A method for preparing high-density, crack-resistant nano-modified composite waterborne epoxy asphalt

By preparing high-density, crack-resistant nano-modified composite waterborne epoxy asphalt, and using a gradient cross-linking curing process and charge matching design to form an interpenetrating network structure, the problems of storage stability, rigidity and toughness, and construction compatibility of waterborne epoxy asphalt materials were solved, and the comprehensive performance of the material was improved, making it suitable for high-grade bridge engineering.

CN123107544APending Publication Date: 2026-11-17WUXI JIAOJIAN NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611392348.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing waterborne epoxy asphalt materials have technical defects such as insufficient storage stability, difficulty in balancing rigidity and toughness, and poor construction adaptability, which cannot meet the performance requirements of high-grade bridge projects.

Method used

A method for preparing highly dense, crack-resistant nano-modified composite waterborne epoxy asphalt is adopted. By preparing multi-component materials and using a gradient cross-linking curing process, an interpenetrating or semi-interpenetrating network structure is formed. Nanofillers with surface-grafted epoxy groups are used as physical cross-linking points and chemical reaction sites. Combined with anionic/nonionic emulsifiers to adjust charge matching, the stability and performance of the material are improved.

Benefits of technology

It improves the storage stability and construction adaptability of materials, enhances bond strength, crack resistance and weather resistance, enables them to withstand complex alternating stresses on bridge decks, extends service life, and solves many defects existing in the prior art.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107544A_ABST
    Figure CN123107544A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of waterborne epoxy asphalt preparation technology, and more particularly to a method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt. First, components A and B, containing surface-grafted epoxy group modified nanofillers, and component C, containing a curing accelerator, are prepared. These components are mixed in a predetermined ratio before construction to obtain a lower-layer room-temperature penetrating adhesive material. Then, the modified nanofiller is dispersed in anionic waterborne epoxy resin emulsion and uniformly mixed with anionic emulsified asphalt and anionic chloroprene latex. The pH of the system is adjusted to match the surface charge of the modified nanofiller to obtain component D. After the lower-layer material is surface-dried, component D is applied, and the mixture is cured through gradient crosslinking to obtain the target product. This preparation method effectively improves the storage stability of the system, simultaneously considering the rigidity and toughness of the material, enhancing water and weather resistance, solving the problem of easy wheel adhesion during construction, and the preparation process is simple and controllable, suitable for various road and bridge waterproof bonding construction scenarios.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of waterborne epoxy asphalt preparation technology, and in particular to a method for preparing high-density, crack-resistant nano-modified composite waterborne epoxy asphalt. Background Technology

[0002] The waterproof bonding layer of a bridge deck is a key functional layer in the bridge deck pavement structure, serving the dual functions of interface waterproofing and interlayer bonding. Its performance directly determines the service life of the bridge deck pavement and driving safety. With the continuous expansion of the construction scale of high-grade highways and bridges in my country and the increasing proportion of heavy-load traffic, the industry has put forward higher requirements for the comprehensive performance of waterproof bonding materials, including storage stability, mechanical strength, weather resistance, and construction adaptability.

[0003] Currently, the mainstream materials used in bridge deck waterproofing bonding fall into two categories. The first category is ordinary emulsified asphalt material, which is prepared by emulsification of asphalt as the main raw material. It has the advantages of simple preparation process, low cost, and convenient construction at room temperature, and was widely used in bridge deck paving projects in the past. However, this type of material has low bonding strength, high temperature sensitivity, and is prone to soft adhesion at high temperatures and brittle cracking at low temperatures, resulting in poor service durability. It is now difficult to meet the performance requirements of high-grade bridge deck projects. The second category is existing ordinary water-based epoxy emulsified asphalt material. It introduces water-based epoxy resin and curing agent into the emulsified asphalt system, relying on the epoxy-amine crosslinking reaction to form a three-dimensional network structure. It combines the high adhesion of epoxy resin with the construction convenience of emulsified asphalt, and is currently the most widely used bridge deck waterproofing bonding material.

[0004] However, this type of material still has many technical defects: First, the components have poor compatibility. The charge matching between water-based epoxy curing agents and emulsified asphalt is not good, which can easily cause the system to demulsify and self-cur, resulting in insufficient storage stability and greatly limiting transportation and engineering applications. Second, it is difficult to balance mechanical properties and flexibility. After epoxy crosslinking, the system is brittle and lacks low-temperature flexibility, making it prone to cracking and failure under the complex alternating stress of the bridge deck. Third, the weather resistance is insufficient. Unmodified bisphenol A epoxy resin has poor aging resistance and its performance degrades rapidly during long-term service, which cannot guarantee the long-term service life of the bridge deck pavement. Fourth, the construction adaptability is poor. High-temperature construction can easily cause wheel sticking problems, which can damage the already applied waterproof bonding layer and affect the quality and progress of the project.

[0005] In response to the common technical defects of existing waterborne epoxy asphalt waterproofing adhesives, the industry urgently needs to develop waterborne epoxy asphalt preparation technologies with better overall performance to meet the application needs of high-grade bridges, composite pavements and other projects. Summary of the Invention

[0006] To address the technical shortcomings of existing waterborne epoxy asphalt, such as insufficient storage stability, difficulty in balancing rigidity and toughness, and poor construction adaptability, this invention provides a method for preparing high-density, crack-resistant nano-modified composite waterborne epoxy asphalt.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for preparing highly dense, crack-resistant nano-modified composite waterborne epoxy asphalt includes the following steps: S1. Preparation of the lower layer room temperature penetrating adhesive material: Prepare components A, B, and C separately. Before construction, mix components A, B, and C evenly in a mass ratio of 100:150:150. Component A contains water-based modified epoxy resin, modified nanofiller, and composite coupling agent; component B contains water-based amine epoxy curing agent, modified nanofiller, and film-forming aid; and component C contains water-based epoxy curing accelerator. The modified nanofiller is one or more of zero-dimensional, one-dimensional, and two-dimensional nanofillers, and the surface of the modified nanofiller is grafted with epoxy groups. S2. Preparation of component D of the upper thermosetting second-order reactive waterproof adhesive material: Anionic emulsified asphalt was prepared using anionic / nonionic emulsifiers. Modified nanofillers were dispersed in anionic waterborne modified epoxy resin emulsion, and then mixed with anionic emulsified asphalt and anionic chloroprene latex. The pH of the system was adjusted to match the surface charge of the modified nanofillers, and the mixture was stirred evenly to obtain component D. S3, Gradient crosslinking curing: First, the lower layer of room temperature penetrating adhesive material is applied to the substrate to be treated and allowed to dry on the surface. Then, component D is applied. The temperature and humidity of the curing environment are controlled to achieve simultaneous evaporation of moisture, crosslinking of epoxy, and fusion of asphalt particles. The modified nanofiller also participates in the epoxy curing reaction as a physical crosslinking point and a chemical reaction site, forming an interpenetrating network or semi-interpenetrating network structure, thus obtaining the target product.

[0008] Furthermore, the zero-dimensional nanofiller with surface-grafted epoxy groups is nano-silica or nano-calcium carbonate modified with a silane coupling agent, the one-dimensional nanofiller is carbon nanotubes or nano-cellulose with surface-grafted epoxy groups, and the two-dimensional nanofiller is graphene oxide with surface-grafted epoxy groups.

[0009] Furthermore, component A comprises, by weight, 60-80 parts of waterborne modified epoxy resin, 5-10 parts of modified nanofiller, 0.5-1.5 parts of composite coupling agent, 0.1-0.5 parts of defoamer, 10-20 parts of industrial pure water, and 0.2-0.6 parts of additives. During preparation, the modified nanofiller is added to the waterborne modified epoxy resin emulsion and dispersed at a high speed of 800-1200 rpm for 15-20 minutes. The remaining raw materials are then added and stirred until homogeneous, and the viscosity is adjusted accordingly.

[0010] Furthermore, component B comprises, by weight, 60-80 parts of waterborne amine epoxy curing agent, 0.2-0.8 parts of dispersant, 1-3 parts of film-forming aid, 5-10 parts of modified nanofiller, 20-40 parts of industrial pure water, and 0.2-0.6 parts of additives. In preparation, the waterborne amine epoxy curing agent is first dispersed in water, then the dispersant is added and stirred until homogeneous. The modified nanofiller is then added and dispersed at a high speed of 800-1200 rpm for 15-20 minutes. Finally, the film-forming aid is added and stirred until homogeneous.

[0011] Furthermore, component C comprises 60-80 parts by weight of a waterborne epoxy curing accelerator, wherein the waterborne epoxy curing accelerator is selected from one or more of 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), benzyldimethylamine, and 2-methylimidazole, and also comprises 0.2-0.8 parts of dispersant, 20-40 parts of industrial pure water, and 0.2-0.6 parts of additives; during preparation, all raw materials are mixed and dispersed at a low speed of 300-500 rpm for 15-20 minutes until the system is homogeneous.

[0012] Furthermore, component D, by weight, comprises 25-35 parts anionic emulsified asphalt, 25-65 parts anionic waterborne modified epoxy resin, 5-15 parts anionic chloroprene latex, 5-10 parts modified nanofiller, 0.5-2 parts composite coupling agent, 0.1-0.5 parts defoamer, 10-20 parts industrial pure water, and 0.2-0.6 parts additives.

[0013] Furthermore, in preparing component D, the modified nanofiller is first added to the anionic aqueous modified epoxy resin emulsion, and then uniformly dispersed by high-speed shearing at 800~1200 rpm for 15~20 min and ultrasonic dispersion for 10~15 min. Then, it is mixed with anionic emulsified asphalt and anionic chloroprene latex at 300~500 rpm for 10~15 min. The pH of the system is adjusted to 8.0~9.0 to match the charge of the negatively charged modified nanofiller and avoid system demulsification.

[0014] Furthermore, the control conditions for gradient cross-linking curing in S3 are as follows: first, cure for 12-24 hours at a temperature of 20-30℃ and a relative humidity of 40%-70%, and then cure for 24-36 hours at an ambient temperature of 35-45℃, so as to achieve gradual evaporation of moisture, gradual cross-linking of epoxy groups, and gradual fusion of asphalt particles.

[0015] Furthermore, the anionic emulsified asphalt is anionic slow-cracking type 70# emulsified asphalt with a solid content of 50%~65%, and the anionic waterborne modified epoxy resin is a bisphenol A type waterborne epoxy resin modified by methacrylic acid resin and polyurethane; the composite coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane.

[0016] Furthermore, the coating amount of the lower layer of S3 room temperature penetrating adhesive is 0.2~0.3 kg / m². 2 After surface drying, the coating amount of component D is 0.6~0.8 kg / m². 2 After coating, the surface should be sealed and cured for 48 hours before proceeding with the subsequent paving process.

[0017] The present invention has the following beneficial effects: This invention improves the overall charge consistency of the system by adjusting the pH of the D-component system to match the surface charge of the modified nanofiller with grafted epoxy groups, and by compounding anionic emulsified asphalt prepared with anionic / nonionic emulsifiers with anionic waterborne modified epoxy resin and anionic chloroprene latex. This effectively solves the defects of existing technologies, such as charge mismatch between waterborne epoxy components and emulsified asphalt, premature demulsification and self-curing, and insufficient storage stability. The stability of the material during storage, transportation, and pre-construction static setting is reliably guaranteed.

[0018] This invention employs multidimensional modified nanofillers with surface-grafted epoxy groups, which simultaneously serve as physical crosslinking points and chemical reaction sites in the epoxy curing reaction. Combined with a gradient crosslinking curing process, it forms an interpenetrating or semi-interpenetrating network structure. Simultaneously, anionic chloroprene latex is introduced to toughen the system, thereby synergistically improving the material's bonding strength, crack resistance, temperature change resistance, and aging resistance. This effectively solves the defects of existing technologies, such as the difficulty in balancing mechanical strength and low-temperature flexibility, and insufficient weather resistance during long-term service, which easily leads to cracking and failure. It can withstand the complex alternating stress of bridge decks, significantly extending its service life.

[0019] This invention adopts a double-layer gradient functional structure design, with the lower layer being a room-temperature penetrating adhesive material and the upper layer being a thermosetting two-stage reactive waterproof adhesive material. Combined with a staged curing control process, the surface drying rate of the material is controllable, there is no problem of sticking to the wheel during high-temperature construction, and it can be cured and formed normally in low-temperature environments. This effectively solves the defects of poor construction adaptability and easy sticking to the wheel and damage to the formed waterproof adhesive layer at high temperatures in the existing technology, and the construction window is significantly widened.

[0020] The material prepared by the method described in this invention is not only suitable for conventional highway bridge paving waterproof bonding layer scenarios, but also adaptable to complex working conditions such as heavy-duty traffic bridges, steel bridge deck paving, and composite pavement transition sections, meeting the engineering application needs of different climate regions and different construction periods, and has high industry promotion value. Attached Figure Description

[0021] Figure 1 This is a flowchart of a method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt proposed in this invention. Figure 2 This is a dual Y-axis bar chart comparing the core performance of different samples proposed in this invention; Figure 3 This is a line graph showing the correlation between pH of component D and Zeta potential and storage stability proposed in this invention. Figure 4 This is a radar chart showing the comprehensive performance of the core sample proposed in this invention. Detailed Implementation

[0022] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] I. Preparation Example Preparation Example 1: Preparation of modified nano-SiO2 with surface-grafted epoxy groups Vaporized SiO2 nanoparticles with a particle size of 20 nm were dried in a vacuum drying oven at 120℃ for 2 hours to remove surface adsorbed water. 100 g of the dried nanoparticles were then dispersed in 1000 mL of anhydrous ethanol and ultrasonically dispersed for 30 min to obtain a uniform suspension. 3 g of γ-glycidyl etheroxypropyltrimethoxysilane (KH560) was added, and the pH of the system was adjusted to 5.5 with glacial acetic acid. The mixture was heated to 60℃ and stirred for 4 hours. After the reaction was complete, the product was centrifuged at 8000 rpm for 10 min, and the precipitate was washed three times with anhydrous ethanol to remove unreacted coupling agent. The precipitate was then dried in a vacuum drying oven at 60℃ for 24 hours and ground through a 200-mesh sieve to obtain modified nanoparticles with surface-grafted epoxy groups. This grafting reaction introduces active sites on the surface of the nanofiller that can participate in epoxy curing, solving the defects of poor compatibility and easy agglomeration of ordinary nanofillers with epoxy systems.

[0024] Preparation Example 2: Preparation of Anionic Slow-Cracking Emulsified Asphalt 70# Grade A road petroleum asphalt was selected and preheated to 140℃ for later use. Sodium dodecyl sulfate and OP-10 were compounded at a mass ratio of 2:1 to obtain anionic / nonionic composite emulsifier. The total mass of the emulsifier was 2.5% of the mass of the asphalt. The emulsifier was added to industrial pure water at 60℃ and stirred to dissolve it to obtain an emulsifier aqueous solution. The preheated asphalt and the emulsifier aqueous solution were fed into a colloid mill at a mass ratio of 6:4. The colloid mill speed was controlled at 3000 rpm and sheared and dispersed for 10 minutes. After cooling to room temperature, anionic slow-cracking emulsified asphalt with a solid content of 60% was obtained.

[0025] Preparation Example 3: Preparation of Graphene Oxide Modified with Surface Grafted Epoxy Groups 10 g of monolayer graphene oxide prepared by the Hummers method was dispersed in 1000 mL of N,N-dimethylformamide and ultrasonically dispersed for 1 h to obtain a uniform suspension. 0.5 g of KH560 was added to adjust the pH of the system to 5.5. The system was heated to 80 °C and stirred for 6 h. After the reaction was completed, the product was placed in a dialysis bag and dialyzed for 7 days to remove the solvent and unreacted coupling agent. The dialyzed product was freeze-dried for 48 h to obtain modified graphene oxide with surface grafted epoxy groups.

[0026] Preparation Example 4: Preparation of modified nanocellulose with surface-grafted epoxy groups 10g of nanocellulose with a diameter of 10-20nm and a length of 100-500nm prepared from coniferous wood pulp was dispersed in 1000mL of deionized water and ultrasonically dispersed for 40min to obtain a uniform suspension. 2g of KH560 was added to adjust the pH of the system to 5.5. The system was heated to 70℃ and stirred for 5h. After the reaction was completed, the product was centrifuged at 10000rpm for 15min. The precipitate was washed three times with deionized water and dried in a vacuum drying oven at 50℃ for 36h. The precipitate was then ground through a 200-mesh sieve to obtain modified nanocellulose with surface-grafted epoxy groups.

[0027] II. Core Implementation Examples Example 1

[0028] Group A allocation: 70 parts by weight of methacrylic resin, polyurethane-modified bisphenol A type waterborne epoxy resin, 8 parts of modified nano-SiO2 obtained in Preparation Example 1, 1 part of composite coupling agent of γ-aminopropyltriethoxysilane and KH560 in a mass ratio of 1:1, 0.3 parts of organosilicon defoamer, 15 parts of industrial pure water, and 0.4 parts of polyurethane leveling agent.

[0029] In the preparation process, modified nano-SiO2 is first added to an aqueous modified epoxy resin emulsion and dispersed at a high speed of 1000 rpm for 18 min. Then, the remaining raw materials are added and stirred evenly. The viscosity of the system is adjusted to 25 s using a Forefinger 4 cup to obtain component A. In this step, the modified nanofiller is uniformly dispersed in the epoxy system, providing active sites for the subsequent crosslinking reaction and solving the defect of poor system compatibility.

[0030] Component B is prepared by weight as follows: 70 parts modified aliphatic amine-based waterborne amine epoxy curing agent, 0.5 parts sodium polyacrylate dispersant, 2 parts propylene glycol methyl ether acetate film-forming aid, 8 parts modified nano-SiO2 obtained in Preparation Example 1, 30 parts industrial pure water, and 0.4 parts polyurethane leveling aid. In preparation, the waterborne amine epoxy curing agent is first dispersed in industrial pure water, then the dispersant is added and stirred until homogeneous. The modified nano-SiO2 is then added and dispersed at a high speed of 1000 rpm for 18 minutes. Finally, the film-forming aid is added and stirred until homogeneous to obtain component B.

[0031] Component C is prepared by mixing 70 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol, 0.5 parts of sodium polyacrylate dispersant, 30 parts of industrial pure water, and 0.4 parts of polyurethane leveling agent. All raw materials are mixed and dispersed at a low speed of 400 rpm for 18 minutes until the system is homogeneous to obtain component C.

[0032] Group D allocation: 30 parts by weight of the anionic emulsified asphalt obtained in Preparation Example 2, 45 parts of anionic double-modified waterborne epoxy resin, 10 parts of anionic chloroprene latex with a solid content of 50%, 8 parts of modified nano-SiO2 obtained in Preparation Example 1, 1.2 parts of composite coupling agent, 0.3 parts of organosilicon defoamer, 15 parts of industrial pure water, and 0.4 parts of polyurethane leveling agent.

[0033] In the preparation process, modified nano-SiO2 was first added to anionic aqueous modified epoxy resin emulsion. The emulsion was then sheared at 1000 rpm for 18 min and ultrasonically dispersed for 12 min to achieve uniform dispersion. It was then mixed with anionic emulsified asphalt and anionic chloroprene latex at 400 rpm for 12 min. The pH of the system was adjusted to 8.5 ± 0.2 using a 2% NaOH solution. The measured Zeta potential of the system was -32 mV. All components had negative Zeta potentials, achieving electrostatic stability and preventing premature demulsification, thus solving the defect of insufficient storage stability.

[0034] Application and Curing: Before application, mix components A, B, and C evenly in a mass ratio of 100:150:150 to obtain the lower layer of room temperature penetrating adhesive material. Control the coating amount to 0.25 kg / m². 2 Apply the coating to the cement concrete bridge deck substrate. After 30 minutes of surface drying, apply component D as the upper waterproof adhesive layer, controlling the application rate to 0.7 kg / m². 2 .

[0035] A gradient cross-linking curing process is adopted: In the first stage, the system is cured for 18 hours at a temperature of 25℃ and a relative humidity of 55%, during which most of the moisture in the system evaporates and the surface is dry and not sticky. In the second stage, the system is cured for 30 hours at an ambient temperature of 40℃, during which the system is completely hardened, the epoxy groups are cross-linked, the asphalt particles are fully fused, and the modified nanofiller participates in the curing reaction as both a physical cross-linking point and a chemical reaction site, forming an interpenetrating network structure. This solves the problems of difficulty in balancing rigidity and toughness and the adhesion of the construction wheel.

[0036] Example 2

[0037] Group A allocation: 70 parts by weight of methacrylic resin, polyurethane-modified bisphenol A type waterborne epoxy resin, 8 parts of modified graphene oxide obtained in Preparation Example 3, 1 part of composite coupling agent of γ-aminopropyltriethoxysilane and KH560 in a mass ratio of 1:1, 0.3 parts of organosilicon defoamer, 15 parts of industrial pure water, and 0.4 parts of polyurethane leveling agent.

[0038] In the preparation process, modified graphene oxide is first added to an aqueous modified epoxy resin emulsion and dispersed at a high speed of 1000 rpm for 18 minutes. Then, the remaining raw materials are added and stirred evenly. The viscosity of the system is adjusted to 25 seconds for a Forecast cup 4 to obtain component A.

[0039] Component B is prepared by weight as follows: 70 parts modified aliphatic amine-based waterborne amine epoxy curing agent, 0.5 parts sodium polyacrylate dispersant, 2 parts propylene glycol methyl ether acetate film-forming aid, 8 parts modified graphene oxide obtained in Preparation Example 3, 30 parts industrial pure water, and 0.4 parts polyurethane leveling aid. In preparation, the waterborne amine epoxy curing agent is first dispersed in industrial pure water, then the dispersant is added and stirred until homogeneous. The modified graphene oxide is then added and dispersed at a high speed of 1000 rpm for 18 minutes. Finally, the film-forming aid is added and stirred until homogeneous to obtain component B.

[0040] Component C is prepared by mixing 70 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol, 0.5 parts of sodium polyacrylate dispersant, 30 parts of industrial pure water, and 0.4 parts of polyurethane leveling agent. All raw materials are mixed and dispersed at a low speed of 400 rpm for 18 minutes until the system is homogeneous to obtain component C.

[0041] Group D allocation: 30 parts by weight of the anionic emulsified asphalt obtained in Preparation Example 2, 45 parts by weight of the anionic double-modified waterborne epoxy resin, 10 parts by weight of the anionic chloroprene latex with a solid content of 50%, 8 parts by weight of the modified graphene oxide obtained in Preparation Example 3, 1.2 parts by weight of the composite coupling agent, 0.3 parts by weight of the organosilicon defoamer, 15 parts by weight of industrial pure water, and 0.4 parts by weight of the polyurethane leveling agent.

[0042] In the preparation process, modified graphene oxide was first added to anionic aqueous modified epoxy resin emulsion. The emulsion was then sheared at 1000 rpm for 18 min and ultrasonically dispersed for 12 min to achieve uniform dispersion. It was then mixed with anionic emulsified asphalt and anionic chloroprene latex at 400 rpm for 12 min. The pH of the system was adjusted to 8.5 ± 0.2 using a 2% NaOH solution. The measured Zeta potential of the system was -31.8 mV, and the Zeta potential of all components was negative.

[0043] Application and Curing: Before application, mix components A, B, and C evenly in a mass ratio of 100:150:150 to obtain the lower layer of room temperature penetrating adhesive material. Control the coating amount to 0.25 kg / m². 2 Apply the coating to the cement concrete bridge deck substrate. After 30 minutes of surface drying, apply component D as the upper waterproof adhesive layer, controlling the application rate to 0.7 kg / m². 2 .

[0044] A gradient crosslinking curing process is adopted: In the first stage, the system is cured for 18 hours at a temperature of 25℃ and a relative humidity of 55%, at which point most of the water in the system evaporates and the surface is dry and not sticky. In the second stage, the system is cured for 30 hours at an ambient temperature of 40℃, at which point the system is completely hardened, the epoxy groups are crosslinked, the asphalt particles are fully fused, and the modified nanofiller participates in the curing reaction as both a physical crosslinking point and a chemical reaction site, forming an interpenetrating network structure.

[0045] Example 3

[0046] Component A is prepared by weight as follows: 60 parts methacrylic acid resin, polyurethane-modified bisphenol A type waterborne epoxy resin, 5 parts modified nano-SiO2 obtained in Preparation Example 1, 0.5 parts composite coupling agent (γ-aminopropyltriethoxysilane and KH560 in a 1:1 mass ratio), 0.1 parts organosilicon defoamer, 10 parts industrial pure water, and 0.2 parts polyurethane leveling agent. In preparation, the modified nano-SiO2 is first added to the waterborne modified epoxy resin emulsion and dispersed at 800 rpm for 15 minutes. Then, the remaining raw materials are added and stirred until homogeneous. The viscosity of the system is adjusted to 22 seconds using a Forecast 4 cup to obtain component A.

[0047] Component B is prepared by weight as follows: 60 parts of modified aliphatic amine-based waterborne amine epoxy curing agent, 0.2 parts of sodium polyacrylate dispersant, 1 part of propylene glycol methyl ether acetate film-forming aid, 5 parts of modified nano-SiO2 obtained in Preparation Example 1, 20 parts of industrial pure water, and 0.2 parts of polyurethane leveling aid. In preparation, the waterborne amine epoxy curing agent is first dispersed in industrial pure water, then the dispersant is added and stirred until homogeneous. The modified nano-SiO2 is then added and dispersed at a high speed of 800 rpm for 15 minutes. Finally, the film-forming aid is added and stirred until homogeneous to obtain component B.

[0048] Component C is prepared by mixing 60 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol, 0.2 parts by weight of sodium polyacrylate dispersant, 20 parts by weight of industrial pure water, and 0.2 parts by weight of polyurethane leveling agent. All raw materials are mixed and dispersed at a low speed of 300 rpm for 15 minutes until the system is homogeneous to obtain component C.

[0049] Group D allocation: 25 parts by weight of the anionic emulsified asphalt obtained in Preparation Example 2, 25 parts of anionic double-modified waterborne epoxy resin, 5 parts of anionic chloroprene latex with a solid content of 50%, 5 parts of modified nano-SiO2 obtained in Preparation Example 1, 0.5 parts of composite coupling agent, 0.1 parts of organosilicon defoamer, 10 parts of industrial pure water, and 0.2 parts of polyurethane leveling agent.

[0050] In the preparation process, modified nano-SiO2 was first added to anionic aqueous modified epoxy resin emulsion. The emulsion was then sheared at 800 rpm for 15 min and ultrasonically dispersed for 10 min to achieve uniform dispersion. It was then mixed with anionic emulsified asphalt and anionic chloroprene latex at 300 rpm for 10 min. The pH of the system was adjusted to 8.0 ± 0.2 using a 2% NaOH solution. The measured Zeta potential of the system was -31.4 mV. All components had negative Zeta potentials, achieving electrostatic stability and preventing premature demulsification of the system.

[0051] Application and Curing: Before application, mix components A, B, and C evenly in a mass ratio of 100:150:150 to obtain the lower layer of room temperature penetrating adhesive material. Control the coating amount to 0.2 kg / m². 2 Apply the coating to the cement concrete bridge deck substrate. After 25 minutes of surface drying, apply component D as the upper waterproof adhesive layer, controlling the application rate to 0.6 kg / m². 2 .

[0052] A gradient crosslinking curing process is adopted: In the first stage, the system is cured for 12 hours at a temperature of 20℃ and a relative humidity of 40%, during which most of the water in the system evaporates and the surface is dry and not sticky. In the second stage, the ambient temperature is adjusted to 35℃ and the system is cured for 24 hours. The system is completely hardened, the epoxy groups are crosslinked, the asphalt particles are fully fused, and the modified nanofiller participates in the curing reaction as both a physical crosslinking point and a chemical reaction site, forming a semi-interpenetrating network structure.

[0053] Example 4

[0054] Component A is prepared by weight as follows: 80 parts methacrylic acid resin, polyurethane-modified bisphenol A type waterborne epoxy resin, 10 parts modified nanocellulose obtained in Preparation Example 4, 1.5 parts composite coupling agent of γ-aminopropyltriethoxysilane and KH560 in a 1:1 mass ratio, 0.5 parts organosilicon defoamer, 20 parts industrial pure water, and 0.6 parts polyurethane leveling agent. In preparation, the modified nanocellulose is first added to the waterborne modified epoxy resin emulsion and dispersed at 1200 rpm for 20 minutes. Then, the remaining raw materials are added and stirred until homogeneous. The viscosity of the system is adjusted to 28 s using a Forecast 4 cup to obtain component A.

[0055] Component B is prepared by weight as follows: 80 parts of modified aliphatic amine-based waterborne amine epoxy curing agent, 0.8 parts of sodium polyacrylate dispersant, 3 parts of propylene glycol methyl ether acetate film-forming aid, 10 parts of modified nanocellulose obtained in Preparation Example 4, 40 parts of industrial pure water, and 0.6 parts of polyurethane leveling aid. In preparation, the waterborne amine epoxy curing agent is first dispersed in industrial pure water, then the dispersant is added and stirred until homogeneous. The modified nanocellulose is then added and dispersed at a high speed of 1200 rpm for 20 minutes. Finally, the film-forming aid is added and stirred until homogeneous to obtain component B.

[0056] Component C is prepared by mixing 80 parts by weight of 2,4,6-tris(dimethylaminomethyl)phenol, 0.8 parts by weight of sodium polyacrylate dispersant, 40 parts by weight of industrial pure water, and 0.6 parts by weight of polyurethane leveling agent. All raw materials are mixed and dispersed at a low speed of 500 rpm for 20 minutes until the system is homogeneous to obtain component C.

[0057] Group D allocation: 35 parts by weight of the anionic emulsified asphalt obtained in Preparation Example 2, 65 parts by weight of the anionic double-modified waterborne epoxy resin, 15 parts by weight of the anionic chloroprene latex with a solid content of 50%, 10 parts by weight of the modified nanocellulose obtained in Preparation Example 4, 2 parts by weight of the composite coupling agent, 0.5 parts by weight of the organosilicon defoamer, 20 parts by weight of industrial pure water, and 0.6 parts by weight of the polyurethane leveling agent.

[0058] In the preparation process, modified nanocellulose was first added to anionic aqueous modified epoxy resin emulsion. The emulsion was then sheared at 1200 rpm for 20 min and ultrasonically dispersed for 15 min to achieve uniform dispersion. It was then mixed with anionic emulsified asphalt and anionic chloroprene latex at 500 rpm for 15 min. The pH of the system was adjusted to 9.0 ± 0.2 using a 2% NaOH solution. The measured Zeta potential of the system was -30.7 mV. All components had negative Zeta potentials, achieving electrostatic stability and preventing premature demulsification of the system.

[0059] Application and Curing: Before application, mix components A, B, and C evenly in a mass ratio of 100:150:150 to obtain the lower layer of room temperature penetrating adhesive material. Control the coating amount to 0.3 kg / m². 2Apply the coating to the cement concrete bridge deck substrate and allow it to surface dry for 35 minutes. Then apply component D as the upper waterproof adhesive layer, controlling the application rate to be 0.8 kg / m². 2 A gradient cross-linking curing process is adopted: In the first stage, the system is cured for 24 hours at 30℃ and 70% relative humidity, during which most of the moisture in the system evaporates and the surface is dry and non-sticky; in the second stage, the ambient temperature is adjusted to 45℃ and cured for 36 hours, during which the system is completely hardened, the epoxy groups are cross-linked, the asphalt particles are fully fused, and the modified nanocellulose participates in the curing reaction as both a physical cross-linking point and a chemical reaction site, forming a highly dense interpenetrating network structure. This solves the problems of difficulty in balancing rigidity and toughness under heavy load conditions and wheel sticking during high-temperature construction.

[0060] Comparative Example 1 This comparative example is based on existing common waterborne epoxy asphalt technology. All formulations, preparation processes, and curing parameters are completely consistent with Example 1, except that no modified nanofillers are added.

[0061] Comparative Example 2 This comparative example is an existing technical solution with added unmodified nanofillers. All formulations, preparation processes, and curing parameters are completely consistent with Example 1, except that the modified nano-SiO2 is replaced with an equal amount of unmodified ordinary gas-phase nano-SiO2.

[0062] Component A is prepared by weight as follows: 70 parts methacrylic resin, polyurethane-modified bisphenol A type waterborne epoxy resin, 8 parts unmodified ordinary nano-SiO2, 1 part a composite coupling agent (γ-aminopropyltriethoxysilane and KH560 in a 1:1 mass ratio), 0.3 parts silicone defoamer, 15 parts industrial pure water, and 0.4 parts polyurethane leveling agent. In preparation, unmodified nano-SiO2 is first added to the waterborne modified epoxy resin emulsion and dispersed at 1000 rpm for 18 minutes. Then, the remaining raw materials are added and stirred until homogeneous. The viscosity of the system is adjusted to 25 seconds using a Forecast 4 cup to obtain component A.

[0063] The preparation, application, and curing steps for the remaining components are completely consistent with those in Example 1.

[0064] Comparative Example 3 This comparative example is an existing room-temperature curing waterborne epoxy asphalt technology solution. All formulations and component preparation processes are completely consistent with Example 1, except that the gradient curing process is replaced with continuous curing at room temperature of 25°C and relative humidity of 55% for 48 hours.

[0065] IV. Explanation of Reaction Molecular Formula hydroxyl reaction formula on the surface of KH560 grafted nanofiller: ≡Si-OH+(CH3O)3SiCH2CH2CH2OCH2CH(O)CH2→≡Si-O-Si(OCH3)2CH2CH2CH2OCH2CH(O)CH2+ CH3OH, where "CH(O)CH2" represents the epoxy three-membered ring structure. In this reaction, the epoxy groups grafted on the surface of the nanofiller simultaneously participate in cross-linking, forming a three-dimensional cross-linked network with nanoparticles as chemical anchors. This improves the density and mechanical properties of the system, and solves the defects of ordinary epoxy cross-linked networks, such as high brittleness and poor weather resistance.

[0066] The epoxy-amine crosslinking curing reaction formula is: ~CH2CH(O)CH2+ H2N-R-NH2→ ~CH2CH(OH)CH2-NH-R-NH-CH2CH(OH)CH2~. In this reaction, the epoxy groups grafted on the surface of the nanofiller participate in crosslinking at the same time, forming a multi-dimensional three-dimensional crosslinking network, which improves the density and mechanical properties of the system and solves the defects of ordinary epoxy crosslinking networks such as high brittleness and poor weather resistance.

[0067] V. Performance Testing and Data All test methods adopted current transportation industry standards: storage stability was tested according to GB / T 16777-2008, which determined the stratification rate after 5 days of storage; bond strength was tested according to JT / T 535-2019, which determined the tensile bond strength at 25℃; low-temperature flexibility was tested according to GB / T16777-2008, which determined the crack width after bending 180° at -10℃; water resistance was tested according to JT / T 535-2019, which determined the bond strength retention rate after boiling in water for 7 days; and construction anti-adhesion was tested by rolling the material 10 times with a rubber tire at 60℃ and recording the proportion of adhesive material mass.

[0068] Table 1. Test results of core performance of each sample

[0069] As shown in the table, the 5-day delamination rate of all four examples is less than 1%, which is much lower than that of the comparative example. This confirms that the charge-matching design and the introduction of modified nanofillers effectively solve the defects of easy demulsification and delamination and poor storage stability of the existing technology system. The bonding strength and water boiling retention rate of the examples are significantly higher than those of the comparative example. There are no cracks when bending at low temperature and the amount of material adhering to the material when rolling at high temperature is negligible. This confirms that the multi-dimensional cross-linking network and gradient curing process simultaneously solve the defects of existing technology, such as difficulty in balancing rigidity and toughness, poor weather resistance, and poor construction adaptability. The performance is stable under different dimensional fillers and upper and lower limit parameters, which verifies the adaptability of the technical solution.

[0070] Table 2. Zeta potential and storage stability of component D at different pH values

[0071] As shown in the table, when the pH of the system is in the range of 8.0-9.0 as specified by the technical requirements, the absolute value of the Zeta potential of the system is greater than 30mV, which is in the electrostatic stability range. The 5-day stratification rate is less than 1%, and the storage performance is optimal. This confirms that pH control achieves charge matching of the entire system and effectively solves the problem of premature demulsification caused by charge incompatibility of different components.

[0072] refer to Figure 2 This figure visually presents the core performance differences between the four embodiments and the three comparative examples. The 25°C tensile bond strength of all embodiments is higher than 2.6 MPa, which is much higher than the highest value of 2.1 MPa of the three comparative examples. This confirms that the nanofiller with surface-grafted epoxy groups participates in the reaction as a crosslinking site, effectively improving the crosslinking density of the system and solving the defect of insufficient mechanical strength in the prior art. The 5-day storage stratification rate of the embodiments is less than 1%, which is much lower than 4.2% of comparative example 1 and 7.5% of comparative example 2. It is only comparable to comparative example 3 with no change in formulation. This confirms that the charge matching design of the whole system effectively solves the defects of component incompatibility and easy premature demulsification and stratification in the prior art. The stratification rate of comparative example 2 is the highest because the surface charge of the unmodified nano SiO2 is incompatible with the system, making it easy to agglomerate and settle.

[0073] refer to Figure 3 This figure clearly shows the correlation between the pH value of component D and the zeta potential and storage stability of the system. When the pH is within the technically defined range of 8.0 to 9.0, the absolute value of the zeta potential of the system is higher than 30 mV, which is above the electrostatic stability threshold of the colloidal system. The corresponding stratification rate after 5 days of storage is less than 1%. The optimal value is reached at pH 8.5, with a zeta potential of -32.1 mV and a stratification rate of only 0.6%. When the pH is lower than 8.0 or higher than 9.0, the absolute value of the zeta potential drops rapidly to below 30 mV, and the stratification rate increases to more than 2%. This confirms that pH control achieves charge consistency among the modified nanofiller, anionic emulsified asphalt, and anionic waterborne epoxy, effectively avoiding demulsification and flocculation problems caused by charge mismatch between different components. This provides quantitative support for the storage stability of the system and verifies the scientific validity of the pH range defined by the technical requirements.

[0074] refer to Figure 4This figure compares the overall performance of Example 1 with two typical comparative examples from five core performance dimensions. Example 1's performance in all five dimensions is in the high range above 0.9, achieving a synergistic improvement in all performance aspects. Comparative Example 1 did not add nanofillers, and only its water resistance was at a medium level, while the other performances were in the low range, failing to meet the multiple requirements of storage, mechanics, and construction simultaneously. Comparative Example 3 used a room temperature curing process, and only its storage stability was comparable to Example 1, while the other performances, especially the anti-sticking performance, were far lower than those of Example 1. This confirms that the gradient curing process, by controlling the matching of the rates of water evaporation, epoxy crosslinking, and asphalt fusion, effectively solves the defects of existing technologies, such as difficulty in balancing rigidity and toughness and easy sticking during high-temperature construction, and can adapt to the engineering application needs under complex working conditions.

[0075] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt, characterized in that, Includes the following steps: S1. Preparation of the lower layer room temperature penetrating adhesive material: Prepare components A, B, and C separately. Before construction, mix components A, B, and C evenly in a mass ratio of 100:150:

150. Component A contains water-based modified epoxy resin, modified nanofiller, and composite coupling agent; component B contains water-based amine epoxy curing agent, modified nanofiller, and film-forming aid; and component C contains water-based epoxy curing accelerator. The modified nanofiller is one or more of zero-dimensional, one-dimensional, and two-dimensional nanofillers, and the surface of the modified nanofiller is grafted with epoxy groups. S2. Preparation of component D of the upper thermosetting second-order reactive waterproof adhesive material: Anionic emulsified asphalt was prepared using anionic / nonionic emulsifiers. Modified nanofillers were dispersed in anionic waterborne modified epoxy resin emulsion, and then mixed with anionic emulsified asphalt and anionic chloroprene latex. The pH of the system was adjusted to match the surface charge of the modified nanofillers, and the mixture was stirred evenly to obtain component D. S3, Gradient crosslinking curing: First, apply the lower layer of room temperature penetrating adhesive material to the substrate to be treated and wait for it to dry on the surface. Then, apply component D. Control the temperature and humidity of the curing environment so that water evaporation, epoxy crosslinking, and asphalt particle fusion can proceed simultaneously. The modified nanofiller also participates in the epoxy curing reaction as a physical crosslinking point and a chemical reaction site, forming an interpenetrating network or semi-interpenetrating network structure, thus obtaining the target product.

2. The preparation method of a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, The zero-dimensional nanofiller with surface-grafted epoxy groups is nano-silica or nano-calcium carbonate modified with a silane coupling agent, the one-dimensional nanofiller is carbon nanotube or nano-cellulose with surface-grafted epoxy groups, and the two-dimensional nanofiller is graphene oxide with surface-grafted epoxy groups.

3. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, Component A comprises, by weight, 60-80 parts of waterborne modified epoxy resin, 5-10 parts of modified nanofiller, 0.5-1.5 parts of composite coupling agent, 0.1-0.5 parts of defoamer, 10-20 parts of industrial pure water, and 0.2-0.6 parts of additives. In preparation, the modified nanofiller is added to the waterborne modified epoxy resin emulsion and dispersed at 800-1200 rpm for 15-20 minutes. The remaining raw materials are then added and stirred until homogeneous, and the viscosity is adjusted accordingly.

4. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, Component B comprises, by weight, 60-80 parts of waterborne amine epoxy curing agent, 0.2-0.8 parts of dispersant, 1-3 parts of film-forming aid, 5-10 parts of modified nanofiller, 20-40 parts of industrial pure water, and 0.2-0.6 parts of additives. In preparation, the waterborne amine epoxy curing agent is first dispersed in water, then the dispersant is added and stirred until homogeneous. The modified nanofiller is then added and dispersed at 800-1200 rpm for 15-20 minutes. Finally, the film-forming aid is added and stirred until homogeneous.

5. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, Component C comprises, by weight, 60-80 parts of waterborne epoxy curing agent accelerator, wherein the waterborne epoxy curing agent accelerator is selected from one or more of 2,4,6-tris(dimethylaminomethyl)phenol (DMP-30), benzyldimethylamine, and 2-methylimidazole, and further comprises 0.2-0.8 parts of dispersant, 20-40 parts of industrial pure water, and 0.2-0.6 parts of additives; during preparation, all raw materials are mixed and dispersed at 300-500 rpm for 15-20 minutes until the system is homogeneous.

6. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, The D component, by weight, comprises 25-35 parts anionic emulsified asphalt, 25-65 parts anionic waterborne modified epoxy resin, 5-15 parts anionic chloroprene latex, 5-10 parts modified nanofiller, 0.5-2 parts composite coupling agent, 0.1-0.5 parts defoamer, 10-20 parts industrial pure water, and 0.2-0.6 parts additives.

7. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 6, characterized in that, When preparing component D, the modified nanofiller is first added to anionic aqueous modified epoxy resin emulsion, and then sheared at 800~1200 rpm for 15~20 min and ultrasonically dispersed for 10~15 min. Then, it is mixed with anionic emulsified asphalt and anionic chloroprene latex at 300~500 rpm for 10~15 min. The pH of the system is adjusted to 8.0~9.0 to match the charge of the negatively charged modified nanofiller.

8. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt according to claim 1, characterized in that, The control conditions for gradient crosslinking curing in S3 are as follows: first, cure for 12-24 hours at a temperature of 20-30℃ and a relative humidity of 40%-70%, and then cure for 24-36 hours at an ambient temperature of 35-45℃.

9. The preparation method of a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt as described in claim 1, characterized in that, The anionic emulsified asphalt is anionic slow-cracking type 70# emulsified asphalt with a solid content of 50%~65%, and the anionic waterborne modified epoxy resin is a bisphenol A type waterborne epoxy resin modified by methacrylic acid resin and polyurethane; the composite coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-methacryloyloxypropyltrimethoxysilane.

10. The method for preparing a high-density, crack-resistant nano-modified composite waterborne epoxy asphalt as described in claim 1, characterized in that, The coating amount of the lower layer of S3 room temperature penetrating adhesive is 0.2~0.3 kg / m². 2 After surface drying, the coating amount of component D is 0.6~0.8 kg / m². 2 After coating, seal and cure for 48 hours before proceeding with the subsequent paving process.