A vehicle-mounted 3A explosion-proof film and its preparation method

By using an AGAR composite layer made of hollow SiO2 nanoparticles and micron-sized SiO2 particles and a micro-dimpled structure, the problem of achieving both nanoscale interference anti-reflection and micron-sized diffuse reflection in automotive explosion-proof films has been solved, thus achieving highly efficient anti-reflection and anti-glare effects.

CN123107560APending Publication Date: 2026-11-17GUANGDONG CONTINENTAL HIGH-TECH MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611478128.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing automotive explosion-proof films cannot simultaneously meet the requirements of nanoscale interference anti-reflection and micron-level diffuse reflection anti-glare in a single film layer system.

Method used

An AGAR composite layer, composed of hollow SiO2 nanoparticles and micron-sized SiO2 particles, combined with a micro-dimpled structure, is formed by UV curing to create an anti-reflective and anti-glare automotive 3A explosion-proof film.

Benefits of technology

It achieves the synergistic effect of nanoscale interference antireflection and micron-level diffuse reflection antiglare in a single film layer system, reducing reflectivity and increasing transmittance, making it suitable for automotive displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application discloses a vehicle-mounted 3A explosion-proof film and its preparation method. The vehicle-mounted 3A explosion-proof film includes an ultra-thin anti-fingerprint layer, an AGAR composite layer, a PET substrate layer, an OCA optical adhesive layer, and a release film layer stacked sequentially. The AGAR composite layer has a micro-pit structure on the side away from the PET substrate layer. The AGAR composite layer is formed by coating with an AGAR coating liquid, which includes a fluorinated acrylate oligomer, hollow SiO2 nanoparticles, micron-sized SiO2 particles, a fluorocarbon surfactant, a photoinitiator, and a solvent. The hollow SiO2 nanoparticles have an average particle size of 50nm~100nm and a shell thickness of 10nm~20nm. The micron-sized SiO2 particles have an average particle size of 1μm~3μm. This achieves both nanoscale interference anti-reflection and micron-level diffuse reflection anti-glare in a single film system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of membrane technology, and in particular to a vehicle-mounted 3A explosion-proof film and its preparation method. Background Technology

[0002] Automotive explosion-proof film is applied to the surface of the glass of a vehicle's display screen to prevent glass shattering and improve display visibility. Currently, to achieve anti-fingerprint, anti-glare, and anti-reflective functions in automotive explosion-proof film, a multi-layer functional film is usually used. For example, an anti-glare layer is set on one side of a PET substrate, an anti-reflective layer is set on the other side, and then an anti-fingerprint layer is coated on the surface of the anti-glare layer.

[0003] However, anti-reflection (AR) requires a nanoscale smooth interface in the film layer to satisfy the λ / 4 interference destructive condition, while anti-glare (AG) requires a micrometer-scale rough structure on the surface to achieve diffuse reflection. The scale requirements for surface morphology differ by 2 to 3 orders of magnitude. In existing technologies, when the AR layer is placed below the AG layer, the micrometer-scale unevenness of the AG layer disrupts the AR interference condition, making it difficult to reduce reflectivity below 1.5%. When the AR layer is placed above the AG layer, it fills in the micro-pits, causing anti-glare failure. Simultaneously, the thickness of traditional anti-fingerprint layers is much greater than the depth of the micro-pits, and filling in the microstructure during coating leads to a loss of anti-glare function. Therefore, existing automotive explosion-proof films cannot simultaneously satisfy nanometer-scale interference anti-reflection and micrometer-scale diffuse reflection anti-glare in a single film layer system. Summary of the Invention

[0004] This application provides a vehicle-mounted 3A explosion-proof film and its preparation method to solve the technical problem that a single film layer system cannot simultaneously satisfy nanoscale interference anti-reflection and micron-level diffuse reflection anti-glare.

[0005] In a first aspect, this application provides a vehicle-mounted 3A explosion-proof film, comprising, sequentially stacked, an ultra-thin anti-fingerprint (AF) layer, an AGAR composite layer, a PET substrate layer, an OCA optical adhesive layer, and a release film layer; the AGAR composite layer has a micro-pit structure on the side away from the PET substrate layer; the AGAR composite layer is formed by coating with an AGAR coating liquid, the AGAR coating liquid comprising the following raw material components in parts by mass: 20 to 50 parts of fluorinated acrylate oligomer; 5 to 20 parts of hollow SiO2 nanoparticles; 3 to 8 parts of micron-sized SiO2 particles; 1 to 3 parts of fluorocarbon surfactant; Photoinitiator 0.5 to 3 parts; Solvent: 30-60 parts; The hollow SiO2 nanoparticles have an average particle size of 50nm~100nm and a shell thickness of 10nm~20nm; the micron-sized SiO2 particles have an average particle size of 1μm~3μm.

[0006] The AGAR composite layer simultaneously achieves anti-glare and anti-reflection functions. Hollow SiO2 nanoparticles have an outer shell and an inner cavity structure; the inner cavity is air (refractive index ≈ 1), and the outer shell is SiO2 (refractive index ≈ 1.46). By adjusting the ratio of shell thickness to particle size, the equivalent refractive index of the hollow SiO2 nanoparticles can be reduced to 1.2~1.3. Uniformly dispersing these hollow SiO2 nanoparticles in a fluorinated acrylate oligomer matrix reduces the overall effective refractive index of the AGAR composite layer, bringing it close to the square root of the substrate's refractive index, thereby reducing Fresnel reflection at the air / AGAR composite layer interface.

[0007] The AGAR composite layer features a micro-dimpled structure on the side away from the PET substrate layer. Incident light undergoes diffuse reflection on the surface of these micro-dimples, avoiding glare caused by specular reflection. Hollow SiO2 nanoparticles and micron-sized SiO2 particles are combined. The hollow SiO2 nanoparticles provide a low refractive index for anti-reflection, while the micron-sized SiO2 particles provide micron-level roughness to help form diffuse reflection centers. Together, they achieve integrated anti-glare and anti-reflection effects. If only hollow SiO2 nanoparticles are used, the coating surface is too smooth, resulting in insufficient anti-glare performance; if only micron-sized SiO2 particles are used, the refractive index cannot be effectively reduced, leading to poor anti-reflection performance.

[0008] In some embodiments, the hollow SiO2 nanoparticles are hollow SiO2 nanoparticles with surfaces modified by silane coupling agents; the micron-sized SiO2 particles are solid SiO2 particles.

[0009] Silane coupling agent modification can improve the interfacial bonding force between hollow SiO2 nanoparticles and the fluorinated acrylate oligomer matrix, prevent the agglomeration of hollow SiO2 nanoparticles in the coating solution, and ensure uniform dispersion. Optionally, the silane coupling agent is γ-methacryloyloxypropyltrimethoxysilane (KH570). The modification method is as follows: hollow SiO2 nanoparticles are dispersed in ethanol, KH570 is added, and the mixture is stirred at 60℃ for 2 hours. After filtration and drying, modified hollow SiO2 nanoparticles are obtained. Solid SiO2 particles have higher mechanical strength than hollow particles and are less prone to breakage during the imprinting process, ensuring the integrity of the micro-pit structure.

[0010] In some embodiments, the mass ratio of the hollow SiO2 nanoparticles to the micron-sized SiO2 particles is (1~5):1, ensuring that the anti-reflection and anti-glare effects are optimally balanced.

[0011] In some embodiments, the diameter of the micro-pit structure is 5μm to 15μm to ensure a moderate scattering angle for visible light, guaranteeing high light transmittance and optimal anti-glare effect; the depth is 0.5μm to 1.5μm to ensure that the micro-pits are of moderate size, thereby achieving optimal diffuse reflection effect and reducing dust accumulation; the spacing is 10μm to 50μm to ensure that the spacing between the micro-pits is moderate, avoiding both increased haze and uneven anti-glare.

[0012] In some embodiments, the fluorinated acrylate oligomer is a fluorinated polyurethane acrylate oligomer and / or a fluorinated epoxy acrylate oligomer; The fluorocarbon surfactant is a nonionic fluorocarbon surfactant; The photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide; The solvent is propylene glycol methyl ether acetate.

[0013] Among them, fluorinated polyurethane acrylate oligomers combine the flexibility of polyurethane with the low surface energy of fluorinated segments, resulting in coatings with good flexibility, hydrophobicity, and oleophobicity after curing; fluorinated epoxy acrylate oligomers exhibit high hardness and good chemical resistance after curing. Nonionic fluorocarbon surfactants can reduce the surface tension of the coating solution and improve coating leveling; Capstone FS-30 from Chemours is a suitable option. The photoinitiator 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) has high absorption efficiency in the UV-A region and is suitable for thick film curing. The solvent propylene glycol methyl ether acetate (PGMEA) has good dispersibility for both fluorinated acrylate oligomers and hollow SiO2 nanoparticles, and has a moderate boiling point (146℃) and a suitable evaporation rate.

[0014] In some embodiments, the thickness of the ultra-thin anti-fingerprint layer is 0.05μm to 0.15μm; when the thickness of the ultra-thin anti-fingerprint layer is less than 0.05μm, the wear resistance is insufficient, and the hydrophobicity decreases after 500 Taber rubs; when the thickness is greater than 0.15μm, it may partially fill the micro-pits, and the anti-glare effect decreases.

[0015] The thickness of the AGAR composite layer is 3μm~8μm; when the thickness of the AGAR composite layer is less than 3μm, the depth of the micro-pits is difficult to reach more than 0.5μm, and the anti-glare effect is insufficient; when the thickness is greater than 8μm, the internal scattering of the coating increases and the light transmittance decreases.

[0016] The thickness of the PET substrate layer is 75μm~100μm; when the thickness of the PET substrate layer is less than 75μm, the explosion-proof performance is insufficient; when the thickness is greater than 100μm, the flexibility decreases and the edges are prone to lifting when bonding to curved screens.

[0017] The thickness of the OCA optical adhesive layer is 25μm~35μm; the thickness of the release film layer is 50μm~75μm. When the thickness of the OCA optical adhesive layer is less than 25μm, the adhesion is insufficient; when the thickness is greater than 35μm, the light transmittance decreases. When the thickness of the release film layer is less than 50μm, the protective performance is insufficient; when the thickness is greater than 75μm, the cost increases and the operation is inconvenient during bonding.

[0018] In some embodiments, the ultrathin anti-fingerprint layer is formed by crosslinking perfluoropolyether silane; the PET substrate layer is an optical grade PET substrate layer; and the OCA optical adhesive layer includes acrylate pressure-sensitive adhesive, hydroxyphenyl triazine UV absorber, and silane coupling agent.

[0019] The perfluoropolyether silane molecular chain ends contain hydrolyzable silane groups, which can condense with the silanol groups on the surface of the AGAR composite layer to form chemical bonds. Simultaneously, the perfluoropolyether segments accumulate on the surface, imparting hydrophobic and oleophobic properties. Optionally, the perfluoropolyether silane can be selected from Daikin Industries, Ltd.'s OPTOOL DSX or Shin-Etsu Chemical Co., Ltd.'s KY series; the optical-grade PET substrate layer can be selected from SKC's SH81 or Toray Industries, Ltd.'s Lumirror series; the hydroxyphenyl triazine UV absorber can be selected from BASF's Tinuvin 479, which has good compatibility with acrylate pressure-sensitive adhesives, no photocatalytic activity, and can effectively absorb ultraviolet rays from 280nm to 380nm without accelerating the aging of the adhesive layer; the silane coupling agent can be selected from KH570, used to improve the adhesion between the OCA adhesive layer and the PET substrate layer and the glass surface.

[0020] Secondly, this application also provides a method for preparing the vehicle-mounted 3A explosion-proof film as described in the first aspect, comprising the following steps: S1. Fluorinated acrylate oligomer, hollow SiO2 nanoparticles, micron-sized SiO2 particles, fluorocarbon surfactant, photoinitiator and solvent are mixed evenly under light-protected conditions to obtain AGAR coating liquid. S2, the AGAR coating liquid is applied to one side of the plasma-treated PET substrate layer to form a wet film with a thickness of 5μm~10μm; S3, The wet film is pressed using a mold with a surface treated for demolding, so as to form a micro-pit structure on the surface of the wet film; S4, under nitrogen protection, at 600 mJ / cm 2 ~800 mJ / cm 2 The embossed wet film is then UV cured to form an AGAR composite layer. S5, the surface of the AGAR composite layer is activated by oxygen plasma; S6. Perfluoropolyether silane is vapor-deposited on the surface of the activated AGAR composite layer and cured at 80℃±5℃ for 25min~35min to form an ultra-thin anti-fingerprint layer. S7. An OCA optical adhesive layer is coated on the other side of the PET substrate layer, and a release film layer is bonded to the surface of the OCA optical adhesive layer to obtain a vehicle-mounted 3A explosion-proof film.

[0021] In S1, the light-shielding condition prevents the photoinitiator from prematurely initiating polymerization. Mixing can be done using a high-speed disperser at a speed of 2000-3000 r / min for 30-60 min. In S2, plasma treatment generates hydroxyl and carboxyl groups on the surface of the PET substrate layer, improving the wettability and adhesion of the AGAR coating solution. Coating can be done using microgravure roller coating with a wet film thickness of 5μm-10μm. If the wet film is too thin, the depth of the micro-indentations after imprinting will be insufficient; if the wet film is too thick, the shrinkage stress during UV curing will be large, easily leading to micro-indentations. The process involves several steps: S3 involves embossing to create micro-pits on the wet film surface, followed by mold release treatment to prevent resin adhesion; S4 involves nitrogen protection to eliminate oxygen and prevent incomplete curing due to oxygen inhibition; S5 involves oxygen plasma activation to generate silanol groups on the AGAR composite layer surface, providing bonding sites for perfluoropolyether silane; S6 involves vapor deposition to uniformly deposit perfluoropolyether silane on the micro-pit surface, with the curing temperature ensuring full condensation of the silane with the surface hydroxyl groups; and S7 involves OCA adhesive coating and release film lamination in a cleanroom to avoid dust contamination.

[0022] In some embodiments, in step S3, the mold is a nickel mold coated with diamond-like carbon (DLC), and the surface of the mold is treated with fluorosilane for mold release; the imprinting pressure is 0.2 MPa to 0.5 MPa; the diamond-like carbon (DLC) coating has high hardness and low coefficient of friction, which can extend the service life of the nickel mold; the fluorosilane mold release treatment reduces the surface energy of the mold and prevents the UV-cured resin from sticking to the mold.

[0023] In some embodiments, in step S5, the oxygen plasma activation power is 100W~300W and the processing time is 30s~120s to ensure that the surface hydroxyl density and perfluoropolyether silane bonding amount are sufficient, thereby improving the hydrophobic effect without damaging the micro-pit structure.

[0024] Compared with the prior art, this application has the following beneficial effects: This invention combines hollow SiO2 nanoparticles and micron-sized SiO2 particles in a UV-curable hybrid resin, along with a specific micro-pit structure formed by microimprinting. The hollow SiO2 nanoparticles' internal cavity structure reduces their equivalent refractive index to 1.20-1.30, thus reducing Fresnel reflection at the air / AGAR composite layer interface. The micron-sized SiO2 particles and the micro-pit structure cause diffuse reflection of incident light, eliminating glare. This allows a single film system to simultaneously satisfy nanoscale interference anti-reflection and micron-level diffuse reflection anti-glare.

[0025] Meanwhile, this invention employs a full coating, micro-imprinting, and UV curing process, eliminating the need for magnetron sputtering and high-temperature calcination. It is compatible with PET substrates, with a process temperature not exceeding 80°C, thus avoiding thermal deformation of the PET substrate. It is also compatible with roll-to-roll production, resulting in low cost and high yield. Detailed Implementation

[0026] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention are described in detail below. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0027] As used herein, the terms “prepared from” and “comprising” are synonymous. The terms “comprising,” “including,” “having,” “containing,” or any other variations thereof, as used herein, are intended to cover non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such composition, step, method, article, or apparatus.

[0028] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including the ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range.

[0029] Furthermore, the indefinite articles “a” and “an” preceding the elements or components of this invention do not impose any limitation on the quantity requirement (i.e., the number of times) of the elements or components. Therefore, “an” or “a” should be interpreted as including one or at least one, and the singular form of an element or component also includes the plural form, unless the quantity clearly refers to the singular form.

[0030] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Example 1

[0031] AGAR coating solution comprises the following raw materials in parts by weight: 35 parts of fluorinated polyurethane acrylate oligomer (fluorine content 12 wt%, functionality 3, viscosity 8000 mPa·s / 25℃, number average molecular weight 3000); 10 parts of silane-modified hollow SiO2 nanoparticles (average particle size 82nm, shell thickness 15nm, surface silane grafting rate 3.5wt%). Five portions of micron-sized solid SiO2 particles (average particle size 2 μm, purity ≥99.5%, sphericity ≥0.9); Two parts of nonionic fluorocarbon surfactant (surface tension ≤20 mN / m, HLB value 8~10); 1.5 parts of photoinitiator TPO (purity ≥99%); Solvent: 46.5 parts of propylene glycol methyl ether acetate (purity ≥99.5%, boiling point 146℃).

[0032] The preparation method of vehicle-mounted 3A explosion-proof film includes the following steps: S1. Stir the above AGAR coating liquid raw materials at 2000 rpm for 45 minutes under light-protected conditions until they are evenly mixed to obtain the AGAR coating liquid. S2, oxygen plasma treatment (power 200 W, time 60 s) is performed on one side of an optical grade PET substrate layer with a thickness of 100 μm (transmittance ≥95%, haze ≤0.8%, tensile strength ≥150MPa, elongation at break ≥180%), and then AGAR coating liquid is applied by micro-gravure roller coating to form a wet film with a thickness of 8 μm. S3 uses a nickel mold plated with diamond-like carbon (the surface is treated with fluorosilane for demolding, and the surface energy of the mold is ≤15 mN / m) to imprint the wet film. The imprinting pressure is 0.3 MPa, forming a micro-pit structure with a diameter of 8 μm, a depth of 1.0 μm, and a spacing of 25 μm on the surface of the wet film. S4, under nitrogen protection, UV curing is performed on the imprinted wet film with an energy of 700 mJ / cm² to form an AGAR composite layer with a thickness of 5μm. S5, oxygen plasma activation of the AGAR composite layer surface (power 200 W, time 60 s). S6. A perfluoropolyether silane (fluorine content ≥50 wt%, number average molecular weight 2000~4000, terminal trimethoxysilane group) was vapor-deposited on the surface of the activated AGAR composite layer and cured at 80℃ for 30 min to form an ultrathin anti-fingerprint layer with a thickness of 0.08 μm. S7. On the other side of the PET substrate layer, apply OCA optical adhesive (100 parts of acrylate pressure-sensitive adhesive, 0.8 parts of hydroxyphenyl triazine UV absorber and 0.8 parts of KH570) with a thickness of 30 μm. Then, apply a 50 μm thick PET release film (release force 0.1~0.3 N / 25mm) to the surface of the OCA optical adhesive layer with a pressure of 0.4 MPa to obtain the vehicle 3A explosion-proof film. Example 2

[0033] The difference from Example 1 is that the following components are used: 20 parts of fluorinated polyurethane acrylate oligomer; 5 parts of modified hollow SiO2 nanoparticles (average particle size 51 nm, shell thickness 10 nm); 3 parts of micron-sized solid SiO2 particles; 1 part of fluorocarbon surfactant; 0.5 parts of photoinitiator; and 30 parts of solvent. The micro-pits have a diameter of 5 μm, a depth of 0.5 μm, and a spacing of 10 μm. The ultrathin anti-fingerprint layer has a thickness of 0.05 μm; the AGAR composite layer has a thickness of 3 μm; the PET substrate layer has a thickness of 75 μm; the OCA optical adhesive layer has a thickness of 25 μm; and the release film layer has a thickness of 50 μm. Example 3

[0034] The difference from Example 1 is that it contains 50 parts of fluorinated polyurethane acrylate oligomer; 20 parts of modified hollow SiO2 nanoparticles (average particle size 98 nm, shell thickness 19 nm); 8 parts of micron-sized solid SiO2 particles; 3 parts of fluorocarbon surfactant; 3 parts of photoinitiator; and 60 parts of solvent. The micro-pits have a diameter of 15 μm, a depth of 1.5 μm, and a spacing of 50 μm. The ultrathin anti-fingerprint layer has a thickness of 0.15 μm; the AGAR composite layer has a thickness of 8 μm; the PET substrate layer has a thickness of 100 μm; the OCA optical adhesive layer has a thickness of 35 μm; and the release film layer has a thickness of 75 μm. Example 4

[0035] The difference from Example 1 is that it contains 35 parts of fluorinated polyurethane acrylate oligomer; 12 parts of modified hollow SiO2 nanoparticles; 5 parts of micron-sized solid SiO2 particles; 2 parts of fluorocarbon surfactant; 1.5 parts of photoinitiator; and 45 parts of solvent. The micro-pits have a diameter of 10 μm, a depth of 1 μm, and a spacing of 30 μm. The ultrathin anti-fingerprint layer has a thickness of 0.1 μm; the AGAR composite layer has a thickness of 5 μm; the PET substrate layer has a thickness of 85 μm; the OCA optical adhesive layer has a thickness of 30 μm; and the release film layer has a thickness of 60 μm. Example 5

[0036] The difference from Example 1 is that the fluorinated acrylate oligomer is a fluorinated epoxy acrylate oligomer (fluorine content 10 wt%, functionality 2, viscosity 5000 mPa·s / 25℃, number average molecular weight 2500) 35 parts; the fluorocarbon surfactant is perfluorooctyl sulfonic acid quaternary ammonium salt (surface tension ≤18 mN / m, ionic); the photoinitiator is 1.5 parts of 1-hydroxycyclohexylphenyl ketone (purity ≥99%); and the solvent is ethyl acetate (purity ≥99.5%, boiling point 77℃) 46.5 parts. The hollow SiO2 uses unmodified hollow SiO2 nanoparticles (average particle size 80 nm, shell thickness 15 nm, specific surface area 180 m² / g). Example 6

[0037] The difference from Example 1 is that 20 parts of modified hollow SiO2 nanoparticles and 4 parts of micron-sized solid SiO2 particles were used.

[0038] Comparative Example 1 The difference from Example 1 is that the modified hollow SiO2 nanoparticles in Comparative Example 1 were replaced with an equal amount of solid SiO2 nanoparticles (average particle size 80 nm).

[0039] Comparative Example 2 The difference from Example 1 is that Comparative Example 2 removes the micron-sized solid SiO2 particles and replaces them with an equal amount of modified hollow SiO2 nanoparticles.

[0040] Comparative Example 3 The difference from Example 1 is that step S3 of Comparative Example 3 does not involve embossing, and the surface of the AGAR composite layer is a flat surface without micro-pit structures.

[0041] Comparative Example 4 The difference from Example 1 is that Comparative Example 4 contains 20 parts of modified hollow SiO2 nanoparticles and 2 parts of micron-sized solid SiO2 particles.

[0042] Comparative Example 5 The difference from Example 1 is that the hollow SiO2 nanoparticles in Comparative Example 5 have an average particle size of 200 nm, a shell thickness of 30 nm, and a specific surface area of ​​80 m². 2 / g Comparative Example 6 The difference from Example 1 is that the micro-pits in Comparative Example 6 have a diameter of 20 μm and a depth of 2.0 μm.

[0043] Comparative Example 7 The difference from Example 1 is that the micro-pits in Comparative Example 7 have a diameter of 3 μm and a depth of 0.3 μm.

[0044] Comparative Example 8 The difference from Example 1 is that the ultrathin anti-fingerprint layer of Comparative Example 8 was formed by coating method, with a thickness of 1 μm, and the coating liquid was an ethyl acetate solution of perfluoropolyether silane (solid content 5%).

[0045] Performance testing Reflectance: The reflectance at 550 nm was measured using a UV-Vis-NIR spectrophotometer, in accordance with GB / T 2680-2021.

[0046] Haze and transmittance: According to ASTM D1003, haze was tested using a haze meter and transmittance was tested using a spectrophotometer.

[0047] Gloss: Gloss at 60° was tested using a gloss meter in accordance with GB / T 9754-2025.

[0048] Table 1 Performance test results of the examples and comparative examples

[0049] As shown in Table 1, Examples 1 to 6 all achieved a synergistic effect of low reflectivity (≤2.0%), low gloss (75~88), and moderate haze (2.0%~2.9%). This indicates that the hollow SiO2 nanoparticles provide a low refractive index to achieve anti-reflection, while the micron-sized SiO2 particles and micro-pit structure provide diffuse reflection to achieve anti-glare. An effective synergy is formed in a single AGAR composite layer, successfully solving the technical problem that a single film system cannot simultaneously satisfy nano-level interference anti-reflection and micron-level diffuse reflection anti-glare.

[0050] Compared to Example 1, the reflectivity of Comparative Example 1 increased from 1.8% to 3.2%, indicating that replacing hollow SiO2 with solid SiO2 did not effectively reduce the refractive index of the coating; the hollow structure is what achieves low reflectivity. The reflectivity of Comparative Example 2 increased from 1.8% to 2.5%, and the gloss increased from 85 to 120, indicating that removing micron-sized SiO2 resulted in a lack of micron-sized diffuse reflection centers, essentially eliminating the anti-glare function. The reflectivity of Comparative Example 3 increased from 1.8% to 2.8%, and the gloss increased from 85 to 130, indicating that without embossing and a micro-dimple structure, diffuse reflection could not be formed on the surface, rendering the anti-glare function ineffective. The reflectivity of Comparative Example 4 increased from 1.8% to 2.9%, and the gloss increased from 85 to 110, indicating that when the mass ratio of hollow SiO2 to micron-sized SiO2 exceeded the range of (1~5):1 (10:1), both anti-reflection and anti-glare performance deteriorated simultaneously. The reflectivity of Comparative Example 5 increased from 1.8% to 2.9%, and the gloss increased from 85 to 110. The reflectance of Comparative Example 6 increased from 1.8% to 2.2%, haze increased from 2.2% to 5.5%, and transmittance decreased from 93% to 88%, indicating that excessively large hollow SiO2 particle size led to Mie scattering, which not only worsened the anti-reflection effect but also severely reduced transmittance. The reflectance of Comparative Example 6 increased from 1.8% to 2.0%, haze increased from 2.2% to 4.2%, and transmittance decreased from 93% to 91%, indicating that excessively large micro-dimple size led to excessive scattering, a sharp increase in haze, and impaired display clarity. Clarity; Comparative Example 7 showed an increase in reflectivity from 1.8% to 2.4% and gloss from 85 to 125, indicating that when the micro-dimple size is too small, diffuse reflection is insufficient and the anti-glare function is inadequate; Comparative Example 8 showed an increase in reflectivity from 1.8% to 2.6% and gloss from 85 to 135, while haze decreased from 2.2% to 0.5%, and scratches appeared after 500 abrasion cycles, indicating that the excessively thick anti-fingerprint layer filled the micro-dimple structure, causing the anti-glare function to fail, and at the same time, the abrasion resistance decreased.

[0051] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0052] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of this application. It should be understood that the above descriptions are merely specific embodiments of this application and are not intended to limit the scope of protection of this application. In particular, it should be noted that any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the scope of protection of this application for those skilled in the art.

Claims

1. A vehicle-mounted 3A explosion-proof film, characterized in that, The material comprises, in sequence, an ultra-thin anti-fingerprint layer, an AGAR composite layer, a PET substrate layer, an OCA optical adhesive layer, and a release film layer; the AGAR composite layer has a micro-pit structure on the side away from the PET substrate layer; the AGAR composite layer is formed by coating with an AGAR coating liquid, which comprises the following raw material components in parts by mass: 20 to 50 parts of fluorinated acrylate oligomer; 5 to 20 parts of hollow SiO2 nanoparticles; 3 to 8 parts of micron-sized SiO2 particles; 1 to 3 parts of fluorocarbon surfactant; Photoinitiator 0.5 to 3 parts; Solvent: 30-60 parts; The hollow SiO2 nanoparticles have an average particle size of 50nm~100nm and a shell thickness of 10nm~20nm; the micron-sized SiO2 particles have an average particle size of 1μm~3μm.

2. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The hollow SiO2 nanoparticles are hollow SiO2 nanoparticles with surfaces modified by silane coupling agents; the micron-sized SiO2 particles are solid SiO2 particles.

3. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The mass ratio of the hollow SiO2 nanoparticles to the micron-sized SiO2 particles is (1~5):

1.

4. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The diameter of the micro-pit structure is 5μm~15μm, the depth is 0.5μm~1.5μm, and the spacing is 10μm~50μm.

5. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The fluorinated acrylate oligomer is a fluorinated polyurethane acrylate oligomer and / or a fluorinated epoxy acrylate oligomer. The fluorocarbon surfactant is a nonionic fluorocarbon surfactant; The photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide; The solvent is propylene glycol methyl ether acetate.

6. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The thickness of the ultra-thin anti-fingerprint layer is 0.05μm~0.15μm; the thickness of the AGAR composite layer is 3μm~8μm; the thickness of the PET substrate layer is 75μm~100μm; the thickness of the OCA optical adhesive layer is 25μm~35μm; and the thickness of the release film layer is 50μm~75μm.

7. The vehicle-mounted 3A explosion-proof film as described in claim 1, characterized in that, The ultra-thin anti-fingerprint layer is formed by crosslinking perfluoropolyether silane; the PET substrate layer is an optical grade PET substrate layer; the OCA optical adhesive layer includes acrylate pressure-sensitive adhesive, hydroxyphenyl triazine UV absorber and silane coupling agent.

8. A method for preparing a vehicle-mounted 3A explosion-proof film as described in any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Fluorinated acrylate oligomer, hollow SiO2 nanoparticles, micron-sized SiO2 particles, fluorocarbon surfactant, photoinitiator and solvent are mixed evenly under light-protected conditions to obtain AGAR coating liquid. S2, the AGAR coating liquid is applied to one side of the plasma-treated PET substrate layer to form a wet film with a thickness of 5μm~10μm; S3, The wet film is pressed using a mold with a surface treated for demolding, so as to form a micro-pit structure on the surface of the wet film; S4, under nitrogen protection, at 600 mJ / cm 2 ~800 mJ / cm 2 The embossed wet film is then UV cured to form an AGAR composite layer. S5, the surface of the AGAR composite layer is activated by oxygen plasma; S6. Perfluoropolyether silane is vapor-deposited on the surface of the activated AGAR composite layer and cured at 80℃±5℃ for 25min~35min to form an ultra-thin anti-fingerprint layer. S7. An OCA optical adhesive layer is coated on the other side of the PET substrate layer, and a release film layer is bonded to the surface of the OCA optical adhesive layer to obtain a vehicle-mounted 3A explosion-proof film.

9. The method for preparing the vehicle-mounted 3A explosion-proof film as described in claim 7, characterized in that, In step S3, the mold is a nickel mold plated with diamond-like carbon, and the surface of the mold is treated with fluorosilane for demolding; the imprinting pressure is 0.2MPa~0.5MPa.

10. The method for preparing the vehicle-mounted 3A explosion-proof film as described in claim 7, characterized in that, In step S5, the power of the oxygen plasma activation is 100W~300W, and the processing time is 30s~120s.