A low surface energy component self-replenishing anti-adhesion composite coating, its preparation method and application
By introducing dual-scale functionalized silica particles and polyether-modified silicone oil into a polyamide-imide matrix, a self-repairing anti-adhesion composite coating is constructed, which solves the problem of irreversible performance of existing coatings after wear, realizes the self-repair and long-term anti-adhesion performance of the coating, and is suitable for anti-adhesion treatment of various liquids.
Patent Information
- Application Number
- CN202611595488.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-15
- Publication Date
- 2026-11-17
AI Technical Summary
Existing anti-adhesion coatings cannot restore their anti-adhesion performance after wear, have poor durability and insufficient mechanical properties, and cannot effectively solve the problems of high cleaning and maintenance costs, material loss and low heat transfer efficiency caused by adhesion during the service of industrial equipment.
Using polyamide-imide (PAI) as the matrix, combined with dual-scale functionalized silica particles and polyether-modified silicone oil, a micro-nano-level rough structure is constructed. The coating stores polyether-modified silicone oil inside, which migrates and reconstructs a low surface energy interface when damaged, thus achieving self-replenishing anti-adhesion performance.
The coating can self-recover its anti-adhesion properties after wear, extending its service life, reducing the difficulty of cleaning and maintenance, and is suitable for anti-adhesion treatment of various liquids, improving the durability and ease of cleaning of equipment.
Smart Images

Figure CN123107536A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of functional protective coatings and surface engineering technology; in particular, it relates to a low surface energy component self-replenishing anti-adhesion composite coating, its preparation method and application. Background Technology
[0002] During service, industrial equipment, food processing equipment, chemical containers, pipelines, and mold components come into contact with water-based pollutants, oil, glue, and high-viscosity materials. Adhesion of viscous materials increases the cost of equipment cleaning and maintenance, causes material loss, reduces heat transfer efficiency, and leads to problems such as jamming, corrosion, and product quality decline. Developing long-lasting anti-adhesion functional surfaces has significant engineering value.
[0003] Existing anti-adhesion solutions fall into two categories: low surface energy coatings and micro / nano roughened super-wetting composite coatings. Simple low surface energy coatings suffer from poor mechanical properties and insufficient substrate adhesion. While constructing micro / nano roughened structures can reduce the solid-liquid contact area, the protruding microstructures are not resistant to friction and scratching; mechanical wear directly destroys the roughened structure, causing rapid failure of anti-adhesion performance. In traditional coatings, low surface energy materials are only distributed on the outermost layer, exposing the high surface energy substrate after wear. The coating lacks the ability to self-repair its interfacial chemical composition, resulting in a short service life.
[0004] Polyamide-imide (PAI) possesses excellent film-forming ability, heat resistance, mechanical strength, and substrate adhesion, making it suitable as a substrate for durable protective coatings. However, pure PAI has a high surface energy, resulting in insufficient self-anti-adhesion and anti-fouling capabilities. Therefore, there is an urgent need to develop composite anti-adhesion coatings that use PAI as a high-strength substrate, while also incorporating micro- to nano-level rough structures, migratable low-surface-energy components, and the ability of these low-surface-energy components to self-repair and reconstruct the interface after wear. This would address the shortcomings of existing technologies, such as poor durability and irreversible performance degradation after damage. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing anti-adhesion coatings, such as poor wear resistance and irrecoverable anti-adhesion ability after wear, and to provide a low surface energy component self-replenishing anti-adhesion composite coating, along with its preparation method and industrial applications. This invention utilizes the synergistic effect of a high-strength PAI matrix, dual-scale fluorinated silica particles, and migratable polyether-modified silicone oil: PAI ensures the coating's mechanical strength, toughness, and adhesion to the substrate; dual-scale functionalized silica constructs a micro-nano-level rough morphology, reducing the actual solid-liquid contact area; polyether-modified silicone oil, as a migratable low surface energy component, accumulates on the surface during the curing stage, leaving a component reservoir within the coating; when the surface is damaged, the internal silicone oil migrates to a new interface and rearranges, achieving self-replenishment and recovery of anti-adhesion performance.
[0006] This invention is achieved through the following technical solution:
[0007] This invention relates to a low surface energy component self-replenishing anti-adhesion composite coating, the raw materials of which include polyamide-imide (PAI), dual-scale functionalized silica particles, polyether-modified silicone oil (PEMS), and organic mixed solvent; the dual-scale functionalized silica particles include first functionalized silica particles and second functionalized silica particles; the average particle size of the first functionalized silica particles is larger than the average particle size of the second functionalized silica particles; at least a portion of the polyether-modified silicone oil is enriched in the surface layer of the coating in contact with air, and a reservoir of polyether-modified silicone oil components that can migrate and rearrange to the damaged interface is retained inside the coating.
[0008] Furthermore, the average particle size of the first functionalized silica particles is 1-5 μm, preferably 3 μm; the average particle size of the second functionalized silica particles is 50-100 nm, preferably 80 nm; and the mass ratio of the first functionalized silica particles to the second functionalized silica particles is 1:1.
[0009] Furthermore, the mass ratio of polyamide-imide, the total mass of dual-scale functionalized silica particles, and polyether-modified silicone oil is 100:40 to 140:3 to 20.
[0010] Furthermore, the organic mixed solvent is composed of N-methylpyrrolidone, N,N-dimethylformamide, xylene, and ethyl acetate; the volume ratio of the four components is 1-3:1-3:0.2-1.5:0.2-1.5, with a preferred volume ratio of 2:2:1:1.
[0011] The present invention also provides a method for preparing the above-mentioned coating, comprising the following steps:
[0012] Step S1: Surface modification of large-particle-size and small-particle-size hydrophilic silica particles with fluorinated silanes is performed to obtain dual-scale functionalized F-SiO2 particles (first functionalized silica particles and second functionalized silica particles); the preferred modification reagent is 1H,1H,2H,2H-perfluorodecyltriethoxysilane.
[0013] Step S2: Disperse the two types of F-SiO2 particles of different sizes in ethanol and sonicate them to obtain two stable particle suspensions; the mass-volume ratio of a single functionalized silica particle to ethanol is 1.5-1.8 g: 30-40 mL.
[0014] Step S3: Dissolve the polyamide-imide powder in an organic mixed solvent and stir at room temperature for no less than 3 hours to obtain a uniform and transparent PAI matrix solution;
[0015] Step S4: Add polyether-modified silicone oil to the PAI matrix solution and stir at low speed for no less than 30 minutes;
[0016] Step S5: Add two portions of F-SiO2 particle suspension to the mixing system in sequence and stir continuously for no less than 1 hour to obtain a stable composite coating; wherein, the mixing system includes N-methylpyrrolidone, N,N-dimethylformamide, xylene and ethyl acetate, with a volume ratio of 1~3:1~3:0.2~1.5:0.2~1.5, preferably 2:2:1:1.
[0017] Step S6: Apply the composite coating to the pretreated substrate surface to form a wet film; the coating method is selected from spraying, brushing, dipping, spin coating, and roller coating, with spraying being preferred; the substrate is selected from metal, glass, ceramic, or solvent-resistant polymer substrate;
[0018] Step S7: The wet film undergoes stepped temperature curing, which is divided into three stages: the first stage is room temperature evaporation for 0.5 to 2 hours; the second stage is low-temperature pre-curing at 50 to 80°C for 1 to 2 hours; and the third stage is medium-temperature curing at 90 to 130°C for 1 to 2 hours. A low surface energy component self-replenishing anti-adhesion composite coating is obtained.
[0019] The coating prepared according to this method has the following characteristics: the interior of the coating is a continuous PAI matrix phase, in which dual-scale F-SiO2 particles are dispersed and embedded; larger-diameter F-SiO2 particles construct a first-order undulating structure, while smaller-diameter F-SiO2 particles fill the gaps between large particles, together forming a micro-nano-level rough topology; the coating exhibits a compositional gradient of silicon and fluorine elements that decreases from the surface to the interior along the depth direction; after the coating surface is damaged, the polyether-modified silicone oil stored inside migrates to the damaged interface under the drive of concentration gradient and interfacial free energy, reconstructs the low surface energy surface layer, and restores the anti-adhesion performance of the coating.
[0020] This invention also protects the application of the above-mentioned composite coating: applying the composite coating to the surface of metal, glass, ceramic, and polymer material substrates to achieve anti-fouling, anti-oil, anti-adhesive material adhesion, easy cleaning, demolding, and anti-scaling protection of the substrate surface; the application objects include storage tanks, conveying pipelines, reactors, stirring devices, filling equipment, and molds.
[0021] The present invention has the following advantages:
[0022] (1) This invention introduces polyether-modified silicone oil into the PAI / F-SiO2 composite system, enabling the coating to simultaneously possess low surface energy interface regulation and dynamic interface reconstruction capabilities. During the coating curing process, the polyether-modified silicone oil and related low surface energy components can gradually migrate and accumulate towards the coating-air interface under the driving force of interfacial free energy, thereby forming a low surface energy functional layer on the surface of the PAI high-strength film-forming substrate. This structure avoids the problems of easy wear and difficulty in recovery after failure of the functional layer caused by simply relying on surface grafting or one-time low surface energy treatment.
[0023] (2) This invention endows the coating with adaptive and restorative anti-adhesion properties. When the coating surface suffers localized damage due to friction, scratching, cleaning, or long-term use, resulting in a reduction of low surface energy components, the polyether-modified silicone oil and low surface energy components retained inside the coating can further migrate and rearrange to the newly exposed interface, allowing the damaged area to reform a low surface energy surface, thereby restoring at least part of the anti-adhesion properties. Thus, this invention achieves not only initial low adhesion, but also an anti-adhesion interface with a certain degree of continuous replenishment and dynamic recovery capability, which is beneficial for extending the effective service life of the coating.
[0024] (3) This invention achieves a balance between anti-adhesion performance and coating structural stability through the synergistic effect of the PAI continuous phase, dual-scale F-SiO2 particles, and PEMS low surface energy phase. PAI provides excellent film-forming properties, mechanical strength, heat resistance, and substrate adhesion; dual-scale F-SiO2 is used to construct a stable hierarchical structure and reduce interfacial energy; and PEMS further regulates surface composition and surface free energy. The three components work together to improve the problem of simultaneously maintaining anti-adhesion performance and mechanical stability, which is common in traditional low surface energy coatings.
[0025] (4) Through the combined regulation of multi-scale surface structure and low surface energy chemical composition, the coating of this invention can reduce the adhesion and residue of different types of liquids on the surface. It can be used for anti-adhesion treatment of various media such as aqueous liquids, oily liquids, and organic liquids with high viscosity, thereby improving the ability of pollutants to be removed and the surface easy to clean, and has good broad-spectrum anti-adhesion potential. It is particularly suitable for high viscosity liquids that are prone to wall adhesion, residue and adhesion during filling, storage, transportation, mixing and processing.
[0026] (5) This invention employs a preparation method combining spraying and stepped temperature curing, which is simple, highly operable, and easy to apply over large areas. Through room temperature evaporation, low-temperature pre-curing, and medium-temperature curing, the gradual evaporation of solvent, PAI substrate film formation, and PEMS migration and enrichment to the surface can be simultaneously achieved, allowing the coating structure and surface function to form synchronously. The method is applicable to metal, glass, ceramic, and other substrates resistant to corresponding solvents and curing temperatures, and has the potential for further scale-up preparation and engineering applications.
[0027] (6) The composite anti-adhesion coating formed by the present invention has good application scalability. The coating can be used on the surface of equipment and components in chemical equipment, machinery manufacturing, aerospace, biomedicine, food processing and other equipment involving contact with high viscosity liquids. It is especially suitable for storage tanks, pipelines, reactors, stirring devices, conveying equipment, filling equipment and molds, etc., where high viscosity materials are prone to residue and accumulation, which can reduce material loss and cleaning and maintenance difficulty. Attached Figure Description
[0028] Figure 1 This is a complete process flow diagram for the preparation of the composite coating of the present invention;
[0029] Figure 2 These are SEM images of the coating surface at different magnifications in Example 1 of the present invention, showing the micro-nano level rough topology;
[0030] Figure 3 Static wetting photographs of various test droplets on the coating surface of this invention;
[0031] Figure 4 The graph shows the changes in the atomic content of fluorine, silicon, carbon, nitrogen, and oxygen elements as the coating is etched to different depths from the surface inwards.
[0032] Figure 5 This is a sandpaper cyclic abrasion test, showing the changes in the coating's water contact angle and mass loss with the number of abrasion cycles; it is used to illustrate the coating's performance maintenance and self-replenishment effect after wear.
[0033] Figure 6 This is a schematic diagram illustrating the self-replenishment mechanism of the low surface energy components in the coating of the present invention.
[0034] Figure 7 This is a photograph showing the droplet wetting state on the coating surface in a comparative example (without SiO2 particles).
[0035] Figure 8 Comparison of cupping tests for coatings with different PAI contents to characterize the mechanical toughness of the coatings;
[0036] Figure 9 These are photographs showing the wetting states of various droplets in the bending area after the coating of the present invention has been bent; these images characterize the retention of the anti-adhesion function of the coating after deformation.
[0037] Figure 10 A schematic diagram of the entire process of draining high-viscosity dyeing adhesive to coat a variable-diameter steel container with the coating of the present invention, verifying the anti-adhesion and residue-free effect. Detailed Implementation
[0038] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are merely further illustrations of the present invention, but the scope of protection of the present invention is not limited to the following embodiments.
[0039] Example 1
[0040] This embodiment relates to a method for preparing a low surface energy component self-replenishing anti-adhesion composite coating, see [link to documentation]. Figure 1 As shown, the specific steps are as follows:
[0041] (1) Measure 22 mL of anhydrous ethanol into 30 mL beakers and stir for 10 min at room temperature. Then add 1 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and continue stirring for 30 min to obtain two identical modified mother liquors A and B. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 3 μm and place them in modified mother liquor A. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 80 nm and place them in modified mother liquor B. Stir the two mixtures magnetically at room temperature in the dark for 1 h. Then place the two mixtures into petri dishes A and B respectively and place them in an electric resistance furnace to dry at 60 °C for more than 2 h until the particles are completely dry, thus obtaining F-SiO2 particles of two different particle sizes.
[0042] (2) Measure 20 mL of N-methylpyrrolidone (NMP), 20 mL of N,N-dimethylformamide (DMF), 10 mL of xylene, and 10 mL of ethyl acetate into a beaker, seal and magnetically stir for 30 min at room temperature to obtain a mixed good solvent. Add 2 g of polyamide-imide (PAI) powder to the above mixed good solvent, and magnetically stir for more than 3 h at room temperature until a pale yellow transparent clear solution is obtained. Then add 0.2 g of polyether modified silicone oil (PEMS) and magnetically stir at low speed for 30 min.
[0043] (3) The two types of F-SiO2 particles obtained above were ultrasonically dispersed in 5 mL of ethanol for more than 30 min to obtain a dispersion. The F-SiO2 dispersion with a particle size of 3 μm was slowly added to the above mixture and stirred for more than 30 min. Then, the F-SiO2 dispersion with a particle size of 80 nm was added and magnetically stirred at room temperature for more than 1 h to form a stable and uniform composite coating.
[0044] (4) Select tinplate as the substrate and rinse the surface of the tinplate thoroughly with anhydrous ethanol to remove surface impurities and oil stains. Then place it in a vacuum drying oven and dry at 60°C for 10 minutes before taking it out.
[0045] (5) The composite coating was sprayed onto the dried iron sheet using a spray bottle. A stepped temperature curing procedure was adopted, and the coating was cured at room temperature for 1 hour to allow some solvent to evaporate. Then, pre-curing at 60°C was performed to enrich PEMS on the surface. Then, the coating was placed at 100°C for medium-temperature curing to allow partial cross-linking of PAI. During this process, PEMS and low surface energy components gradually migrated to the air interface and accumulated, thus obtaining a low surface energy component self-replenishing anti-adhesion composite coating.
[0046] (6) See Figure 2As shown in the SEM images, interconnected pores and recesses are observed between the PAI framework, with micron-sized SiO2 particles anchored within. At higher magnification, the framework surface and the surface of the micron-sized SiO2 particles are densely covered by nano-sized SiO2 particles, forming a finer secondary texture and thus creating a hierarchical topology. This morphology can be attributed to the structural locking of the particle framework by PAI curing shrinkage. The rough features help trap air at the solid-liquid interface, significantly reducing the actual contact area, thereby promoting a stable Cassie-Baxter wet state and achieving high contact angle and low adhesion behavior.
[0047] (7) See Figure 3 As shown, when various complex liquids are placed on the coating surface and left to stand, they all shrink into an approximately spherical shape, indicating that the coating has excellent liquid-repellent properties.
[0048] (8) See Figure 4 As shown, extremely high F and Si signals were observed on the surface. With increasing etching depth, the concentrations of F and Si atoms gradually decreased, while the concentration ratio of N and O also changed, which further confirmed the enrichment of PEMS on the surface.
[0049] (9) See Figure 5 As shown, with increasing wear cycles, the water contact angle of the coating slowly decreases from approximately 173° to approximately 163–166°, remaining generally within the hydrophobic or even superhydrophobic range. Simultaneously, the coating quality loss shows a gradual upward trend, but the rate of increase is relatively small. See... Figure 6 As shown, this is because after the coating surface is damaged, the internally migratable PEMS migrate, diffuse, and reorient to the newly formed air interface under the drive of interfacial free energy and concentration gradient, so that the low surface energy components of the damaged surface are replenished, thereby partially or basically restoring the anti-adhesion performance.
[0050] Example 2
[0051] This embodiment relates to a method for preparing a low surface energy component self-replenishing anti-adhesion composite coating. The process of this embodiment is the same as that of Embodiment 1, except for whether or not SiO2 particles are added, as detailed below:
[0052] (1) Measure 20 mL of N-methylpyrrolidone (NMP), 20 mL of N,N-dimethylformamide (DMF), 10 mL of xylene, and 10 mL of ethyl acetate into a beaker, seal and magnetically stir for 30 min at room temperature to obtain a mixed good solvent. Add 2 g of polyamide-imide (PAI) powder to the above mixed good solvent, and magnetically stir for more than 3 h at room temperature until a pale yellow transparent clear solution is obtained. Then add 0.2 g of polyether modified silicone oil (PEMS), and magnetically stir at low speed for 30 min to obtain a stable and uniform composite coating.
[0053] (2) Use tinplate as the substrate and rinse the surface of the tinplate thoroughly with anhydrous ethanol to remove surface impurities and oil. Then place it in a vacuum drying oven and dry at 60°C for 10 minutes before taking it out.
[0054] (3) The composite coating was sprayed onto the dried iron sheet using a spray bottle. A stepped temperature curing procedure was adopted, and the coating was cured at room temperature for 1 hour to allow some solvent to evaporate. Then, it was pre-cured at 60°C to enrich PEMS on the surface. Then, it was placed at 100°C for medium-temperature curing to allow partial cross-linking of PAI. During this process, PEMS gradually migrated to the air interface and became enriched, thus obtaining a low surface energy component self-replenishing anti-adhesion composite coating.
[0055] (4) See Figure 7 As shown, in this embodiment, the droplets spread out in a flat elliptical shape on the coating surface, with a small contact angle and a large contact area between the droplets and the surface. There is a certain degree of spreading and wetting at the edges.
[0056] Example 3
[0057] This embodiment relates to a method for preparing a low surface energy component self-replenishing anti-adhesion composite coating. This embodiment is the same as Embodiment 1, except that the PAI content is different. The specific steps include:
[0058] (1) Measure 22 mL of anhydrous ethanol into 30 mL beakers and stir for 10 min at room temperature. Then add 1 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and continue stirring for 30 min to obtain two identical modified mother liquors A and B. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 3 μm and place them in modified mother liquor A. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 80 nm and place them in modified mother liquor B. Stir the two mixtures magnetically at room temperature in the dark for 1 h. Then place the two mixtures into petri dishes A and B respectively and place them in an electric resistance furnace to dry at 60 °C for more than 2 h until the particles are completely dry to obtain F-SiO2 particles of two particle sizes. Repeat the above method to obtain three sets of identical dual-particle-size F-SiO2 particles.
[0059] (2) Measure 20 mL of N-methylpyrrolidone (NMP), 20 mL of N,N-dimethylformamide (DMF), 10 mL of xylene, and 10 mL of ethyl acetate into a beaker, seal and magnetically stir for 30 min at room temperature to obtain mixed good solvent 1. Repeat the above method to obtain the same mixed good solvents 2, 3, and 4. Weigh 0.5 g, 1 g, 2 g, and 3 g of polyamide-imide (PAI) powder respectively, and place them into the above four mixed good solvents respectively. Stir magnetically for more than 3 h at room temperature until a pale yellow transparent clear solution is obtained. Then add 0.2 g of polyether modified silicone oil (PEMS) to each of the four solutions and stir magnetically at low speed for 30 min.
[0060] (3) Disperse two types of F-SiO2 particles of different sizes in 5 mL of ethanol by ultrasonication for more than 30 min to obtain dispersions A and B. Slowly add dispersion A to the above mixture 1 and stir for more than 30 min. Then add dispersion B and stir magnetically at room temperature for more than 1 h to form a stable and uniform composite coating 1. Obtain composite coatings 2, 3 and 4 in the same way.
[0061] (4) Select tinplate as the substrate and rinse the surface of the tinplate thoroughly with anhydrous ethanol to remove surface impurities and oil stains. Then place it in a vacuum drying oven and dry at 60°C for 10 min before taking it out.
[0062] (5) The composite coating 1 was sprayed onto the dried iron sheet using a spray bottle. A stepped temperature curing procedure was adopted, and the sheet was cured at room temperature for 1 h to allow some solvent to evaporate. Then, it was pre-cured at 60℃ to enrich PEMS on the surface. Then, it was placed at 100℃ for medium-temperature curing to allow partial cross-linking of PAI. During this process, PEMS and low surface energy components gradually migrated to the air interface and accumulated, resulting in sample 1. Samples 2, 3, and 4 were obtained in the same manner.
[0063] (6) See Figure 8 As shown, with the increase of PAI content, the cupping height of samples 1, 2, 3, and 4 significantly increased, far exceeding that of the pure PAI coating and the PAI / PEMS coating. This demonstrates the important role of continuous PAI load-bearing in the system's stability. When the PAI content is low, the coating lacks a continuous phase and has a relatively high proportion of inorganic fillers, making particle agglomeration and porosity defects more likely to form. This leads to significant stress concentration under biaxial tension, and the coating tends to fail prematurely via brittle cracking or interfacial delamination. As the PAI content increases, its proportion as a continuous framework phase increases, enabling more complete coating of SiO2 and improving interfacial bonding strength. Defect sensitivity decreases, and the coating's toughness and load-bearing capacity improve simultaneously, resulting in a significant increase in cupping height.
[0064] (7) See Figure 9As shown, after repeated bending on the metal shaft, the coating still maintained continuous coverage in the bending area without large-scale delamination, and various droplets maintained a high contact angle in the bending area. This indicates that under a reasonable PAI content, the coating not only has good crack resistance and peel resistance, but its surface functional layer is not completely destroyed during the plastic forming process.
[0065] Example 4
[0066] This embodiment relates to a method for preparing a low surface energy component self-replenishing anti-adhesion composite coating. This embodiment is the same as Embodiment 1, except for the substrate and spraying method. The specific steps include:
[0067] (1) Measure 22 mL of anhydrous ethanol into 30 mL beakers and stir for 10 min at room temperature. Then add 1 mL of 1H,1H,2H,2H-perfluorodecyltriethoxysilane and continue stirring for 30 min to obtain two identical modified mother liquors A and B. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 3 μm and place them in modified mother liquor A. Weigh 1.5 g of dry hydrophilic SiO2 particles with a particle size of 80 nm and place them in modified mother liquor B. Stir the two mixtures magnetically at room temperature in the dark for 1 h. Then place the two mixtures into petri dishes A and B respectively and place them in an electric resistance furnace to dry at 60 °C for more than 2 h until the particles are completely dry, thus obtaining F-SiO2 particles of two different particle sizes.
[0068] (2) Measure 20 mL of N-methylpyrrolidone (NMP), 20 mL of N,N-dimethylformamide (DMF), 10 mL of xylene, and 10 mL of ethyl acetate into a beaker, seal and magnetically stir for 30 min at room temperature to obtain a mixed good solvent. Add 2 g of polyamide-imide (PAI) powder to the above mixed good solvent, and magnetically stir for more than 3 h at room temperature until a pale yellow transparent clear solution is obtained. Then add 0.2 g of polyether modified silicone oil (PEMS) and magnetically stir at low speed for 30 min.
[0069] (3) The two types of F-SiO2 particles obtained above were ultrasonically dispersed in 5 mL of ethanol for more than 30 min to obtain a dispersion. The F-SiO2 dispersion with a particle size of 3 μm was slowly added to the above mixture and stirred for more than 30 min. Then, the F-SiO2 dispersion with a particle size of 80 nm was added and magnetically stirred at room temperature for more than 1 h to form a stable and uniform composite coating.
[0070] (4) A truncated cone-shaped hollow steel container with short cylindrical sections at both ends was selected as the base material. The outer diameter of the large diameter end Φ1 = 70 mm and the height is 5 mm; the outer diameter of the small diameter end Φ2 = 40 mm and the height is 5 mm, with a uniformly transitioning tapered diameter section in the middle. The total height of the container H = 80 mm and the wall thickness is uniformly about 2 mm. The inner surface of the steel container was thoroughly sanded with sandpaper, and the surface impurities and oil stains were thoroughly cleaned with anhydrous ethanol. Then it was dried in a vacuum oven at 60 ℃ for 20 min.
[0071] (5) The composite coating was uniformly sprayed onto the inner surface of the dried steel container along a circular path using a small electric airbrush with a nozzle diameter of 0.5 mm. A stepped temperature curing procedure was adopted, and the container was cured at room temperature for 1 h to allow some solvent to evaporate. Subsequently, it was pre-cured at 60℃ to enrich PEMS on the surface. Then, it was placed at 100℃ for medium-temperature curing to allow partial cross-linking of PAI. During this process, PEMS and low surface energy components gradually migrated to the air interface and accumulated, thus obtaining a steel container with a self-replenishing anti-adhesion composite coating of low surface energy components.
[0072] (6) Hang the container vertically on the support with the large diameter end facing up and the small diameter end facing down. Place a baffle horizontally at the bottom of the small diameter end to completely cover and tightly fit the opening of the small diameter end. Pour 60 mL of dyeing glue into the container from the top and let it stand in the container for 10 minutes, then remove the baffle.
[0073] (7) See Figure 10 As shown, under the influence of gravity, the dyed glue gradually drains from the container, and finally the glue is completely drained, leaving no residue on the inner wall of the container.
[0074] This invention uses polyamide-imide (PAI) as the main film-forming matrix, F-SiO2 particles of different sizes as functional fillers, and a mixed solvent system consisting of N-methyl-2-pyrrolidone (NMP), N,N-dimethylformamide (DMF), xylene, and ethyl acetate as a good solvent. Simultaneously, by introducing polyether-modified silicone oil (PEMS) with interfacial migration capabilities, and combining it with a stepped curing strategy of room temperature evaporation, low-temperature pre-curing, and medium-temperature curing, the distribution of PEMS within the coating and its migration and enrichment towards the air interface are controlled, forming a low surface energy functional layer on the coating surface. When the coating surface is subjected to friction, wear, or other minor damage, the PEMS retained internally can migrate and rearrange back to the damaged surface driven by interfacial free energy and concentration gradient, achieving dynamic replenishment of low surface energy components and self-recovery of anti-adhesion properties. The coating exhibits excellent anti-adhesion, easy cleaning, and durability potential. Furthermore, the spraying process is simple and suitable for large-area preparation, making it applicable to fields such as chemical engineering, machinery manufacturing, aerospace, biomedicine, and food processing.
[0075] The specific embodiments of the present invention have been described above. It should be understood that the present invention is not limited to the specific embodiments described above, and those skilled in the art can make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A low surface energy component self-replenishing anti-adhesion composite coating, characterized in that, It contains polyamide-imide (PAI), dual-scale functionalized silica particles, polyether-modified silicone oil (PEMS), and organic mixed solvents; The dual-scale functionalized silica particles comprise a first functionalized silica particle and a second functionalized silica particle; the average particle size of the first functionalized silica particle is larger than the average particle size of the second functionalized silica particle; at least a portion of the polyether-modified silicone oil is enriched in the surface layer of the coating that is in contact with air, and a reservoir of polyether-modified silicone oil components that can migrate and rearrange to the damaged interface is retained inside the coating.
2. The low surface energy component self-replenishing anti-adhesion composite coating as described in claim 1, characterized in that, The average particle size of the first functionalized silica particles is 1-5 μm, and the average particle size of the second functionalized silica particles is 50-100 nm; the mass ratio of the first functionalized silica particles to the second functionalized silica particles is 1:
1.
3. The low surface energy component self-replenishing anti-adhesion composite coating as described in claim 1, characterized in that, The mass ratio of the polyamide-imide, dual-scale functionalized silica particles, and polyether-modified silicone oil is 100:40-140:3-20.
4. A method for preparing a low surface energy component self-replenishing anti-adhesion composite coating as described in claim 1, characterized in that, Includes the following steps: Step S1: Fluorine-containing silanes are used to modify the surfaces of large-particle-size and small-particle-size hydrophilic silica particles respectively, resulting in dual-scale functionalized silica particles, comprising first functionalized silica particles and second functionalized silica particles. Step S2: Disperse the first functionalized silica particles and the second functionalized silica particles in ethanol, respectively, and sonicate them to obtain two F-SiO2 particle suspensions. Step S3: Dissolve the polyamide-imide powder in an organic mixed solvent and stir at room temperature for no less than 3 hours to obtain a uniform and transparent PAI matrix solution; Step S4: Add polyether-modified silicone oil to the PAI matrix solution and stir at low speed for no less than 30 minutes; Step S5: Add two portions of F-SiO2 particle suspension to the mixed solvent system in sequence and stir continuously for no less than 1 hour to obtain a stable composite coating; wherein, the mixed solvent system is composed of N-methylpyrrolidone, N,N-dimethylformamide, xylene and ethyl acetate, and the volume ratio is 1~3:1~3:0.2~1.5:0.2~1.5; Step S6: Apply the composite coating to the pretreated substrate surface to form a wet film; Step S7: The wet film is cured by step temperature increase to obtain a low surface energy component self-replenishing anti-adhesion composite coating.
5. The preparation method according to claim 4, characterized in that, In step S1, the surface modification uses 1H,1H,2H,2H-perfluorodecyltriethoxysilane as the modifying agent.
6. The preparation method according to claim 4, characterized in that, In step S2, the mass-volume ratio of a single SiO2 particle to ethanol in the two particle sizes of F-SiO2 particles is 1.5-1.8g:30-40mL.
7. The preparation method according to claim 4, characterized in that, In step S6, the coating method is selected from any one of spraying, brushing, dipping, spin coating, and roller coating, with spraying being preferred; the substrate is metal, glass, ceramic, or solvent-resistant polymer substrate.
8. The preparation method according to claim 4, characterized in that, In step S7, the stepped temperature curing is divided into three stages: the first stage is room temperature volatilization for 0.5 to 2 hours; the second stage is low temperature pre-curing at 50 to 80°C for 1 to 2 hours; and the third stage is medium temperature curing at 90 to 130°C for 1 to 2 hours. Through stepped curing, the polyether-modified silicone oil migrates and accumulates on the surface of the coating, while the PAI matrix completes film formation and partial cross-linking.
9. The preparation method according to any one of claims 4-7, characterized in that, The low surface energy component self-supplementing anti-adhesion composite coating prepared by this method has a continuous PAI matrix phase inside, with two particle sizes of F-SiO2 particles dispersed and embedded in the continuous matrix phase. Large-diameter particles construct a first-order undulating structure, while small-diameter particles fill the gaps between large particles, together forming a micro-nano hierarchical rough topology. Along the depth direction of the coating, there is a compositional gradient of silicon and fluorine elements that decreases from the surface to the inside. After the coating surface is damaged, the polyether-modified silicone oil stored inside migrates to the damaged interface under the drive of concentration gradient and interfacial free energy, reconstructs the low surface energy surface layer, and restores the anti-adhesion performance of the coating.
10. The application of the low surface energy component self-replenishing anti-adhesion composite coating as described in claim 1, characterized in that, This composite coating is applied to the surface of metal, glass, ceramic, and polymer materials to achieve surface protection against contamination, oil, and adhesives, as well as easy cleaning, demolding, and scaling. Applications include storage tanks, pipelines, reactors, agitators, filling equipment, and molds.