specifically relates to a dual-curing curing coating, its preparation method, and its application. Background Technology
[0002] Polycarbonate (PC) materials are widely used in architectural lighting, automotive parts, electronics, display protection, and optical transparent components due to their excellent transparency, impact resistance, weather resistance, and processing performance. However, PC materials themselves have relatively low surface hardness and insufficient scratch resistance, abrasion resistance, and chemical resistance. Over long-term use, they are prone to surface wear, scratches, loss of gloss, and even degradation of optical performance. Therefore, a hardened protective coating is usually applied to their surface. Among existing surface hardening treatment solutions for PC and other transparent plastic substrates, UV-cured hard coatings are widely used due to their fast curing speed and high efficiency.
[0003] In the prior art, several patents have focused on UV hard coatings for plastic substrates. For example, patent CN103740265A discloses a UV-curable coating for hardening plastic surfaces, which uses various polyurethane acrylates, reactive diluent monomers, photoinitiators, and organic solvents, emphasizing workability, hardness, abrasion resistance, and mechanical properties. Patent CN102040903A discloses a UV-curable hard coating resin composition, focusing on achieving high hardness, adhesion, transparency, stain resistance, and tensile strength. Patent CN104937052A discloses a radiation-cured hard coating with improved weather resistance, emphasizing abrasion resistance, good adhesion to the substrate, resistance to microcracks, resistance to turbidity, and resistance to yellowing and other forms of discoloration. These solutions demonstrate that the prior art recognizes that transparent plastic hard coatings need to balance multiple properties such as hardness, abrasion resistance, adhesion, and weather resistance.
[0004] In addition, some patents have proposed a dual-curing approach. For example, patent CN102181192A discloses a dual-curing coating that improves the chemical corrosion resistance, abrasion resistance, high temperature resistance, flexibility, and adhesion of the coating film by combining thermosetting and photosetting. Patent CN108699212A discloses a dual-curing coating composition containing free radical curable olefinic unsaturated compounds, polyols, and polyisocyanates, and allows the use of polycarbonate polyols and (meth)acrylates containing hydroxyl reactive functional groups.
[0005] However, based on the aforementioned publicly available technology, existing UV hard coating solutions primarily focus on achieving high hardness, abrasion resistance, and transparency through high-functionality acrylate systems. Dual-curing solutions, on the other hand, tend to favor general-purpose coating systems or other surface effect systems, rather than specifically addressing the performance balance issues in the hardening and protection of polycarbonate transparent substrates. For PC substrates, simply increasing the crosslinking density, while beneficial for improving surface hardness and abrasion resistance, often leads to increased coating brittleness, decreased crack resistance, and may affect the notched impact resistance of the substrate due to interfacial stress concentration. Simultaneously, under outdoor or long-term service conditions, the coating also needs to consider resistance to yellowing, weathering, and adhesion stability.
[0006] Therefore, it is still necessary to develop a dual-curing hardening coating suitable for polycarbonate substrate surfaces. Summary of the Invention
[0007] The purpose of this invention is to provide a dual-curing hardening coating, its preparation method, and its application. By using a dual-curing resin for segmented curing, high hardness, high weather resistance, and high tensile toughness are achieved without affecting the notched impact resistance of polycarbonate and the brittleness of the coating, thus solving the problems mentioned in the background art.
[0008] This invention provides a dual-curing hardening coating, comprising the following components by weight: 20-40 parts of polyurethane-modified acrylate; 5-20 parts of silicone-modified acrylate; 5-15 parts of polycarbonate polyol; 5-15 parts of hydroxyacrylic acid; 10-30 parts of acrylic monomer; Catalyst 0.3-0.5 parts; 1-3 parts organic additives; Inorganic additives 1-5 parts; Initiator 0.5-2 parts; 2-4 parts of curing agent; Antioxidant 0.1-1 part; 0.5-3 parts UV agent; The rest are solvents; The polyurethane-modified acrylate is an aliphatic polyurethane-modified acrylate containing both hydroxyl and carbon-carbon double bonds, the curing agent is an isocyanate-based curing agent capable of crosslinking with hydroxyl groups, and the initiator is a photoinitiator capable of initiating the polymerization of acrylic double bonds.
[0009] Preferably, the polyurethane-modified acrylate is selected from A20, EBECRYL ®8210, B-6210, GU3064S, GM64U0G, EBECRYL ® 4900, EBECRYL ® 1205, EBECRYL ® One or more of 8209 and Sartomer-CN9062.
[0010] Preferably, the silicone-modified acrylate is selected from one or more of GU2800Z, GU2860Z, ShinEtsu-X48-1800, and DM528N.
[0011] Preferably, the polycarbonate polyol is selected from one or more of Desmophen C2102, Desmophen C2202, Desmophen C1100, Desmophen C1200, Duranol™ AKN11, UH50, UH200, and UHC50-200.
[0012] Preferably, the hydroxyacrylic acid is selected from 3208-6B, Uralac ® 7134 E-57, Urac ® 7110 X-70, BA-760, 3220070, Uralac ® One or more of 7133 and 3285-80.
[0013] Preferably, the acrylic monomer is selected from one or more of isobornyl acrylate (IBOA), methyl isobornyl acrylate (IBOMA), dicyclopentyl methacrylate (HDCPMA), tris(2-hydroxyethyl) isocyanurate triacrylate (THEICTA), dipentaerythritol hexaacrylate (DPHA), and pentaerythritol triacrylate (PETIA).
[0014] Preferably, the catalyst is selected from one or more of KOSMOST 12N, Borchi Kat21, and Borchi Kat22.
[0015] Preferably, the organic additive is selected from TEGO 100, BYK333, BYK065, BYK054, Wet 270, and Dynasylan. ® MEMO, Dynasylan ® One or more of GLYMO, Rad 2300, Rad 2500, and Rad 2700.
[0016] Preferably, the inorganic additive is selected from AEROSIL. ®R 9200, AEROSIL ® One or more of R 972, MEK-ST-40, C150, and C152.
[0017] Preferably, the initiator is selected from one or more of 2,4,6-trimethylbenzoyl diphenylphosphine oxide, 1-hydroxy-cyclohexyl-phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropanone, ethyl 2,4,6-trimethylbenzoyl phenylphosphonate, benzophenone, and methyl benzoylformate.
[0018] Preferably, the curing agent is selected from one or more of 3300, 1725, 120, 4470, N75, N100, NZ 300, and 3725.
[0019] Preferably, the antioxidant is selected from one or more of 1010, 1076, 1135, 168, and TP-10H.
[0020] Preferably, the UV agent is selected from one or more of UV400, UV1164, UV329, UV384-2, Chimassorb® 81, UV292, UV479, and Hostavin 3058 LIQ.
[0021] Preferably, the solvent is one of ethyl acetate, PMA, butyl acetate, MEK, MIBK, and BAC.
[0022] The present invention also provides a method for preparing a dual-curing hardening coating, comprising the following steps: S1. Mix polyurethane-modified acrylate, silicone-modified acrylate, polycarbonate polyol, hydroxy acrylic acid, acrylic monomer, antioxidant, UV agent, organic additives, inorganic additives, initiator and solvent, and stir evenly to obtain a premixed solution. S2. Add catalyst and curing agent to the premixed liquid, and continue to stir until uniform to obtain coating liquid; S3. Apply the coating liquid to the surface of the polycarbonate substrate; S4. The coated polycarbonate substrate is cured in stages, so that the system undergoes both thermo-curing and photo-curing reactions simultaneously to obtain a double-cured hardened coating.
[0023] Preferably, the coating method in step S3 is one of spraying, roller coating, curtain coating, dip coating, or scraping coating.
[0024] Preferably, the segmented curing in step S4 includes first thermal curing pre-curing and then light curing final curing; or first light curing pre-curing and then thermal curing final curing.
[0025] The present invention also provides an application of a dual-curing hardening coating in the surface hardening protection of polycarbonate substrates.
[0026] Preferably, the polycarbonate substrate is a polycarbonate sheet, a polycarbonate film, or a polycarbonate molded part.
[0027] Beneficial effects (1) This invention constructs a coating crosslinking network through a dual curing method, which can improve the toughness of the coating while ensuring high hardness, wear resistance and chemical resistance, and reduce the risk of coating brittleness and cracking. By combining photocuring and thermal curing, the resin system is cured in stages, avoiding the problem of increased brittleness caused by excessive crosslinking density in a single highly crosslinked acrylate system, so that the resulting hardened coating has both high surface hardness and good mechanical toughness.
[0028] (2) The present invention can effectively reduce the adverse effects of hardened coating on the impact performance of polycarbonate substrate and improve the compatibility between substrate and coating system. By introducing polyurethane modified acrylate, polycarbonate polyol and hydroxy acrylic acid into the system, the flexibility and stress buffering capacity of the coating are enhanced, and the stress concentration caused by excessive hardness and brittleness of the coating is reduced, which is conducive to maintaining the notched impact performance of polycarbonate substrate. Detailed Implementation
[0029] The present invention will be further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. Furthermore, it should be understood that after reading the teachings of this invention, those skilled in the art can make various alterations or modifications to the invention, and these equivalent forms also fall within the scope defined by the appended claims.
[0030] Table 1 Formulations for Examples 1-20 (by weight) Table 1 Explanation: Except for the changes in components and dosages listed in Table 1, the dosages of all other components remain the same, as detailed below: Catalyst: 0.4 parts; Organic additives: 1.2 parts; Inorganic additives: 2.5 parts; Initiator: 1.2 parts; Hardener: 3.0 parts; Antioxidant: 0.3 parts; UV agent: 1.3 parts; Remaining solvent.
[0031] Preferred raw material description: The polyurethane-modified acrylate is EBECRYL® 4900; The organosilicon-modified acrylate is GU2800Z; The polycarbonate polyol is Desmophen C2102; The hydroxyacrylic acid is Uralac® 7134 E-57; The acrylic monomer is a mixture of IBOA, HDCPMA and PETIA.
[0032] More preferably, the weight ratio of IBOA, HDCPMA, and PETIA in the acrylic monomers is 5:3:2.
[0033] Preferred formulation with fixed components: Catalyst: 0.4 parts Borchi Kat22; Organic additives: TEGO 100 0.4 parts, BYK333 0.3 parts, Wet 270 0.5 parts; Inorganic additives: 2.5 parts of AEROSIL® R 9200; Initiator: 0.6 parts 184, 0.6 parts TPO-L; Hardener: 3300 3.0 parts; Antioxidant: 1135 0.3 parts; UV agents: 0.9 parts UV400, 0.4 parts UV292; Solvent: Butyl acetate, PMA and MEK in a volume ratio of 9:8:8.
[0034] The preparation methods of Examples 1 to 20 are the same, the only difference being the amount of the main components listed in Table 1.
[0035] The preparation method includes the following steps: S1. Mix polyurethane-modified acrylate, silicone-modified acrylate, polycarbonate polyol, hydroxy acrylic acid, acrylic monomer, antioxidant, UV agent, organic additives, inorganic additives, initiator and solvent, and stir evenly to obtain a premixed solution. S2. Add catalyst and curing agent to the premixed liquid, and continue to stir until uniform to obtain coating liquid; S3. Apply the coating liquid to the surface of the polycarbonate substrate, and control the dry film thickness to be uniformly 10μm. S4. The coated polycarbonate substrate is cured in stages, so that the system undergoes both thermo-curing and photo-curing reactions simultaneously to obtain a double-cured hardened coating.
[0036] The segmented curing in step S4 includes either pre-curing with heat followed by final curing with light; or pre-curing with light followed by final curing with heat. The heat curing temperature is 80-120℃, and the time is 10-30 minutes; the light curing uses a mercury lamp with a total energy ≥2000 mJ / m². 2 .
[0037] Except for the variables listed in Table 1, the other components and their amounts remained consistent. Examples 1-4 were used to investigate the effect of polyurethane-modified acrylate dosage on the overall performance of the coating; Examples 5-8 were used to investigate the effect of silicone-modified acrylate dosage on weather resistance and surface properties; Examples 9-12 were used to investigate the effect of polycarbonate polyol dosage on coating toughness and impact retention of the polycarbonate substrate; Examples 13-16 were used to investigate the effect of hydroxyl acrylic acid dosage on system compatibility and flexibility; Examples 17-20 were used to investigate the effect of acrylic monomer dosage on coating hardness, abrasion resistance, and brittleness.
[0038] The following comparative examples use the basic formulation of Example 19 as a reference. Except for the changes listed in Table 2, the other components and their amounts remain the same. To ensure the workability of the system, the difference in the absence of a certain resin is preferably made up with acrylic monomer or solvent.
[0039] Table 2 Formulations for Comparative Examples 1–5 (by weight) Except for the changes in components and dosages listed in Table 2, the dosages of all other components remain the same, as detailed below: Catalyst: 0.4 parts; Organic additives: 1.2 parts; Inorganic additives: 2.5 parts; Initiator: 1.2 parts; Hardener: 3.0 parts; Antioxidant: 0.3 parts; UV agent: 1.3 parts; The remainder is solvent; In the comparative example, the acrylic monomers added are preferably still a mixture of IBOA, HDCPMA and PETIA, and the original ratio remains unchanged.
[0040] The coating performance test methods for the examples and comparative examples are shown below: Visible light transmittance and haze: GB / T2410-2008; Yellowing value: GB / T 39822-2021; Coating adhesion: ASTM D3359; Multiaxial impact: ISO 6272-2; Abrasion resistance (1000g, 1000 revolutions): ASTM D1044-19; Chemical resistance: GB / T 30648.1-2014; Xenon lamp aging: GB / T 16422.2-2014 Method A Cycle 1 standard.
[0041] Table 3. Coating Test Results of PC Sheets As shown in the table above, the dual-curing hardened coatings prepared in Examples 1-20 exhibit excellent hardness and wear resistance. After 8000 hours of xenon lamp aging, their performance remains largely unchanged. The coating and PC interface are firmly bonded without cracking, and they demonstrate excellent impact resistance. Comparative Examples 1-5 show that the overall performance of the coatings decreases to varying degrees when any key resin component is missing from the system. Specifically, without polyurethane-modified acrylate, the coating's toughness and crack resistance decrease; without silicone-modified acrylate, weather resistance, surface hardness, and wear resistance decrease; without polycarbonate polyol, the coating lacks flexibility and is detrimental to the impact resistance of the polycarbonate substrate; without hydroxyl acrylic acid, the system's compatibility and crosslinking balance are affected; and with both polyurethane-modified acrylate and hydroxyl acrylic acid absent, the dual-curing network is difficult to establish effectively, making the coating more prone to brittleness or cracking. This further demonstrates that the present invention, through the synergistic design of multiple resin components, achieves a good balance between high hardness, high weather resistance, and high toughness.
[0042] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.
[0043] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A dual-curing hardening coating, characterized in that, By weight, it includes the following components: 20-40 parts of polyurethane-modified acrylate; 5-20 parts of silicone-modified acrylate; 5-15 parts of polycarbonate polyol; 5-15 parts of hydroxyacrylic acid; 10-30 parts of acrylic monomer; Catalyst 0.3-0.5 parts; 1-3 parts organic additives; Inorganic additives 1-5 parts; Initiator 0.5-2 parts; 2-4 parts of curing agent; Antioxidant 0.1-1 part; 0.5-3 parts UV agent; The rest are solvents; The polyurethane-modified acrylate is an aliphatic polyurethane-modified acrylate containing both hydroxyl and carbon-carbon double bonds, the curing agent is an isocyanate-based curing agent capable of crosslinking with hydroxyl groups, and the initiator is a photoinitiator capable of initiating the polymerization of acrylic double bonds.
2. The dual-curing hardening coating according to claim 1, characterized in that, The polyurethane-modified acrylate is selected from A20 and EBECRYL. ® 8210, B-6210, GU3064S, GM64U0G, EBECRYL ® 4900, EBECRYL ® 1205, EBECRYL ® One or more of 8209 and Sartomer-CN9062.
3. The dual-curing hardening coating according to claim 1, characterized in that, The organosilicon-modified acrylate is selected from one or more of GU2800Z, GU2860Z, ShinEtsu-X48-1800, and DM 528N.
4. The dual-curing hardening coating according to claim 1, characterized in that, The polycarbonate polyol is selected from one or more of Desmophen C2102, Desmophen C2202, Desmophen C1100, Desmophen C1200, Duranol™ AKN11, UH50, UH200, and UHC50-200.
5. A dual-curing hardening coating according to claim 1, characterized in that, The hydroxyacrylic acid is selected from 3208-6B, Uralac ® 7134 E-57, Urac ® 7110 X-70, BA-760, 3220070, Uralac ® One or more of 7133 and 3285-80.
6. A dual-curing hardening coating according to claim 1, characterized in that, The acrylic monomer is selected from one or more of isobornyl acrylate, methyl isobornyl acrylate, dicyclopentyl methacrylate, tri(2-hydroxyethyl) isocyanurate triacrylate, dipentaerythritol hexaacrylate, and pentaerythritol triacrylate.
7. A dual-curing hardening coating according to claim 1, characterized in that, The catalyst is selected from one or more of KOSMOST 12N, Borchi Kat21, and Borchi Kat22.
8. A dual-curing hardening coating according to claim 1, characterized in that, The organic additives are selected from TEGO 100, BYK333, BYK065, BYK054, Wet 270, and Dynasylan. ® MEMO, Dynasylan ® One or more of GLYMO, Rad2300, Rad 2500, and Rad 2700; the inorganic additive is selected from AEROSIL. ® R 9200, AEROSIL ® One or more of R972, MEK-ST-40, C150, and C152.
9. A method for preparing a dual-curing hardening coating as described in any one of claims 1 to 8, characterized in that, Includes the following steps: S1. Mix polyurethane-modified acrylate, silicone-modified acrylate, polycarbonate polyol, hydroxy acrylic acid, acrylic monomer, antioxidant, UV agent, organic additives, inorganic additives, initiator and solvent, and stir evenly to obtain a premixed solution. S2. Add catalyst and curing agent to the premixed liquid, and continue to stir until uniform to obtain coating liquid; S3. Apply the coating liquid to the surface of the polycarbonate substrate; S4. The coated polycarbonate substrate is cured in stages, so that the system undergoes both thermo-curing and photo-curing reactions simultaneously to obtain a double-cured hardened coating.
10. The application of a dual-curing hardening coating as described in any one of claims 1 to 8 in the surface hardening protection of polycarbonate substrates.
Citation Information
Patent Citations
Uv curable resin composition for hard coat, and hard coated film and hard coated moldings using the same
CN102040903A
Dual-curing coating and preparation method thereof
CN102181192A
Ultraviolet curable coating for hardening treatment of plastic surfaces and preparation method of ultraviolet curable coating
CN103740265A
Radiation curable hardcoat with improved weatherability
CN104937052A
Dual cure soft touch coatings
CN108699212A