An environmentally friendly biodegradable adhesive tape for packaging materials and its preparation method
By optimizing the composition and structure of the substrate layer of the environmentally friendly tape and utilizing materials such as polylactic acid, starch, plasticizers, and alkyl ketene dimers, the problems of low strength and poor adhesion of the environmentally friendly tape have been solved, resulting in environmentally friendly tapes with high strength, wear resistance, and long service life.
Patent Information
- Application Number
- CN202410224038.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-29
- Publication Date
- 2026-11-17
AI Technical Summary
Existing environmentally friendly tapes suffer from low strength, easy breakage, and poor adhesion.
Polylactic acid, starch, plasticizer and alkyl ketene dimer are used as substrate layer materials, and starch-based biodegradable adhesive is used in the adhesive layer. The composition and structure of the substrate layer are optimized by combining vermiculite, straw ultrafine powder and silicone rubber.
It improves the strength, abrasion resistance, hydrophobicity and low-temperature toughness of the tape, extends its service life and enhances its environmental friendliness.
Smart Images

Figure BDA0004718985140000091 
Figure BDA0004718985140000101 
Figure BDA0004718985140000121
Abstract
Description
Technical Field
[0001] This application relates to the technical field of adhesive tapes, and more specifically, to an environmentally friendly biodegradable adhesive tape for packaging materials and a method for preparing the same. Background Technology
[0002] Packaging tape, also known as BOPP tape or sealing tape, is a roll of adhesive tape made by coating pressure-sensitive adhesive evenly onto plastic films such as BOPP, PVC, PET, and PE. It is an indispensable item in daily life.
[0003] Adhesive tapes used in packaging are typically torn off and discarded. However, since the base layer of these tapes is mostly a film made of materials such as BOPP, PVC, PET, and PE, these materials cannot be degraded or recycled and can only be disposed of through incineration, leading to environmental pollution. While environmentally friendly tapes exist on the market, most suffer from low strength, easy breakage, and poor adhesion. Summary of the Invention
[0004] To address the shortcomings of environmentally friendly adhesive tapes, such as low strength, easy breakage, and poor adhesion, this application provides an environmentally friendly biodegradable adhesive tape for packaging materials and its preparation method, employing the following technical solution:
[0005] In a first aspect, this application provides an environmentally friendly biodegradable tape for packaging materials, comprising a substrate layer and an adhesive layer, wherein the substrate layer comprises the following materials in parts by weight: 60-80 parts polylactic acid, 40-50 parts starch, 5-25 parts plasticizer, and 8-10 parts alkyl ketene dimer.
[0006] The adhesive layer comprises a starch-based biodegradable adhesive.
[0007] By adopting the above technical solution, polylactic acid (PLA) possesses excellent physicochemical properties and is widely available and recyclable. Starch also exhibits good environmental friendliness. Therefore, this application preferably uses a combination of starch and PLA. Starch can fill the continuous phase of PLA, reducing the amount of PLA added, lowering the cost of the substrate layer, and maintaining the high flexibility and strength of PLA. The addition of plasticizers can insert into the gaps between the PLA and starch system, reducing intermolecular stress, enhancing chain segment mobility, and thus improving the compatibility and interfacial bonding strength between starch and PLA. Simultaneously, the amount of plasticizer added is optimized; a suitable amount of plasticizer can improve the tensile strength of the substrate layer. Preferably, a biodegradable adhesive is used as the adhesive layer, which can further improve the biodegradability of the tape and enhance its environmental friendliness.
[0008] This application preferably adds an alkyl ketene dimer to the substrate layer. The alkyl ketene dimer has a highly chemically active lactone ring that can react with the hydroxyl groups in starch to undergo hydroxyl esterification, thereby grafting long-chain alkyl groups onto the starch surface. This not only reduces the active hydrophilic groups on the surface of the substrate layer but also introduces long-chain alkyl groups, thereby effectively improving the hydrophobicity of the substrate layer and thus increasing the service life of the tape.
[0009] Optionally, the substrate layer may further include 5-10 parts by weight of straw ultrafine powder or sorghum ultrafine powder.
[0010] By adopting the above technical solution, straw, consisting mostly of the stems and leaves of mature crops and primarily agricultural waste, and sweet sorghum, also known as sorghum pomace, which can be used for sugar production and brewing, are both valuable. Both straw and sweet sorghum pomace contain significant amounts of cellulose and lignin. Adding these to the substrate layer increases the tensile strength between components, improves the density, strength, and hydrophobicity of the substrate layer. Simultaneously, the lignin in the sweet sorghum pomace, with its network structure, further enhances the strength of the fiber network in the substrate layer, thereby further improving its strength and density. Preparing both straw and sweet sorghum pomace into ultrafine powder mechanically activates them, resulting in a loose crystal structure and uniform strength in the substrate layer. Furthermore, pulverizing the straw and sweet sorghum pomace into ultrafine powder can, to a certain extent, increase the bonding effect between the substrate layer and the adhesive layer, thus imparting excellent strength and bonding strength to the biodegradable tape.
[0011] Optionally, the straw ultrafine powder or sorghum ultrafine powder is loaded with vermiculite.
[0012] By adopting the above technical solution, vermiculite, a layered silicate mineral, possesses excellent intercalation properties due to its layered structure, enabling it to bond strongly with other components in the substrate layer. Using vermiculite loaded onto straw ultrafine powder or sorghum ultrafine powder firstly enhances the strength of the fiber network within the powder, further improving the strength and toughness of the substrate layer. Secondly, the addition of vermiculite increases the amount of wear-resistant particles in the substrate layer, improving the tape's abrasion resistance and extending its service life. Simultaneously, vermiculite exhibits good frost resistance and heat resistance, effectively improving the substrate layer's frost resistance and reducing the likelihood of tape breakage in winter.
[0013] Optionally, the vermiculite is vermiculite sheets modified with hexadecyltrimethylammonium bromide.
[0014] By adopting the above technical solution, hexadecyltrimethylammonium bromide is used to modify vermiculite. Hexadecyltrimethylammonium bromide can enter between the layers of vermiculite, enabling vermiculite to form a layered structure and graft organic groups, which effectively improves the dispersion uniformity of vermiculite in the substrate layer. At the same time, it can form a shielding layer in the substrate layer, which can further improve the wear resistance of the substrate layer and extend the service life of the tape.
[0015] Optionally, the preparation method of vermiculite-loaded ultrafine powder of sorghum includes: placing sorghum ultrafine powder in a phosphoric acid modification solution, stirring and mixing to obtain modified sorghum ultrafine powder; dispersing vermiculite in an ethanol solution to obtain a dispersion; adding modified lignin to the dispersion, stirring and mixing, aging, and spray drying to obtain sorghum ultrafine powder loaded with vermiculite.
[0016] Optionally, the substrate layer may further include 5-10 parts by weight of silicone rubber.
[0017] By adopting the above technical solution, since the main chain of silicone rubber molecules is Si-O bond, the distance between the two atoms is short, the bond energy is high, and it is not easy to break at high temperature. The molecular chain has good flexibility, which makes silicone rubber have better high and low temperature resistance and high elasticity. Therefore, adding silicone rubber to the substrate layer can effectively improve the low temperature toughness of the substrate layer. In other words, in areas with low winter temperatures, the tape is not easy to break or shatter due to low temperature, thus extending the service life of the tape.
[0018] Optionally, the silicone rubber is an epoxy-modified silicone rubber.
[0019] By adopting the above technical solution, epoxy groups are grafted onto silicone rubber. The epoxy groups react with polylactic acid end groups, thereby effectively improving the compatibility between silicone rubber and the substrate layer. This results in the substrate layer obtaining uniform toughness and low-temperature resistance, further extending the service life of the tape.
[0020] Optionally, the polylactic acid is selected from any one of REVODE 101, REVODE 110, and REVODE 1711B.
[0021] Optionally, the biodegradable adhesive comprises the following materials in parts by weight: 40-50 parts starch, 0.4-0.5 parts nanocellulose, 0.16-0.2 parts ferrous sulfate, 20-30 parts hydrogen peroxide, 4-5 parts sodium hydroxide, 0.05-0.1 parts sodium tetraborate, 0.05-0.1 parts tributyl phosphate, and 1-2 parts borax.
[0022] By employing the above technical solution and using starch as the substrate of the biodegradable adhesive, the bonding strength between the adhesive and the substrate layer is improved by utilizing the principle of "like dissolves like." Adding nanocellulose to the adhesive allows it to penetrate starch molecules and fill their pores, effectively increasing the adhesive's viscosity and bonding strength. The addition of nanocellulose introduces a fibrous network structure into the adhesive, increasing its specific surface area. Furthermore, the addition of cellulose allows the fibrous structures in the adhesive layer and the substrate layer to intertwine, further enhancing the bonding effect between the adhesive and the substrate layer.
[0023] Secondly, this application provides a method for preparing environmentally friendly biodegradable adhesive tape for packaging materials, using the following technical solution:
[0024] A method for preparing an environmentally friendly biodegradable adhesive tape for packaging materials includes the following steps:
[0025] S1. Preparation of substrate layer: Mix starch with solvent, gelatinize in water bath, add alkyl ketene dimer and polylactic acid, continue heating and stirring, then add plasticizer to obtain film-forming liquid, cast into film, dry to obtain substrate layer;
[0026] S2. Tape preparation: A release agent is coated on one side of the substrate layer, and a biodegradable adhesive is coated on the other side of the substrate layer to prepare the tape.
[0027] In summary, this application has the following beneficial effects:
[0028] 1. Since this application preferably uses a combination of starch and polylactic acid (PLA), starch can fill the continuous phase of PLA, reducing the amount of PLA added, lowering the cost of the substrate layer, and maintaining the high flexibility and strength of PLA. The addition of plasticizers can insert into the gaps between the PLA and starch system, reducing intermolecular stress, improving chain segment mobility, and thus improving the compatibility and interfacial bonding strength between starch and PLA. Simultaneously, the addition of alkyl ketene dimers to the substrate layer, which have a highly chemically active lactone ring, can react with the hydroxyl groups in starch to undergo hydroxyl esterification, thereby grafting long-chain alkyl groups onto the starch surface. This not only reduces the active hydrophilic groups on the substrate layer surface but also introduces long-chain alkyl groups, effectively improving the hydrophobicity of the substrate layer and thus increasing the tape's service life.
[0029] 2. Since both straw and sorghum residue contain abundant cellulose and lignin, adding them to the substrate layer can increase the tensile strength between the components, improve the density, strength, and hydrophobicity of the substrate layer. Simultaneously, the lignin in sorghum residue, with its network structure, can further enhance the strength of the fiber network in the substrate layer, thereby further improving its strength and density. Preparing both straw and sorghum residue into ultrafine powder mechanically activates them, resulting in a loose crystal structure and uniform strength in the substrate layer. Furthermore, pulverizing straw and sorghum residue into ultrafine powder can, to a certain extent, increase the bonding effect between the substrate layer and the adhesive layer, thus imparting excellent strength and bonding strength to the biodegradable tape.
[0030] 3. This application utilizes vermiculite loaded onto straw ultrafine powder or sorghum ultrafine powder. Firstly, it enhances the strength of the fiber network in the straw ultrafine powder or sorghum ultrafine powder, further improving the strength and toughness of the substrate layer. Secondly, the addition of vermiculite increases the number of wear-resistant particles in the substrate layer, improving the tape's wear resistance and extending its service life. Simultaneously, vermiculite possesses excellent frost resistance and heat resistance, effectively improving the frost resistance of the substrate layer and reducing the likelihood of tape breakage in winter.
[0031] 4. Because the main chain of silicone rubber molecules is Si-O bond, the distance between the two atoms is short and the bond energy is high. It is not easy to break at high temperature and the molecular chain has good flexibility. As a result, silicone rubber has better high and low temperature resistance and high elasticity. Therefore, adding silicone rubber to the substrate layer can effectively improve the low temperature toughness of the substrate layer. In other words, in areas with low winter temperatures, the tape is not easy to break or shatter due to low temperature, thus extending the service life of the tape. Detailed Implementation
[0032] The present application will be further described in detail below with reference to the embodiments.
[0033] The drugs selected in this application embodiment are shown below, but are not limited thereto:
[0034] Pharmaceuticals: Alkyl ketene dimer is alkyl ketene dimer from Maclean Biochemical Technology Co., Ltd.; vermiculite is natural vermiculite from Pengjian Mineral Products Processing Plant in Lingshou County, Hebei Province; poppy residue is the product after poppy pressing; reagents are commercially available standard reagents.
[0035] Preparation Example
[0036] Example of preparation of ultrafine powder of sorghum stalks
[0037] Preparation Example 1
[0038] Wash and dry the sorghum residue, place it in a vibrating pulverizer, and grind it for 15 minutes at a power of 1.1kW to obtain sorghum ultrafine powder.
[0039] Preparation Example 2
[0040] Mix 0.358 kg of sodium hydrogen phosphate hydrate with 0.5 L of water, stir at 50 °C for 15 min, add 0.1 kg of epichlorohydrin, and react at 85 °C for 1 h to obtain sodium 3-chloro-2-hydroxypropyl phosphate. Recrystallize and purify to obtain a sodium 3-chloro-2-hydroxypropyl phosphate solution. Add 20% sodium hydroxide to adjust the pH to 11, add 1.8 kg of psyllium husk ultrafine powder, and react at 85 °C for 1.5 h to obtain phosphoric acid modified micro powder.
[0041] 0.1 kg of vermiculite was dispersed in an ethanol solution (ethanol:water = 2:1) and ultrasonically dispersed. Then, 0.12 kg of phosphoric acid modified micro powder was added, stirred and mixed, and the pH was adjusted to 3.5. The mixture was aged at 50°C for 1 hour and spray-dried to obtain vermiculite-loaded sorghum ultrafine powder.
[0042] Preparation Example 3
[0043] Mix 0.358 kg of sodium hydrogen phosphate hydrate with 0.5 L of water, stir at 50 °C for 15 min, add 0.1 kg of epichlorohydrin, and react at 85 °C for 1 h to obtain sodium 3-chloro-2-hydroxypropyl phosphate. Recrystallize and purify to obtain a sodium 3-chloro-2-hydroxypropyl phosphate solution. Add 20% sodium hydroxide to adjust the pH to 11, add 1.8 kg of psyllium husk ultrafine powder, and react at 85 °C for 1.5 h to obtain phosphoric acid modified micro powder.
[0044] The vermiculite was pulverized and passed through a 200-mesh sieve to obtain pulverized vermiculite. The pulverized vermiculite was placed in a hydrochloric acid solution, stirred at 75°C for 2 hours, allowed to stand for 2 hours, washed with deionized water, and dried at 80°C to obtain acidified vermiculite. The acidified vermiculite was placed in a hexadecyltrimethylammonium bromide solution, stirred at 60°C for 2 hours, allowed to stand for 12 hours, filtered, and the solid was retained. The solid was washed three times with water and dried at 80°C to obtain modified vermiculite.
[0045] 0.1 kg of modified vermiculite was dispersed in an ethanol solution (ethanol:water = 2:1) and ultrasonically dispersed. Then, 0.12 kg of phosphoric acid modified micro powder was added, stirred and mixed, and the pH was adjusted to 3.5. The mixture was aged at 50°C for 1 hour and spray-dried to obtain vermiculite-loaded sorghum ultrafine powder.
[0046] Preparation Example 4
[0047] Mix 0.358 kg of sodium hydrogen phosphate hydrate with 0.5 L of water, stir at 50 °C for 15 min, add 0.1 kg of epichlorohydrin, and react at 85 °C for 1 h to obtain sodium 3-chloro-2-hydroxypropyl phosphate. Recrystallize and purify to obtain a sodium 3-chloro-2-hydroxypropyl phosphate solution. Add 20% sodium hydroxide to adjust the pH to 11, add 1.8 kg of psyllium husk ultrafine powder, and react at 85 °C for 1.5 h to obtain phosphoric acid modified micro powder.
[0048] The vermiculite was pulverized and passed through a 200-mesh sieve to obtain pulverized vermiculite. 0.1 kg of the pulverized vermiculite was placed in 1 L of 0.006 mmol / L hydrochloric acid solution, stirred at 75°C for 2 h, allowed to stand for 2 h, washed with deionized water, and dried at 80°C to obtain acidified vermiculite. The acidified vermiculite was placed in a hexadecyltrimethylammonium bromide solution, stirred at 60°C for 2 h, allowed to stand for 12 h, filtered, and the solid was retained. The solid was washed three times with water and dried at 80°C to obtain modified vermiculite.
[0049] 0.1 kg of modified vermiculite was placed in 0.1 L of 2% polyvinyl alcohol solution and ground (colloidal mill slit width of 1 μm, grinding time of 40 min), filtered, the solid was retained, and dried to obtain lamellar vermiculite.
[0050] 0.1 kg of lamellar vermiculite was dispersed in an ethanol solution (ethanol:water = 2:1) and ultrasonically dispersed. Then, 0.12 kg of phosphoric acid modified micro powder was added, stirred and mixed, and the pH was adjusted to 3.5. The mixture was aged at 50°C for 1 h and spray-dried to obtain vermiculite-loaded sorghum ultrafine powder.
[0051] Example of preparation of epoxy modified silicone rubber
[0052] Preparation Example 5
[0053] 700 mL of chloroform solvent and 21 g of phenyl silicone rubber were added to a container and stirred at 25 °C. After the phenyl silicone rubber was completely dissolved, 12.48 g of meta-monochloroperoxybenzoic acid was added. After a reaction of 96 h, the rubber was precipitated with methanol, washed several times, and dried in a vacuum oven at 40 °C for 12 h to obtain epoxy modified silicone rubber.
[0054] Example
[0055] Examples 1-3
[0056] On the one hand, this application provides an environmentally friendly biodegradable tape for packaging materials, including a substrate layer and an adhesive layer. The substrate layer includes the following materials: polylactic acid, starch, plasticizer, and alkyl ketene dimer, the specific quantities of which are shown in the table below.
[0057] Optionally, the plasticizer can be epoxidized soybean oil or tributyl acetylacetonate. Specifically, in this embodiment, tributyl acetylacetonate is selected as the plasticizer. The starch is thermoplastic starch (HL-100C food grade), and the polylactic acid is REVODE 101 (melting point 150-155℃, tensile strength ≥50MPa, elongation at break ≥3%).
[0058] The adhesive layer comprises a starch-based biodegradable adhesive, which includes 40 parts by weight of starch, 0.4 parts by weight of nanocellulose, 0.16 parts by weight of ferrous sulfate, 20 parts by weight of hydrogen peroxide, 4 parts by weight of sodium hydroxide, 0.05 parts by weight of sodium tetraborate, 0.05 parts by weight of tributyl phosphate and 1 part by weight of borax.
[0059] On the other hand, this application provides a method for preparing environmentally friendly biodegradable adhesive tape for packaging materials, comprising the following steps:
[0060] S1. Preparation of substrate layer: Starch and solvent (100:15 water and glycerol) are mixed at a mass ratio of 5:115, gelatinized in a water bath at 95°C, alkyl ketene dimer is added, and heating is continued at 65°C until the alkyl ketene dimer melts. The mixture is dried at 95°C for 24 hours, pulverized, and the modified starch is obtained. The modified starch, plasticizer, and polylactic acid are mixed at 150°C for 15 minutes, hot-pressed into a film, and dried to obtain the substrate layer.
[0061] S2. Tape preparation: A release agent is coated on one side of the substrate layer, and a biodegradable adhesive is coated on the other side of the substrate layer to prepare the tape.
[0062] Table 1. Substrate layer composition in Examples 1-3
[0063]
[0064]
[0065] Examples 4-5
[0066] The difference from Example 1 is that the adhesive layer includes a starch-based biodegradable adhesive, which includes starch, nanocellulose, ferrous sulfate, hydrogen peroxide, sodium hydroxide, sodium tetraborate, tributyl phosphate and borax, with specific quantities shown in the table below.
[0067] Table 2 Adhesive composition of Examples 1 and 4-5
[0068] weight / kg Example 2 Example 4 Example 5 starch 40 45 50 Nanocellulose 0.4 0.45 0.5 Ferrous sulfate 0.16 0.18 0.20 hydrogen peroxide 20 25 30 Sodium hydroxide 4 4.5 5 Sodium tetraborate 0.05 0.07 0.10 Tributyl phosphate 0.05 0.07 0.10 Borax 1 1.5 2
[0069] Example 6
[0070] The difference from Example 1 is that the substrate layer also includes 8 kg of the sorghum ultrafine powder from Example 1.
[0071] Example 7
[0072] The difference from Example 1 is that the substrate layer also includes 8 kg of vermiculite-loaded prickly ash ultrafine powder from Preparation Example 2.
[0073] Example 8
[0074] The difference from Example 1 is that the substrate layer also includes 4 kg of vermiculite-loaded ultrafine powder of sorghum as in Preparation Example 2 and 4 kg of vermiculite-loaded ultrafine powder of sorghum as in Preparation Example 3.
[0075] Example 9
[0076] The difference from Example 1 is that the substrate layer also includes 4 kg of vermiculite-loaded sorghum ultrafine powder from Preparation Example 2 and 4 kg of vermiculite-loaded sorghum ultrafine powder from Preparation Example 4.
[0077] Example 10
[0078] The difference from Example 6 is that the substrate layer also includes 8 kg of silicone rubber.
[0079] Example 11
[0080] The difference from Example 6 is that the substrate layer also includes 8 kg of the epoxy-modified silicone rubber prepared in Example 5.
[0081] Example 12
[0082] The difference from Example 1 is that the polylactic acid in this example is REVODE 110, which replaces the polylactic acid in Example 1 to prepare the substrate layer.
[0083] Example 13
[0084] The difference from Example 1 is that the polylactic acid in this example is REVODE 1711B, which is used instead of the polylactic acid in Example 1 to prepare the substrate layer.
[0085] Comparative Example
[0086] Comparative Example 1
[0087] The difference between this comparative example and Example 3 is that no alkyl ketene dimer was added in this comparative example.
[0088] Comparative Example 2
[0089] The difference between this comparative example and Example 3 is that no nanocellulose was added to the adhesive in this comparative example.
[0090] Performance testing
[0091] (1) Water contact angle test: The water contact angle of the biodegradable tape is tested using a water contact angle meter. The larger the water contact angle, the better the hydrophobic effect.
[0092] (2) Mechanical property testing: The biodegradable tape was tested using a universal testing machine to test its tensile strength and elongation at break;
[0093] (3) Abrasion resistance test: The substrate layer was cut into strips 220 nm long and 10 mm wide and tested on an abrasion testing machine. During the test, 800 grit sandpaper was used, the pressure was 250 g, the number of friction cycles was 1000, and the wear was calculated.
[0094] Table 3 Performance Testing
[0095]
[0096]
[0097] The 180° peel strength of the tapes in Examples 2 and 4-5 is greater than 3.8 N / cm; the peel strength of the tape in Comparative Example 2 is 3.5 N / cm.
[0098] By comparing the performance test results in Table 3, we can find that:
[0099] 1. A comparison of Examples 1-3 and Comparative Example 1 reveals that the water contact angle and tensile strength of the substrate layer prepared in Examples 1-3 are improved, while abrasion is reduced. This indicates that the combination of starch and polylactic acid in this application can maintain the high flexibility and strength of polylactic acid. The addition of plasticizer can insert into the gaps between the polylactic acid and starch system, improving the compatibility and interfacial bonding strength between starch and polylactic acid. Simultaneously, the amount of plasticizer added was optimized; an appropriate amount of plasticizer can improve the tensile strength of the substrate layer. Adding alkyl ketene dimers to the substrate layer allows them to react with the hydroxyl groups in starch, undergoing hydroxyl esterification, and subsequently grafting long-chain alkyl groups onto the starch surface, effectively improving the hydrophobicity of the substrate layer and thus increasing the service life of the tape.
[0100] 2. A comparison of Examples 4-5 and Comparative Example 1 reveals that the peel strength of the tapes prepared in Examples 4-5 is improved. This indicates that the addition of nanocellulose in this application can introduce a fiber network structure into the adhesive, increasing the specific surface area of the adhesive. The addition of cellulose allows the fiber structure in the adhesive layer to intertwine with the fiber structure in the substrate layer, further improving the bonding effect between the adhesive and the substrate layer.
[0101] 3. A comparison between Example 6 and Example 2 reveals that the water contact angle and tensile strength of the substrate layer prepared in Example 6 are improved, while abrasion is reduced. This indicates that the prickly ash residue in this application contains a large amount of cellulose and lignin. Adding these to the substrate layer increases the tensile effect between the components, improves the density, strength, and hydrophobicity of the substrate layer. Simultaneously, the lignin in the prickly ash residue, with its network structure, further enhances the strength of the fiber network in the substrate layer, thereby further improving its strength and density. Preparing the prickly ash residue into ultrafine powder mechanically activates it, resulting in a loose crystal structure and uniform strength in the substrate layer. Furthermore, pulverizing the prickly ash residue into ultrafine powder can, to a certain extent, increase the bonding effect between the substrate layer and the adhesive layer, thus imparting excellent strength and bonding strength to the biodegradable tape. In addition, after pulverizing and activating the sorghum residue, active free radicals and plant polysaccharides can be obtained on the surface of the sorghum residue powder, which can further improve the bonding effect between the sorghum residue powder and the substrate layer. At the same time, the plant polysaccharides can improve the adhesion between the substrate layer and the adhesive layer, thereby improving the performance of the tape.
[0102] 4. A comparison between Examples 7-9 and Example 2 reveals that the water contact angle and tensile strength of the substrate layer prepared in Examples 7-9 are improved, while abrasion is reduced. This indicates that, in this application, the use of vermiculite loaded onto straw ultrafine powder or sorghum ultrafine powder firstly enhances the strength of the fiber network in the straw ultrafine powder or sorghum ultrafine powder, further improving the strength and toughness of the substrate layer; secondly, the addition of vermiculite increases the number of abrasion-resistant particles in the substrate layer, improving the abrasion resistance of the tape and extending its service life. Simultaneously, vermiculite possesses excellent frost resistance and heat resistance, effectively improving the frost resistance of the substrate layer and reducing the possibility of tape breakage in winter. Furthermore, the layered structure of vermiculite forms a shielding layer in the substrate layer, further improving the abrasion resistance of the substrate layer and extending the service life of the tape.
[0103] 5. A comparison between Examples 10-11 and Example 6 reveals that the water contact angle and tensile strength of the substrate layer prepared in Examples 10-11 are improved, while abrasion is reduced. This indicates that adding silicone rubber to the substrate layer in this application can effectively improve the low-temperature toughness of the substrate layer, making the tape less prone to breakage or shattering due to low temperatures, thus extending the tape's service life. Grafting epoxy groups onto the silicone rubber and utilizing the reaction between the epoxy groups and polylactic acid end groups effectively improves the compatibility between the silicone rubber and the substrate layer, resulting in uniform toughness and low-temperature resistance in the substrate layer.
[0104] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. An environmentally friendly biodegradable adhesive tape for packaging materials, characterized in that, It includes a substrate layer and an adhesive layer, wherein the substrate layer comprises the following materials in parts by weight: 60-80 parts polylactic acid, 40-50 parts starch, 5-25 parts plasticizer, and 8-10 parts alkyl ketene dimer; The adhesive layer comprises a starch-based biodegradable adhesive.
2. The environmentally friendly biodegradable tape for packaging materials according to claim 1, characterized in that: The substrate layer also includes 5-10 parts by weight of straw ultrafine powder or sorghum ultrafine powder.
3. The environmentally friendly biodegradable tape for packaging materials according to claim 2, characterized in that: The straw ultrafine powder or sorghum ultrafine powder is loaded with vermiculite.
4. The environmentally friendly biodegradable tape for packaging materials according to claim 3, characterized in that: The vermiculite comprises vermiculite sheets modified with hexadecyltrimethylammonium bromide.
5. The environmentally friendly biodegradable tape for packaging materials according to claim 3, characterized in that: The preparation method of vermiculite-loaded ultrafine powder of psyllium includes: placing psyllium ultrafine powder in a phosphoric acid modified solution, stirring and mixing to obtain modified psyllium ultrafine powder; dispersing vermiculite in an ethanol solution to obtain a dispersion; adding modified lignin to the dispersion, stirring and mixing, aging, and spray drying to obtain psyllium ultrafine powder loaded with vermiculite.
6. The environmentally friendly biodegradable tape for packaging materials according to claim 2, characterized in that: The substrate layer also includes 5-10 parts by weight of silicone rubber.
7. The environmentally friendly biodegradable tape for packaging materials according to claim 6, characterized in that: The silicone rubber is epoxy-modified silicone rubber.
8. The environmentally friendly biodegradable tape for packaging materials according to claim 1, characterized in that: The polylactic acid is selected from any one of REVODE 101, REVODE 110 and REVODE 1711B.
9. The environmentally friendly biodegradable tape for packaging materials according to claim 1, characterized in that: The biodegradable adhesive comprises the following materials in parts by weight: 40-50 parts starch, 0.4-0.5 parts nanocellulose, 0.16-0.2 parts ferrous sulfate, 20-30 parts hydrogen peroxide, 4-5 parts sodium hydroxide, 0.05-0.1 parts sodium tetraborate, 0.05-0.1 parts tributyl phosphate, and 1-2 parts borax.
10. A method for preparing an environmentally friendly biodegradable adhesive tape for packaging materials according to any one of claims 1-9, characterized in that, Includes the following steps: S1. Preparation of substrate layer: Mix starch with solvent, gelatinize in water bath, add alkyl ketene dimer, heat and stir, dry, pulverize to obtain modified starch, heat and stir modified starch, plasticizer and polylactic acid, hot press to form film, dry to obtain substrate layer; S2. Tape preparation: A release agent is coated on one side of the substrate layer, and a biodegradable adhesive is coated on the other side of the substrate layer to prepare the tape.