UV-absorbing thermally de-adhesive functional film with interfacial transition structure, its preparation method and application
By constructing a continuous interpenetrating transition interface of a UV-absorbing thermally de-adhesive functional film on the back of a transparent substrate, the problem of bonding stability between the light-absorbing functional layer and the adhesive layer is solved, enabling the suppression of back reflection during UV exposure and controllable peeling after heat treatment, thus improving process compatibility.
Patent Information
- Application Number
- CN202611456607.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-18
- Publication Date
- 2026-11-17
AI Technical Summary
In existing transparent substrate back-side reflection suppression films, the interface bonding stability between the light-absorbing functional layer and the adhesive layer is insufficient, the thermal de-adhesion performance is difficult to control, and the optical performance and peelability are difficult to balance.
A continuous interpenetrating transition interface is constructed between the ultraviolet light-absorbing carrier layer and the transparent heat-reducing pressure-sensitive adhesive layer. Combined with the UV-curable acrylic resin matrix and benzotriazole ultraviolet absorber, the thermally expanding microspheres are distributed in a gradient along the thickness direction of the adhesive layer to form an interpenetrating transition structure.
It improves the interfacial bonding stability of functional films, realizes the suppression of back reflection during UV exposure and controllable peeling after heat treatment, reduces the risk of interfacial failure in traditional heat-release films, and improves process compatibility.
Smart Images

Figure CN123107567A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of functional film materials and optical auxiliary materials, specifically to a UV-absorbing thermally de-adhesive functional film with an interface transition structure, its preparation method, and its application. Background Technology
[0002] In semiconductor manufacturing, micro / nano fabrication, and optical component processing, transparent substrates (such as quartz glass and optical glass) are often used as carrier materials in the exposure process due to their high light transmittance. However, during ultraviolet exposure, incident light may be transmitted and reflected after passing through the transparent substrate, forming back-reflected light. This affects the light field distribution within the exposure area, leading to problems such as standing wave effects within the photoresist, exposure size deviations, and a decrease in pattern quality.
[0003] To reduce back-side reflection of transparent substrates, the common practice is to place a light-absorbing layer or attach a black light-shielding film on the back of the substrate to reduce the reflection of exposed light inside the substrate. Traditional black polymer films (such as black PET films) are typically bonded to the transparent substrate using pressure-sensitive adhesive, utilizing the black film layer to absorb ultraviolet light.
[0004] However, existing light-absorbing film structures still have certain shortcomings: (1) Insufficient stability of the interface bonding between the light-absorbing functional layer and the adhesive layer.
[0005] Traditional black PET film and pressure-sensitive adhesive are usually different material systems, and they are mainly bonded by physical adhesion, with obvious material abrupt changes at the interface. During exposure, heating, and subsequent processing, the differences in thermal expansion coefficients, elastic moduli, and interfacial interactions between the different materials can easily lead to interfacial failure between the film layers, affecting the overall stability of the functional film.
[0006] (2) It is difficult to balance light absorption and peelability.
[0007] Existing heat-resistant adhesives typically reduce adhesion after heating by incorporating thermally responsive materials such as thermally expandable microspheres. However, thermally expandable microspheres are usually uniformly dispersed within the adhesive layer, and their thermally responsive areas lack spatial control, which may lead to problems such as surface unevenness, optical effects, or uncontrollable heat release locations during the bonding stage.
[0008] (3) The failure location after heat treatment is difficult to control.
[0009] In the processing of transparent substrates, it is desirable for the functional film to have sufficient adhesion stability during the exposure stage and to achieve rapid, low-residue peeling during the heat treatment stage. However, in existing thermal de-adhesion structures, failure modes such as internal adhesive layer damage, interlayer separation of adhesive films, and substrate interface detachment are difficult to control, which may lead to residual adhesive contamination or functional film residue.
[0010] Therefore, it is necessary to develop a new composite functional film structure that enables good bonding stability between the light-absorbing functional layer and the thermal de-adhesion functional layer, while allowing for controllable release under heat treatment conditions, thereby meeting the requirements for optical control and reliable peeling during the front exposure process of transparent substrates. Summary of the Invention
[0011] In view of this, the main objective of this invention is to provide a UV-absorbing thermally de-adhesive functional film with an interface transition structure, its preparation method, and its application. The technical problem to be solved is to construct a continuous interpenetrating transition interface between the UV-absorbing carrier layer and the transparent thermally de-adhesive pressure-sensitive adhesive layer by using a process of pre-curing, limited solvent swelling, and low-temperature thermal curing. This eliminates the abrupt interface structure of traditional film layers, eliminates the need for an additional third transition material, significantly improves the interfacial bonding strength between the two functional layers, and avoids the risk of interlayer separation failure during heat treatment. At the same time, the thermally expandable microspheres are set in a gradient distribution pattern with low pressure on both sides and high pressure in the middle along the thickness direction of the adhesive layer, so as to achieve precise control of thermal expansion stress and take into account both the bonding stability of the functional film at room temperature and the peeling performance after heat treatment. The resulting functional film can effectively suppress UV back reflection in the 365nm band and can directly reuse the inherent heat from the post-exposure baking to trigger thermal de-adhesion, eliminating the need for a separate additional heating process. No obvious adhesive residue was observed on the substrate after peeling, achieving complete overall peeling of the functional film.
[0012] The objective of this invention and the technical problem it solves are achieved by the following technical solution. This invention proposes a UV-absorbing thermally de-adhesive functional film with an interface transition structure, comprising a UV-absorbing carrier layer and a transparent thermally de-adhesive pressure-sensitive adhesive layer disposed on one side of the UV-absorbing carrier layer; The ultraviolet light-absorbing support layer comprises a UV-curable acrylic resin matrix, a benzotriazole ultraviolet absorber, and a black light-absorbing material; The transparent heat-resistant pressure-sensitive adhesive layer comprises an acrylic copolymer, poly(docosahexamethicone) and thermally expandable microspheres. A continuous interfacial interpenetration transition region is provided between the ultraviolet light-absorbing carrier layer and the transparent heat-resistant pressure-sensitive adhesive layer. The continuous interfacial interpenetration transition region is formed by the mutual penetration of the UV-cured acrylic resin matrix and the acrylic copolymer at the interface. Along the thickness direction of the transparent heat-resistant pressure-sensitive adhesive layer, the concentration of the thermally expanded microspheres in the middle region is higher than that in the region near the ultraviolet light-absorbing carrier layer and the region near the substrate bonding side, exhibiting a non-uniform distribution with low concentrations on both sides and high concentrations in the middle.
[0013] The objectives of this invention and the technical problems solved can be further achieved by the following technical measures.
[0014] Preferably, in the aforementioned ultraviolet light-absorbing thermal de-adhesion functional film, the thickness of the ultraviolet light-absorbing carrier layer is 3 to 15 μm; Based on a total solid component mass of 100 parts by mass of the ultraviolet light-absorbing support layer, the ultraviolet light-absorbing support layer comprises: 70-82 parts by weight of UV-curable acrylic resin; 10-18 parts by weight of reactive diluent; 2-5 parts by weight of benzotriazole UV absorber; 2-5 parts by weight of black light-absorbing material; Photoinitiator 1.5–3 parts by weight; Dispersant 0.5 to 1.5 parts by weight.
[0015] Preferably, in the aforementioned ultraviolet light-absorbing heat-reducing functional film, the black light-absorbing material is carbon black.
[0016] Preferably, in the aforementioned ultraviolet light-absorbing heat-reducing functional film, the acrylic copolymer is obtained by polymerization of a monomer composition comprising isooctyl acrylate, lauryl acrylate, methyl methacrylate and acrylamide; Based on a total mass of 100 parts by mass of monomer composition, isooctyl acrylate comprises 40-70 parts by mass, lauryl acrylate comprises 5-25 parts by mass, methyl methacrylate comprises 10-35 parts by mass, and acrylamide comprises 0.5-10 parts by mass. Based on 100 parts by weight of the solids of the acrylic copolymer, the amount of poly(2-diethyl acrylate) added is 3 to 15 parts by weight, and it is dispersed in the transparent heat-resistant pressure-sensitive adhesive layer by physical blending.
[0017] Preferably, the aforementioned ultraviolet light-absorbing heat-reducing adhesive functional film is divided into a first low-concentration region, an intermediate high-concentration region, and a second low-concentration region along the thickness direction of the transparent heat-reducing adhesive layer. The thermal expansion microsphere content in the first low concentration region and the second low concentration region is based on the total solid mass of acrylic copolymers and poly(2-diethyl acrylate) in the corresponding region, and is 0.5 to 2 wt% respectively. The thermal expansion microsphere content in the intermediate high concentration region is 4 to 8 wt%.
[0018] Preferably, in the aforementioned ultraviolet light-absorbing thermal de-adhesion functional film, the thermal expansion microsphere content of the first low-concentration region, the intermediate high-concentration region, and the second low-concentration region is based on the total solid mass of acrylic copolymer and poly(dodecyl acrylate) in the corresponding regions, and is 1 wt%, 6 wt%, and 1 wt%, respectively, and the thickness of the corresponding regions is 15 μm, 20 μm, and 15 μm, respectively.
[0019] Preferably, the aforementioned UV-absorbing heat-resistant adhesive functional film further includes a first release protective layer and a second release protective layer; the first release protective layer is disposed on the side of the UV-absorbing carrier layer away from the transparent heat-resistant adhesive layer, and the second release protective layer is disposed on the side of the transparent heat-resistant adhesive layer away from the UV-absorbing carrier layer; both the first and second release protective layers are removable protective layers.
[0020] The objective of this invention and the technical problem it solves are achieved through the following technical solution. This invention proposes a method for preparing the aforementioned ultraviolet light-absorbing thermally de-adhesive functional film, comprising the following steps: (1) Provide a first release protective substrate; (2) A UV-curable acrylic resin, a benzotriazole UV absorber, a black light-absorbing material and a photoinitiator are mixed to obtain a UV-absorbing coating composition; (3) The ultraviolet light-absorbing coating composition is coated on the surface of the first release protective substrate and UV curing is performed in the first stage to obtain a pre-cured ultraviolet light-absorbing carrier layer that maintains the complete film shape and has the ability to be swollen by organic solvents. (4) The acrylic copolymer was physically blended with poly(2-diethyl acrylate), and organic solvent and thermally expandable microspheres with different contents were added to prepare multiple transparent heat-reducing pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres. (5) Transparent thermally resistant pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres are sequentially coated onto the surface of the pre-cured ultraviolet light-absorbing carrier layer. During the coating process, the organic solvent causes limited swelling on the surface of the pre-cured ultraviolet light-absorbing carrier layer. By sequentially coating compositions with different contents of microspheres, the thermally expandable microspheres are distributed in a non-uniform manner along the thickness direction of the formed transparent thermally resistant pressure-sensitive adhesive layer, with low concentration on both sides and high concentration in the middle. (6) Thermal curing is carried out under conditions lower than the initial expansion temperature of the thermal expansion microspheres to evaporate the organic solvent and form a continuous interfacial interpenetration transition region at the interface between the ultraviolet light-absorbing carrier layer and the transparent thermally reducing pressure-sensitive adhesive layer, while stabilizing the spatial distribution of the thermal expansion microspheres along the thickness direction of the transparent thermally reducing pressure-sensitive adhesive layer. (7) A second release protective layer is laminated on the side of the transparent heat-resistant pressure-sensitive adhesive layer away from the ultraviolet light-absorbing carrier layer; (8) Roll up and cut to obtain the ultraviolet light-absorbing heat-reducing functional film.
[0021] The objectives of this invention and the technical problems solved can be further achieved by the following technical measures.
[0022] Preferably, in the aforementioned method for preparing the ultraviolet light-absorbing heat-reducing adhesive functional film, in step (5), transparent heat-reducing adhesive pressure-sensitive adhesive compositions with low thermal expansion microsphere content, high thermal expansion microsphere content, and low thermal expansion microsphere content are sequentially coated, with the thermal expansion microsphere content in the corresponding regions being 0.5-2 wt%, 4-8 wt%, and 0.5-2 wt%, respectively.
[0023] Preferably, in the aforementioned method for preparing the UV-absorbing thermally de-adhesive functional film, the organic solvent comprises ethyl acetate; the thermal curing temperature is 50–80°C, the thermal curing time is 10–60 min, and the thermal curing temperature is lower than the initial expansion temperature of the thermally expanding microspheres used.
[0024] The objective of this invention and the technical problem it solves can also be achieved by the following technical measures. This invention proposes a method for suppressing back reflection during ultraviolet exposure of the front side of a transparent substrate, using the aforementioned ultraviolet-absorbing thermally de-adhesive functional film, comprising the following steps: S1. The second release protective layer for peeling off the functional film is used to attach a transparent heat-resistant pressure-sensitive adhesive layer to the back of a transparent substrate with photoresist on the front side. S2. Peel off the first release protective layer. The ultraviolet light-absorbing carrier layer is on the outside. Ultraviolet exposure is performed from the front of the transparent substrate. The ultraviolet light-absorbing carrier layer suppresses back reflection caused by exposure. S3. After exposure, heat treatment is performed to reduce the peeling force of the transparent heat-resistant pressure-sensitive adhesive layer, and then the functional film is peeled off from the surface of the transparent substrate.
[0025] The objectives of this invention and the technical problems solved can be further achieved by the following technical measures.
[0026] Compared to existing back-reflection suppression films and thermally anti-adhesive tapes for transparent substrate exposure, the UV-absorbing thermally anti-adhesive functional film with an interface transition structure, its preparation method, and its application described in this invention have at least the following beneficial effects: (1) Improve the bonding stability between the light-absorbing carrier layer and the heat-resistant pressure-sensitive adhesive layer. This invention regulates the pre-curing state of the ultraviolet light-absorbing carrier layer and uses the solvent in the pressure-sensitive adhesive composition to cause limited swelling of the surface of the light-absorbing carrier layer, so that the two polymer materials undergo chain segment diffusion and interpenetration, and further forms an interpenetrating transition region through thermal curing.
[0027] Compared to the abrupt physical bonding interface formed between traditional black PET film and pressure-sensitive adhesive, this invention reduces the interface differences between different functional layers by constructing a continuous transition structure, thereby improving the bonding stability between the light-absorbing carrier layer and the heat-resistant pressure-sensitive adhesive layer.
[0028] This helps maintain the structural integrity of the functional film during the bonding, exposure, and subsequent heat treatment processes on the transparent substrate.
[0029] (2) Achieving synergistic design of ultraviolet absorption functional layer and composite structure stability This invention uses UV-curable acrylic resin as the substrate for the ultraviolet light-absorbing carrier layer, and combines it with benzotriazole ultraviolet absorbing materials and black light-absorbing materials to form a composite absorption system.
[0030] Among them, benzotriazole-based ultraviolet absorbing materials can enhance the absorption capacity of ultraviolet light near 365nm, while black light-absorbing materials further improve the overall light absorption level, thereby reducing the influence of back-reflected light during the exposure of transparent substrates.
[0031] Meanwhile, since the light-absorbing carrier layer adopts a polymer continuous phase structure, it can form an interfacial interpenetration transition structure with the transparent heat-resistant pressure-sensitive adhesive layer, avoiding the problem of insufficient bonding stability between the light-absorbing functional layer and the adhesive layer in traditional black film layers.
[0032] Therefore, the present invention can meet the requirement of reducing back reflection during the front exposure process of transparent substrates.
[0033] (3) It has good process synergy with the post-exposure baking process.
[0034] The thermal de-adhesion temperature of this invention can be matched with the post-baking temperature after exposure of the transparent substrate. When the post-baking temperature reaches the response temperature range of the thermal de-adhesion pressure-sensitive adhesive layer, the existing heat during the post-baking process can be directly used to induce a response in the thermally expanded microspheres. Combined with the change in the mechanical state of the adhesive layer caused by docosahexamethicone, the peel force of the functional film is significantly reduced. Therefore, thermal de-adhesion of the functional film can be achieved simultaneously with the post-baking process, eliminating the need for an additional heating step for functional film removal. This reduces process steps, shortens the processing flow, and improves compatibility with existing exposure processing techniques.
[0035] (4) Improve the controllability of the thermal viscosity reduction process This invention introduces poly(2-diethyl acrylate) as a thermal response regulating component into a transparent heat-resistant pressure-sensitive adhesive layer.
[0036] During heat treatment, poly(2-diethyl acrylate) softens or undergoes a phase change, which adjusts the mechanical properties of the pressure-sensitive adhesive layer and reduces the layer's resistance to interfacial deformation.
[0037] Meanwhile, the thermally expanding microspheres expand in volume when heated, further altering the internal stress state of the adhesive layer and promoting a decrease in adhesion performance after heat treatment.
[0038] The combined effect of the aforementioned thermally responsive components improves the controllability of the functional membrane's transition from the adhered state to the release state.
[0039] (5) A balance between adhesion stability and release capacity is achieved through the thermal expansion microsphere gradient structure. This invention differs from the existing method of uniformly distributing thermally expandable microspheres in heat-resistant adhesives. By controlling the thermally expandable microspheres to exhibit a non-uniform gradient distribution along the thickness direction of the functional film, with low-high-low concentration, different regions can perform different functions.
[0040] The first low-concentration region is located on the side close to the ultraviolet light-absorbing carrier layer, which is used to reduce the disturbance to the interlayer interface during thermal expansion; the middle high-concentration region serves as the main thermal response region; and the second low-concentration region is located on the substrate bonding side, which is used to reduce the adverse effects of microspheres on the flatness of the bonding interface and the initial adhesion performance.
[0041] Therefore, the present invention can maintain good structural stability during the exposure and bonding stage, while providing controllable release capability during the heat treatment stage.
[0042] (6) Reduce the problem of uncontrollable interface failure location in traditional heat release membranes This invention enables different regions within the functional membrane to exhibit differentiated bonding and response characteristics through the synergistic design of an interfacial interpenetration transition structure and a gradient thermal response structure.
[0043] During the heat treatment process: polyacrylic acid 22-diester softens → the deformation capacity of the pressure-sensitive adhesive layer is improved → the thermally expanded microspheres generate spatially controlled expansion stress → promoting the controllable peeling between the functional film and the transparent substrate.
[0044] Compared to the random interlayer damage or adhesive residue problems in traditional heat-release films, this invention can improve the controllability of the heat release process and help reduce the risk of residual adhesive during the peeling process.
[0045] (7) It has good process compatibility and application adaptability. The ultraviolet light-absorbing carrier layer, acrylic pressure-sensitive adhesive system, and thermally responsive microsphere structure used in this invention can all be prepared using conventional coating processes. Continuous preparation of the functional film can be achieved through roller coating, multi-stage coating, and thermal curing processes.
[0046] Therefore, this invention is applicable to front-side exposure-assisted processing of transparent substrates such as quartz glass and optical glass.
[0047] The above description is merely an overview of the technical solution of the present invention. In order to better understand the technical means of the present invention and to implement it in accordance with the contents of the specification, the preferred embodiments of the present invention are described in detail below. Attached Figure Description
[0048] Figure 1 This is a schematic diagram showing the overall structure and application of the ultraviolet light-absorbing thermal anti-adhesion functional film of the present invention. Figure 1 (a) is a schematic diagram of the overall structure of the functional membrane. Figure 1 (b) is a schematic diagram of the application state of the functional film being bonded to the back of a transparent substrate; Figure 2 This is an enlarged schematic diagram of the interfacial interpenetration transition region of the present invention; Figure 3 This is a schematic diagram of the low-concentration-high-concentration gradient distribution of the thermally expandable microspheres along the thickness direction of the functional membrane according to the present invention; Figure 4 This is a process flow diagram for preparing the ultraviolet light-absorbing thermal anti-adhesion functional film of the present invention; Figure 5 This is a schematic diagram of the peeling mechanism before and after heat treatment according to the present invention; Figure 6 This is a cross-sectional SEM image (×500) of the gradient distribution of the thermally expanded microspheres in Embodiment 1 of the present invention. Figure 7 SEM images of the transition area between the ultraviolet light-absorbing carrier layer and the transparent thermally de-adhesive pressure-sensitive adhesive layer in Embodiment 1 of the present invention: (a) ×1000; (b) ×5000; Figure 8 SEM images of the interface between the UV-absorbing carrier layer and the transparent heat-resistant pressure-sensitive adhesive layer in Comparative Example 1: (a) ×200; (b) ×1000; Explanation of reference numerals in the attached figures: 1-First release protective layer; 2-UV light-absorbing carrier layer; 3-Interfacial interpenetration transition region; 4-Transparent thermally reducing pressure-sensitive adhesive layer; 5-Second release protective layer; 6-Photoresist; 7-Transparent substrate; 8-First low-concentration region; 9-Intermediate high-concentration region; 10-Second low-concentration region; 11-Thermal expansion microspheres; 12-365nm exposure; 13-Back reflection light; 14-Pre-curing treatment; 15-Limited swelling treatment with organic solvent; 16-Thermal curing treatment; 17-Abrupt interface. Detailed Implementation
[0049] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the following, in conjunction with preferred embodiments, provides a detailed description of the specific implementation methods, structure, features, and effects of the ultraviolet light-absorbing thermal anti-adhesion functional film with an interface transition structure proposed in the present invention, its preparation method, and its application.
[0050] Unless otherwise specified, all materials and reagents mentioned below are commercially available products well-known to those skilled in the art; unless otherwise specified, all methods described are methods known in the art. Unless otherwise defined, the technical or scientific terms used should have the ordinary meaning understood by those skilled in the art. Where specific experimental steps or conditions are not specified below, they can be performed according to the conventional experimental steps or conditions described in the literature in this field.
[0051] To address the problems of insufficient bonding between the light-absorbing layer and the adhesive layer, uncontrollable heat release process, and difficulty in simultaneously achieving optical and adhesive properties in existing back-side reflection suppression films for transparent substrate exposure, some embodiments of the present invention provide a UV-absorbing thermally de-adhesive functional film with an interface transition structure, see [link to relevant documentation]. Figures 1-5 The functional film includes an ultraviolet light-absorbing carrier layer 2 and a transparent heat-resistant pressure-sensitive adhesive layer 4 disposed on one side of the ultraviolet light-absorbing carrier layer 2. The ultraviolet light-absorbing carrier layer 2 is a polymer functional layer with ultraviolet absorption capability, used to absorb ultraviolet light during the exposure process of the transparent substrate 7 and reduce the back reflection generated by the exposure light inside the transparent substrate. The transparent heat-resistant pressure-sensitive adhesive layer 4 is used to achieve stable adhesion between the functional film and the transparent substrate 7 and controllable peeling after heat treatment, and the adhesion performance decreases under heat treatment conditions to achieve controllable peeling of the functional film. The ultraviolet light-absorbing carrier layer 2 comprises a UV-curable acrylic resin matrix, a benzotriazole ultraviolet absorber, and a black light-absorbing material. The UV-curable acrylic resin matrix forms a continuous film, providing the necessary film-forming properties, mechanical strength, and load-bearing capacity during overall peeling, and allowing the carrier layer to retain a certain interfacial response capability through pre-curing 14. The benzotriazole ultraviolet absorber absorbs ultraviolet light around 365nm, reducing the reflection of ultraviolet light transmitted through the transparent substrate 7 on the back side of the substrate. The black light-absorbing material further absorbs ultraviolet light and scattered light that are not fully absorbed by the benzotriazole ultraviolet absorber, improving the overall light absorption capacity of the carrier layer. Through the synergistic effect of these three components, while maintaining the continuous film formation and structural integrity of the ultraviolet light-absorbing carrier layer 2, the absorption capacity for the 365nm exposure band can be improved, thereby effectively reducing the exposure reflection on the back side of the transparent substrate 7. The UV-curable acrylic resin serves as the continuous phase of the light-absorbing carrier layer, providing the polymer base required for the film's mechanical strength, film-forming properties, and subsequent interfacial interpenetration structure formation. The benzotriazole UV absorber exhibits characteristic absorption around 365 nm, enhancing the light-absorbing carrier layer's absorption capacity for exposed UV light and assisting in adjusting the film's optical response characteristics. The benzotriazole UV absorber includes, but is not limited to, 2-(2H-benzotriazole-2-yl)-4,6-di-tert-pentylphenol, 2-(2H-benzotriazole-2-yl)-4,6-di-tert-butylphenol, and other benzotriazole compounds with UV absorption capabilities. The black light-absorbing material further enhances the overall light absorption capacity of the UV light-absorbing carrier layer 2, reducing back-reflected light generated during the exposure of the transparent substrate 7. The black light-absorbing material includes, but is not limited to, nano-carbon black, black organic pigments, and other black fillers with broad-spectrum absorption capabilities. Unlike traditional black PET films that rely on high black pigment content for light blocking, this invention employs a composite design of black light-absorbing materials and molecular-type ultraviolet-absorbing materials. This achieves ultraviolet light absorption capacity with a relatively thin film layer thickness, while maintaining the composite stability between the light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4. The ultraviolet light-absorbing carrier layer 2 in this invention is not simply used as a light-blocking film, but simultaneously serves as: ultraviolet exposure light absorption, mechanical support for the functional film, and a carrier for forming the interfacial interpenetration region 3 with the transparent heat-resistant pressure-sensitive adhesive layer 4.
[0052] The transparent heat-resistant pressure-sensitive adhesive layer 4 comprises an acrylic copolymer, poly(dodecyl acrylate), and thermally expandable microspheres 11. The acrylic copolymer serves as the main component of the pressure-sensitive adhesive, providing initial adhesion, cohesive strength, and basic film-forming properties to the transparent substrate 7 at room temperature. The poly(dodecyl acrylate), as a thermal response modifier, is physically blended and dispersed within the pressure-sensitive adhesive system. During heating, it helps regulate the mechanical state of the adhesive layer, making it easier for the adhesive layer to reduce adhesion after heat treatment. The thermally expandable microspheres 11 expand in volume upon reaching the response temperature, causing localized deformation and expansion stress within the pressure-sensitive adhesive layer and reducing the effective contact between the pressure-sensitive adhesive layer and the transparent substrate 7, thereby further reducing the peel force. Through the synergistic effect of these three components, the transparent heat-resistant pressure-sensitive adhesive layer 4 maintains reliable adhesion at room temperature, while significantly reducing the peel force after heat treatment, achieving a transition from a stable adhesive state to an easily peelable state. The transparent heat-resistant pressure-sensitive adhesive layer 4 is disposed on the side of the interfacial interpenetration transition region 3 away from the ultraviolet light-absorbing carrier layer 2; the acrylic copolymer matrix is formed by copolymerization of soft monomers, hard monomers, and functional monomers. The soft monomers are selected from one or more of isooctyl acrylate and lauryl acrylate. Soft monomers are used to lower the glass transition temperature of the polymer, improve the flexibility of the adhesive layer, and enhance the wettability of the transparent substrate 7 surface. The hard monomers are selected from methyl methacrylate. Hard monomers are used to improve the cohesive strength, dimensional stability, and heat resistance of the adhesive layer. The functional monomers are selected from acrylamide. Functional monomers are used to enhance the inter-segment interaction of the polymer and improve the structural stability of the adhesive layer. Preferably, the acrylic copolymer matrix includes isooctyl acrylate, lauryl acrylate, methyl methacrylate, and acrylamide. The thermal response regulating component includes poly(docosahexamethacrylate). Poly(docosahexamethacrylate) has a long-chain alkyl side chain structure, which can maintain the structural stability of the adhesive layer under normal temperature conditions; under heat treatment conditions, the long-chain side chains soften or undergo phase changes, reducing the storage modulus of the pressure-sensitive adhesive layer and improving the deformation capability of the adhesive layer. The poly(2-diethyl acrylate) is used to assist the thermally expandable microspheres 11 in generating heat release, thereby improving the effect of reducing adhesive adhesion during heat treatment. The thermally expandable microspheres 11 are dispersed in the transparent heat-resistant pressure-sensitive adhesive layer 4. The thermally expandable microspheres include a polymer shell and a low-boiling-point foaming medium encapsulated within the shell. During heat treatment: the low-boiling-point foaming medium vaporizes upon heating, increasing the internal pressure and thus driving the microspheres to expand, altering the internal stress state of the adhesive layer. The thermally expandable microspheres 11 promote changes in the mechanical properties of the transparent heat-resistant pressure-sensitive adhesive layer 4, achieving controllable peeling after heat treatment.
[0053] A continuous interfacial interpenetration transition region 3 is provided between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4. The continuous interfacial interpenetration transition region 3 is formed by pre-curing, limited solvent swelling, and thermal curing. The cross-sectional morphology gradually changes from the ultraviolet light-absorbing carrier layer 2 to the transparent heat-resistant pressure-sensitive adhesive layer 4 without obvious abrupt boundaries. The interfacial interpenetration transition region 3 is used to enhance the bonding stability between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4. The continuous interfacial interpenetration transition region 3 can improve the bonding stability between different functional layers. Unlike the abrupt interface 17 formed between different material layers in traditional light-absorbing films, this invention controls the curing state of the ultraviolet light-absorbing carrier layer 2, so that while maintaining the overall film structure stability, the surface layer retains a certain chain migration ability and swelling response ability. During the formation of the transparent heat-resistant pressure-sensitive adhesive layer 4, the organic solvent in the pressure-sensitive adhesive composition can induce a limited swelling treatment 15 on the surface of the pre-cured ultraviolet light-absorbing carrier layer 2, causing the polymer segments in the pressure-sensitive adhesive to diffuse into the surface region of the ultraviolet light-absorbing carrier layer 2. Subsequently, through a heat curing treatment 16, the polymer segments on both sides further migrate and entangle, thereby forming a continuous transitional interfacial interpenetration region 3 between the two functional layers. The interfacial interpenetration transition region 3 has the following characteristics: (1) The interfacial interpenetration transition region 3 is not an independently set third functional layer, but is formed during the composite process of the ultraviolet light-absorbing bearing layer 2 and the transparent heat-reducing pressure-sensitive adhesive layer 4; (2) The interface region reduces the obvious abrupt interface 17 between different materials in traditional composite films and improves the bonding stability between functional layers; (3) The interface region can improve the structural stability of the functional film during the exposure and bonding process; (4) The interface region can adjust the peeling behavior during the heat treatment process, so that the functional membrane can achieve a more controllable detachment process.
[0054] Preferably, the interfacial interpenetration transition region 3 is formed in the following manner: ① The ultraviolet light-absorbing carrier layer 2 is pre-cured 14; ② Coat the surface of the pre-cured UV-absorbing bearing layer 2 with a transparent heat-resistant pressure-sensitive adhesive composition; ③ The surface of the light-absorbing layer is subjected to limited swelling treatment using organic solvents in the pressure-sensitive adhesive composition 15; ④ Perform thermal curing treatment 16 at a temperature lower than the initial expansion temperature of the thermal expansion microspheres 11 to further diffuse the polymer chain segments and stabilize the interface structure.
[0055] To achieve spatial stress regulation during the heat release process, this invention further designs the distribution of thermally expandable microspheres 11 in the transparent thermally non-adhesive pressure-sensitive adhesive layer 4. Along the thickness direction of the transparent thermally non-adhesive pressure-sensitive adhesive layer, the thermally expandable microspheres 11 exhibit a non-uniform distribution: a high-concentration region 9 in the middle, a first low-concentration region 8 near the ultraviolet light-absorbing carrier layer 2, and two low-concentration regions 10 near the substrate bonding side with lower concentrations on both sides. That is, the thermally expandable microspheres 11 exhibit a non-uniform gradient distribution along the thickness direction of the functional film: first low-concentration region 8 – middle high-concentration region 9 – second low-concentration region 10. (See [reference]). Figure 3 The non-uniform distribution of thermally expanding microspheres 11 along the thickness direction enables stress release regulation during heat treatment. A first low-concentration region 8 near the UV-absorbing carrier layer 2 reduces disturbance to the interlayer interface and localized stress concentration near the interface during thermal expansion. A middle high-concentration region 9 serves as the main thermal response region, generating significant internal expansion stress during heat treatment. A second low-concentration region 10 near the substrate bonding side reduces the impact of the microspheres on the flatness of the substrate bonding interface and the effective adhesion area, maintaining the initial adhesion performance of the functional film. Through this low-high-low gradient structure, the thermally expanding microspheres 11 are transformed from a traditional uniform distribution to a thermally responsive structure with spatial controllability, achieving a balance between stable bonding at room temperature and controllable release during heat treatment.
[0056] In some optional embodiments, the thickness of the ultraviolet absorbing carrier layer 2 can be 3–15 μm. A thickness less than 3 μm may result in insufficient film integrity, mechanical support, and ultraviolet absorption; a thickness greater than 15 μm may increase material usage and affect curing uniformity and subsequent overall peel performance. Therefore, controlling its thickness within 3–15 μm is beneficial for balancing ultraviolet absorption, structural stability, and peel performance. Preferably, it is 5–10 μm, as this range is more conducive to balancing back reflection suppression near 365 nm, film integrity, and the formation of subsequent interface transition structures.
[0057] Based on a total solid component mass of 100 parts by mass of the ultraviolet light-absorbing support layer 2, the ultraviolet light-absorbing support layer 2 comprises: 70-82 parts by weight of UV-curable acrylic resin; 10-18 parts by weight of reactive diluent; 2-5 parts by weight of benzotriazole UV absorber; 2-5 parts by weight of black light-absorbing material; Photoinitiator 1.5–3 parts by weight; Dispersant 0.5 to 1.5 parts by weight.
[0058] The dosage of each component is selected under the premise that the total solid components amount to 100 parts by mass. When the UV-curable acrylic resin dosage is less than 70 parts, it may lead to insufficient film-forming properties and mechanical strength; when it is more than 82 parts, it will relatively reduce the content of other functional components, which is not conducive to UV absorption and curing regulation. When the reactive diluent dosage is less than 10 parts, the system viscosity is high and the coating leveling is poor; when it is more than 18 parts, it may reduce the strength and dimensional stability of the cured film. When the benzotriazole UV absorber dosage is less than 2 parts, the absorption of UV light near 365nm is insufficient; when it is more than 5 parts, it affects the UV curing efficiency and film performance. When the black light-absorbing material dosage is less than 2 parts, the auxiliary light absorption effect is insufficient; when it is more than 5 parts, it leads to enhanced light shielding, affecting the curing depth and film uniformity. When the photoinitiator dosage is less than 1.5 parts, it will lead to insufficient curing; when it is more than 3 parts, it may cause excessively rapid curing and affect the control of the pre-cured state. When the dispersant dosage is less than 0.5 parts, the black light-absorbing material is prone to agglomeration; when it is more than 1.5 parts, it will have an adverse effect on film strength and interfacial properties. The above range is advantageous for balancing coating and film formation, 365nm ultraviolet absorption, controllable pre-curing, and film structure stability.
[0059] In some optional embodiments, the black light-absorbing material is selected from one or more of carbon black, graphite, graphene, carbon nanotubes, iron oxide, or other black inorganic light-absorbing pigments. This black light-absorbing material can further absorb light that has not been fully absorbed by benzotriazole UV absorbers, thereby improving the overall light absorption capacity of the UV light-absorbing carrier layer 2 and reducing back reflection light 13. Preferably, nano-carbon black is used. Nano-carbon black has a high specific surface area and strong light absorption capacity, achieving good light absorption effects at low addition levels. Simultaneously, its small particle size facilitates uniform dispersion in the film, reducing the adverse effects of localized agglomeration on film uniformity and curing performance.
[0060] In some alternative embodiments, the acrylic copolymer is obtained by polymerization of a monomer composition comprising isooctyl acrylate, lauryl acrylate, methyl methacrylate and acrylamide; Based on a total monomer composition of 100 parts by weight, isooctyl acrylate comprises 40–70 parts by weight, lauryl acrylate comprises 5–25 parts by weight, methyl methacrylate comprises 10–35 parts by weight, and acrylamide comprises 0.5–10 parts by weight. Specifically, isooctyl acrylate below 40 parts by weight is detrimental to achieving sufficient flexibility and initial tack; above 70 parts by weight, it tends to result in an overly soft adhesive layer and decreased cohesive strength. Lauryl acrylate below 5 parts by weight does not effectively regulate the flexibility and hydrophobicity of the adhesive layer; above 25 parts by weight, it tends to decrease the cohesive strength and heat resistance of the adhesive layer. Methyl methacrylate below 10 parts by weight is detrimental to improving the rigidity and cohesive strength of the adhesive layer; above 35 parts by weight, it tends to result in an overly hard adhesive layer and decreased initial adhesion. Acrylamide below 0.5 parts by weight is detrimental to improving copolymer polarity and cohesive action; above 10 parts by weight, it tends to result in excessively high system polarity and adversely affects the flexibility and bonding performance of the adhesive layer. The above range is beneficial for balancing the initial adhesion, cohesive strength, flexibility, and heat-induced tack reduction properties of pressure-sensitive adhesives.
[0061] Based on 100 parts by weight of the solids of the acrylic copolymer, the amount of poly(dodecyl acrylate) added is 3-15 parts by weight. Adding less than 3 parts by weight is not conducive to fully utilizing its role in regulating the thermal response and mechanical state of the pressure-sensitive adhesive after heating; adding more than 15 parts by weight can adversely affect the room-temperature adhesion performance, flexibility, and system compatibility of the pressure-sensitive adhesive. Controlling its addition amount to 3-15 parts by weight is beneficial for maintaining room-temperature adhesion performance while improving the anti-tack response after heating, thus balancing initial adhesion and easy peeling performance after heat treatment. It is dispersed in the transparent heat-resistant anti-tack pressure-sensitive adhesive layer through physical blending.
[0062] In some optional embodiments, the transparent heat-resistant pressure-sensitive adhesive layer 4 is sequentially divided into a first low-concentration region 8, an intermediate high-concentration region 9, and a second low-concentration region 10 along its thickness direction. The content of thermally expandable microspheres 11 in the first low-concentration region 8 and the second low-concentration region 10 is based on the total solid mass of acrylic copolymers and poly(dodecyl acrylate) in the corresponding regions, and is 0.5–2 wt% for each. When the content is below 0.5 wt%, it is not conducive to forming sufficient thermal response; when it is above 2 wt%, it is easy to adversely affect the interface stability and initial adhesion performance near the UV-absorbing carrier layer and the substrate bonding side. Controlling it at 0.5–2 wt% is beneficial to provide an auxiliary response for overall thermal de-adhesion while maintaining the stability of the interface and the bonding performance on both sides. The content of thermally expandable microspheres 11 in the intermediate high-concentration region 9 is 4–8 wt%. When the content is below 4 wt%, it is not conducive to forming sufficient central thermal expansion response, and the thermal de-adhesion effect is insufficient; when it is above 8 wt%, it is easy to cause excessive expansion inside the adhesive layer, local stress concentration, and decreased structural stability. Controlling it at 4–8 wt% is beneficial to concentrate the main thermal response in the middle of the adhesive layer, and reduce the disturbance to the interface on both sides while obtaining a significant thermal de-adhesion effect.
[0063] Furthermore, the contents of the thermally expanded microspheres 11 in the first low-concentration region 8, the intermediate high-concentration region 9, and the second low-concentration region 10 are 1wt%, 6wt%, and 1wt% respectively, based on the total solid mass of the acrylic copolymer and poly(dodecyl acrylate) in the corresponding regions, and the thicknesses of the corresponding regions are 15μm, 20μm, and 15μm respectively. The above-mentioned 1wt%-6wt%-1wt% and 15μm-20μm-15μm are preferred parameter combinations, which are beneficial to concentrate the main thermal response in the middle of the adhesive layer, while reducing the microsphere content at the two side interfaces, thereby taking into account the initial adhesion performance, thermal detack reduction effect, and interlayer structural stability.
[0064] In some optional embodiments, the UV-absorbing heat-resistant adhesive functional film further includes a first release protective layer 1 and a second release protective layer 5. The first release protective layer 1 is disposed on the side of the UV-absorbing carrier layer 2 away from the transparent heat-resistant adhesive pressure-sensitive layer 4, and the second release protective layer 5 is disposed on the side of the transparent heat-resistant adhesive pressure-sensitive layer 4 away from the UV-absorbing carrier layer 2. Both the first release protective layer 1 and the second release protective layer 5 are removable protective layers. The first release protective layer 1 and the second release protective layer 5 can protect the surfaces of the UV-absorbing carrier layer 2 and the transparent heat-resistant adhesive pressure-sensitive layer 4 respectively, reducing the risk of contamination, scratches, or adhesion to the functional film during storage, transportation, and cutting. Simultaneously, both release protective layers can be easily removed during use, which helps maintain the stability of the functional film surface and facilitates subsequent bonding of the transparent heat-resistant adhesive pressure-sensitive layer 4 to the transparent substrate 7.
[0065] Some embodiments of the present invention also provide a method for preparing the above-mentioned ultraviolet light-absorbing thermal anti-adhesion functional film, see [link to relevant documentation]. Figure 4The preparation process flow chart includes the following steps: (1) Provide a first release protection substrate; select a substrate with release properties as the carrier substrate in the preparation process of the functional film.
[0066] The first release protective substrate includes, but is not limited to, PET release film, PE release film, and silicone release paper. PET release film is preferred. By performing a release treatment on the surface of the release layer, it can support the subsequent formation of the ultraviolet light-absorbing coating and be peeled off when the functional film is used.
[0067] (2) A UV-curable acrylic resin, a benzotriazole UV absorber, a black light-absorbing material and a photoinitiator are mixed to obtain a UV-absorbing coating composition; (3) The UV-absorbing coating composition is coated onto the surface of the first release protective substrate by roller coating, and a first-stage UV pre-curing treatment 14 is performed to obtain a pre-cured UV-absorbing carrier layer 2 that maintains the complete film morphology and has limited swelling capacity to organic solvents on the surface. Among them, the roller coating method is beneficial to obtain a UV-absorbing carrier layer 2 with uniform thickness and continuous surface; the first-stage UV pre-curing treatment 14 makes the film layer have sufficient structural integrity and mechanical stability, while retaining the limited swelling capacity of the surface layer to organic solvents in the subsequent pressure-sensitive adhesive system, which is conducive to the subsequent diffusion of interfacial segments and the formation of continuous interfacial interpenetration transition region 3, and takes into account the film layer forming stability and interlayer bonding performance.
[0068] (4) Physically blending acrylic copolymers with poly(2-diacrylate) is beneficial to introduce thermal response regulation while maintaining the adhesion performance of the pressure-sensitive adhesive; adding organic solvents can adjust the viscosity and flowability of the system, which is convenient for subsequent uniform coating; by preparing multiple pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres 11, conditions can be provided for the subsequent construction of a microsphere distribution structure of the first low-concentration region 8-intermediate high-concentration region 9-second low-concentration region 10 along the thickness direction of the adhesive layer, thereby taking into account the initial adhesion performance, thermal de-tack response and interlayer structure stability. (5) Using a multi-stage roller coating method, transparent thermally resistant pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres 11 are sequentially coated onto the surface of the pre-cured ultraviolet light-absorbing carrier layer 2. During the coating process, organic solvents produce organic solvent limited swelling treatment 15 on the surface of the pre-cured ultraviolet light-absorbing carrier layer 2. By adjusting the content of thermally expandable microspheres 11 in different coating stages, the thermally expandable microspheres 11 are distributed in a non-uniform manner along the thickness direction of the formed transparent thermally resistant pressure-sensitive adhesive layer 4, with low concentration on both sides and high concentration in the middle. (6) A thermal curing treatment 16 is performed under conditions lower than the initial expansion temperature of the thermally expandable microspheres 11. Preferably, the thermal curing temperature is 50-80°C, the thermal curing time is 10-60 min, and the thermal curing temperature is lower than the initial expansion temperature of the thermally expandable microspheres 11. When the thermal curing temperature is lower than 50°C or the time is less than 10 min, it is not conducive to the full evaporation of organic solvents and the migration and diffusion of polymer chain segments in the interfacial region, and the interfacial interpenetration transition region is not fully formed. When the thermal curing temperature is higher than 80°C, it is easy to approach the initial expansion temperature of the thermally expandable microspheres 11, increasing the risk of premature expansion of microspheres and local deformation of the adhesive layer. When the thermal curing time exceeds 60 min, the further curing effect is limited, and the thermal history and process time will be increased. Controlling the thermal curing conditions within the above range is beneficial to promoting solvent evaporation and interfacial chain segment diffusion, stabilizing the interfacial interpenetration transition region 3 and the spatial distribution of microspheres, and avoiding pre-expansion of microspheres during the preparation stage.
[0069] (7) A second release protective layer 5 is laminated on the side of the transparent heat-resistant pressure-sensitive adhesive layer 4 away from the ultraviolet light-absorbing carrier layer 2; the second release protective layer 5 is used to protect the surface of the heat-resistant pressure-sensitive adhesive and avoid contamination or adhesion during storage and transportation.
[0070] (8) Winding and cutting to obtain the ultraviolet light-absorbing thermal de-adhesion functional film with interfacial interpenetration transition structure and gradient thermal response capability.
[0071] In some optional embodiments, in step (5), a transparent thermally reducing pressure-sensitive adhesive composition with low, high, and low contents of thermally expanding microspheres is sequentially coated, with the contents of thermally expanding microspheres 11 in the corresponding regions being 0.5–2 wt%, 4–8 wt%, and 0.5–2 wt%, respectively. The contents of the low thermally expanding microspheres 11 on both sides are 0.5–2 wt%. When the content is below 0.5 wt%, it is not conducive to the participation of the two side regions in the overall thermal response; when it is above 2 wt%, it is easy to weaken the initial adhesion performance of the substrate bonding side and increase the interface stress during heat treatment on the carrier layer side. The contents of the high thermally expanding microspheres 11 in the middle are 4–8 wt%. When the content is below 4 wt%, the thermal expansion response in the middle region is insufficient; when it is above 8 wt%, it is easy to cause excessive local expansion of the adhesive layer and stress concentration. The use of a low-high-low distribution of 0.5~2wt%-4~8wt%-0.5~2wt% helps to concentrate the main thermal response in the middle of the adhesive layer, while maintaining the adhesion and structural stability of the two side interfaces, thus taking into account room temperature bonding, thermal de-adhesion and whole film peeling performance.
[0072] In some optional embodiments, the organic solvent includes ethyl acetate, which is beneficial for adjusting the viscosity and flowability of the transparent heat-resistant pressure-sensitive adhesive composition, facilitating uniform coating. Simultaneously, ethyl acetate can produce a moderate, limited swelling effect on the surface of the pre-cured UV-absorbing carrier layer 2, providing conditions for subsequent interfacial segment migration and the formation of continuous interfacial transition regions 3. It can also be easily volatilized and removed during the thermal curing treatment 16, thus balancing coating processability, interfacial bonding, and residual solvent control. The thermal curing temperature is lower than the initial expansion temperature of the thermally expandable microspheres 11 used to avoid significant pre-expansion of the thermally expandable microspheres 11 during the thermal curing treatment 16. It should be understood that the thermal curing conditions should promote the volatilization of the organic solvent and the migration and diffusion of polymer segments in the interfacial region, while the thermal curing temperature should be lower than the initial expansion temperature of the selected thermally expandable microspheres 11 to avoid significant pre-expansion of the thermally expandable microspheres 11 during the thermal curing treatment 16.
[0073] Some embodiments of the present invention also provide a method for suppressing back reflection during ultraviolet exposure on the front side of a transparent substrate, using the aforementioned ultraviolet light-absorbing thermal anti-adhesion functional film, see [link to relevant documentation]. Figure 1 (b) Figure 5 It includes the following steps: S1. The second release protective layer for peeling off the functional film is used to attach the transparent heat-resistant pressure-sensitive adhesive layer 4 to the back of the transparent substrate 7. S2. Peel off the first release protective layer 1, with the ultraviolet light-absorbing carrier layer 2 on the outside, and perform 365nm exposure 12. The ultraviolet light-absorbing carrier layer 2 suppresses the back reflection light generated by the exposure 13. S3. After exposure, heat treatment is performed to peel the functional film off the surface of the transparent substrate 7. Photoresist 6 is applied to the front side of the substrate.
[0074] The present invention will be further described below with reference to specific embodiments, but this should not be construed as a limitation on the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the above description of the present invention still fall within the scope of protection of the present invention.
[0075] Performance testing and characterization methods To evaluate the optical properties, thermal de-adhesion properties, peel integrity, and internal structural features of the UV-absorbing thermal de-adhesion functional film of the present invention, the examples and comparative samples were tested and characterized according to the following methods.
[0076] 1.365 nm reflectance test The transparent heat-resistant pressure-sensitive adhesive layer 4 of the functional film to be tested was bonded to the back of a quartz substrate, ensuring that the bonding area was flat and free of obvious bubbles and wrinkles, thus obtaining a composite test sample of "quartz substrate / transparent heat-resistant pressure-sensitive adhesive layer 4 / UV light-absorbing carrier layer 2". An identical quartz substrate without the functional film attached was used as a blank control, and the reflectance at a wavelength of 365 nm was measured under the same test conditions. The reflectance at 365 nm was denoted as R. The relative decrease in reflectance before and after bonding of the functional film was calculated using the following formula: Relative reduction rate of reflectivity = (R0 - R1) / R0 × 100% Wherein: (R0) is the reflectance of the quartz substrate without the functional film at 365 nm; (R1) is the reflectance of the quartz substrate with the functional film attached at 365 nm. The quartz substrate without the functional film used in this embodiment has a reflectance of 5.3% at 365 nm.
[0077] 2. Peel force test before heat treatment The peel force was tested using the same method as the 180° peel test for pressure-sensitive adhesives, with a sample width of 25 mm and a peel rate of 300 mm / min. The release protective layer 5 on the pressure-sensitive adhesive side of the functional film was removed, and the transparent heat-resistant pressure-sensitive adhesive layer 4 was uniformly bonded to the surface of the quartz substrate. Test samples were prepared under the same bonding conditions.
[0078] Peel tests were performed on the functional film in its untreated state. All peel force tests were conducted according to Method 1 of GB / T2792-2014 "Test Method for Peel Strength of Adhesive Tapes" using a 180° peel method. A quartz substrate was used as the test substrate, unlike the stainless steel plate specified in the standard method. Test results are expressed in N / cm and are considered as the peel force of the functional film before heat treatment. All embodiments and comparative examples used the same sample size, bonding method, and peel test conditions to ensure comparability of test results.
[0079] 3. Peel force test after heat treatment Peel strength was tested using the same method as pressure-sensitive adhesive (180° peel test), with a sample width of 25 mm and a peel rate of 300 mm / min. The functional film bonded to the quartz substrate was then heat-treated at 100°C for 90 seconds.
[0080] After heat treatment, the peel force of the functional film was tested under the same peel test conditions as before heat treatment, and the results were expressed in N / cm.
[0081] The peel force reduction rate is calculated using the following formula: Peel force reduction rate = (F0 - F1) / F0 × 100% Where: (F0) is the peeling force before heat treatment; (F1) is the peeling force after treatment at 100℃ for 90s.
[0082] When significant interlayer separation occurs between the UV-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 during the peeling process after heat treatment, resulting in the inability to obtain a meaningful whole-film peeling force, the whole-film peeling force reduction rate is not calculated for the sample, and its actual failure state is recorded.
[0083] 4. Evaluation of the peeling state after heat treatment The actual peeling process of the samples after treatment at 100℃ for 90 seconds was observed, and the following items were mainly evaluated: (1) Residual adhesive: Observe whether there is obvious pressure-sensitive adhesive residue on the surface of the quartz substrate after the functional film is peeled off; (2) Interlayer separation: Observe whether there is visible interlayer separation between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4; (3) Overall peeling: Observe whether the functional film can maintain the overall structure of the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 and peel off from the surface of the quartz substrate.
[0084] Samples in which no obvious pressure-sensitive adhesive residue was observed after peeling, no obvious interlayer separation occurred, and the functional membrane remained intact were recorded as whole-film peelable.
[0085] For samples that can be basically peeled off but exhibit slight interlayer separation during the process, they are recorded as samples that can be basically peeled off with slight interlayer separation.
[0086] For samples where the UV light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 are significantly separated during the peeling process, resulting in some pressure-sensitive adhesive layer remaining on the surface of the quartz substrate, the samples are recorded as samples that cannot be peeled off completely.
[0087] The evaluation levels are divided into: able to peel off the entire film, able to peel off the entire film (with slight interlayer separation), and unable to peel off the entire film.
[0088] 5. Cross-sectional SEM characterization The samples were prepared using a cryogenic fracture method. The functional membrane cross-section was sputter-coated with gold using a scanning electron microscope and observed under an accelerating voltage of 10 kV. (See attached image.) Figure 6 , Figure 7 , Figure 8 The spatial distribution of thermally expanded microspheres 11 along the thickness direction of the pressure-sensitive adhesive layer and the interface morphology between the ultraviolet light-absorbing carrier layer 2 and the transparent thermally de-adhesive pressure-sensitive adhesive layer 4 were evaluated.
[0089] Regarding the distribution structure of thermally expanded microspheres 11, the differences in microsphere distribution density were observed in the first low-concentration region 8 near the ultraviolet light-absorbing support layer 2, the middle high-concentration region 9, and the second low-concentration region 10 near the quartz substrate bonding side.
[0090] Regarding the interface structure, the focus is on observing whether there is a clear abrupt interface 17 boundary between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4, and whether there is a continuous morphological transition region 3 near the interface.
[0091] Example 1 (1) Provide the first release protective substrate A PET release film with a thickness of 50 μm was selected as the first release protective layer 1, and its release treatment surface was used as the coating surface for the subsequent ultraviolet light absorption coating.
[0092] The first release protective layer 1 is used to support the ultraviolet light-absorbing carrier layer 2 during the preparation process, and is peeled off from one side of the ultraviolet light-absorbing carrier layer 2 before the functional film is actually used.
[0093] (2) Preparation of ultraviolet light absorbing coating composition As shown in Table 1, the following components were weighed out based on a total mass of 100 parts by mass of the solid components of the UV-absorbing coating: Table 1
[0094] In this embodiment, the UV-curable acrylic resin used is Allnex EBECRYL 8402, which is a bifunctional aliphatic polyurethane acrylate oligomer. The UV-curable acrylic resin serves as the continuous phase of the UV-absorbing carrier layer 2; benzotriazole UV absorbers are used to enhance the absorption of UV light near 365nm; and nano-carbon black, as a black light-absorbing material, is used to further improve the broad-spectrum absorption capability of the UV-absorbing carrier layer 2.
[0095] In the preparation process, 3 parts by weight of nano-carbon black, 12 parts by weight of reactive diluent tripropylene glycol diacrylate (TPGDA), and 1 part by weight of polymeric wetting and dispersing agent (BYK-161, BYK Chemical Company) were first pre-dispersed. The mixture was stirred at 600 rpm for 8 minutes to initially mix the components, and then dispersed at 2000 rpm for 25 minutes to fully wet and uniformly disperse the nano-carbon black until no visible agglomerates were found in the system. Subsequently, 78 parts by weight of UV-curable acrylic resin were added and stirred until homogeneous. Then, 4 parts by weight of 2-(5-chloro-2H-benzotriazole-2-yl)-6-(1,1-dimethylethyl)-4-methylphenol (UV-326) were added as a benzotriazole UV absorber, and 2 parts by weight of phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (photoinitiator 819) were added and mixed thoroughly to obtain the UV-absorbing coating composition.
[0096] (3) Forming a pre-cured ultraviolet light-absorbing carrier layer The UV light-absorbing coating composition obtained in step (2) is uniformly coated onto the release treatment surface of the first PET release film using a roller coating method.
[0097] The coating amount is controlled so that the thickness of the UV-absorbing carrier layer 2 after curing is approximately 8 μm.
[0098] After coating, the first stage of UV pre-curing is performed using a 365nm UV light source with a light intensity of approximately 50mW / cm². 2 The irradiation time is approximately 5 seconds, corresponding to a UV irradiation energy of approximately 250 mJ / cm². 2 This allows the UV-absorbing coating to form a pre-cured UV-absorbing carrier layer 2 with a continuous film structure.
[0099] The first stage of curing does not completely cure the ultraviolet light-absorbing carrier layer 2. Instead, while ensuring that the film layer has sufficient morphological stability, it retains a certain ability of chain segment migration on its surface and the ability to undergo limited organic solvent swelling treatment 15 for the subsequent pressure-sensitive adhesive solvent, thus providing conditions for the formation of the subsequent interfacial interpenetration transition region.
[0100] It should be noted that although this formula contains benzotriazole UV absorbers, this step only requires complete pre-forming of the film layer, and deep full curing is not necessary; 250 mJ / cm 2 Lower UV irradiation energy is sufficient to form a continuous and complete membrane morphology, while the surface layer retains the ability of segments to migrate and swell to a limited extent with organic solvents, thus meeting the process requirements for the subsequent formation of interfacial interpenetration transition regions.
[0101] (4) Preparation of transparent heat-resistant pressure-sensitive adhesive composition 4.1 Preparation of acrylic copolymer matrix As shown in Table 2, the following monomers are weighed by mass: Table 2
[0102] Acrylic copolymers were prepared by free radical solution polymerization. Ethyl acetate was added as the reaction solvent, with 100 parts by weight of the four comonomers as the total mass. Azobisisobutyronitrile (AIB) was used as the free radical initiator at 0.5 wt% of the total mass of the four comonomers. Before polymerization, nitrogen gas with a purity of not less than 99.99% was introduced into the reaction system at a flow rate of 60 mL / min to replace the air in the system for 20 min. Nitrogen protection was maintained during the reaction. The reaction system was subjected to free radical solution polymerization at 75 °C for 6 h under stirring at 300 r / min to obtain an acrylic copolymer solution with isooctyl acrylate (2-EHA), lauryl acrylate (LA), methyl methacrylate (MMA), and acrylamide (AM) as comonomers.
[0103] After the polymerization reaction is completed, 50 parts by weight of ethyl acetate are added for dilution and solid content adjustment, so that the solid content of the resulting acrylic copolymer solution is about 40 wt%.
[0104] 4.2 Add polydodecyl acrylate Based on 100 parts by weight of the solids of the acrylic copolymer, 8 parts by weight of polydodecyl acrylate (TEGO® SP13-6 produced by Evonik in this example is a long-chain alkyl acrylate polymer containing dodecyl crystalline side chains) are added. The polydodecyl acrylate is slowly added to the acrylic copolymer solution, and stirred at 400 r / min for 45 min at 50°C to uniformly disperse the polydodecyl acrylate in the acrylic pressure-sensitive adhesive system, thus obtaining the basic heat-resistant pressure-sensitive adhesive liquid.
[0105] 4.3 Add thermally expanding microspheres Thermally expandable microspheres 11 were used as the thermally responsive component. The thermally expandable microspheres 11 used in this embodiment are Matsumoto F-48, with a median particle size D50 of 9–15 μm before expansion, an initial expansion temperature Ts of 90°C, and a maximum expansion temperature of 125–135°C. The 70°C thermal curing temperature used in this embodiment is lower than the initial expansion temperature, and the thermally expandable microspheres do not undergo significant pre-expansion during the thermal curing process. The heat treatment condition of 100°C × 90s is within the effective response temperature range of the thermally expandable microspheres, which can trigger volume expansion of the microspheres.
[0106] The base heat-sensitive adhesive liquid was divided into three parts and formulated into a first pressure-sensitive adhesive composition, a second pressure-sensitive adhesive composition, and a third pressure-sensitive adhesive composition with different contents of thermally expandable microspheres 11. Based on the total solid mass of the acrylic copolymer and poly(dodecyl acrylate), the addition amounts of thermally expandable microspheres 11 in the three compositions were as follows: first pressure-sensitive adhesive composition: 1 wt%; second pressure-sensitive adhesive composition: 6 wt%; third pressure-sensitive adhesive composition: 1 wt%.
[0107] (5) Multi-level coating forms a gradient structure of first low concentration region 8 - intermediate high concentration region 9 - second low concentration region 10. The surface of the pre-cured UV-absorbing carrier layer 2 obtained in step (3) is sequentially subjected to three-stage roller coating. Continuous coating is performed using a roller coating machine, with the coating speed controlled at 2 m / min. The thickness of each adhesive layer is controlled by adjusting the roller gap and the coating amount per unit area. Complete drying is not performed between each coating stage. After the previous adhesive layer has been surface-dried for a short time until it has a stable film shape and the surface still maintains a certain degree of tackiness, the next coating stage is immediately applied to ensure a certain compositional transition between adjacent areas and avoid the formation of completely independent interlayer interfaces. First, a first pressure-sensitive adhesive composition with a content of 1 wt% of thermally expandable microspheres 11 is coated to form a first low-concentration region 8 near the UV-absorbing carrier layer 2, with the dry film thickness of this region controlled to be approximately 15 μm. Subsequently, a second pressure-sensitive adhesive composition with a content of 6 wt% of thermally expandable microspheres 11 is coated to form a thermally responsive region 9 with a high concentration in the middle, with the dry film thickness of this region controlled to be approximately 20 μm. Finally, a third pressure-sensitive adhesive composition with a content of 1 wt% of thermally expandable microspheres 11 is coated to form a second low-concentration region 10 away from the ultraviolet light-absorbing carrier layer 2 and used for bonding the quartz substrate, with the dry film thickness of this region controlled to be approximately 15 μm.
[0108] The coating layers are applied in a semi-dry state, meaning that after the previous pressure-sensitive adhesive composition is coated, it is baked at 60°C for 2 minutes for short-term surface drying to form a stable film shape while still maintaining a certain surface fluidity and tackiness. Then, the next pressure-sensitive adhesive composition is coated, so that there is a certain compositional transition between adjacent areas, rather than forming completely independent three-layer adhesive films. This results in a transparent heat-resistant pressure-sensitive adhesive layer 4 with a total thickness of approximately 50 μm, and the thermally expanded microspheres 11 form a non-uniform distribution structure along the thickness direction of the functional film: a first low-concentration region 8 of 1wt%-6wt%-1wt%, an intermediate high-concentration region 9, and a second low-concentration region 10.
[0109] (6) Thermal curing forms a composite structure After multi-stage coating, the composite film is placed in a 70°C hot air oven for 30 minutes for heat curing. The heat curing temperature is lower than the initial expansion temperature of the thermally expandable microspheres 11 used. During the heat curing process, the ethyl acetate in the pressure-sensitive adhesive composition is volatilized, and the ethyl acetate causes organic solvent limited swelling treatment 15 on the surface of the pre-cured UV-absorbing carrier layer 2, and promotes the migration and diffusion of polymer chain segments on both sides of the interface region, thereby forming a continuous interfacial interpenetration transition region 3, and stabilizing the spatial distribution of the thermally expandable microspheres 11 formed by the three-stage coating. The interfacial interpenetration transition region 3 is formed by the UV-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 during the composite process, and is not an independent film layer formed by separate coating.
[0110] (7) Composite second release protective layer A second PET release film is laminated on the side of the transparent heat-resistant pressure-sensitive adhesive layer 4 away from the ultraviolet light-absorbing carrier layer 2. The second release film 5 is used to protect the surface of the pressure-sensitive adhesive that is finally bonded to the quartz substrate, preventing contamination or unintended adhesion during storage, transportation, and cutting. This forms a composite structure that, from the first side to the second side, includes: a first PET release film (first release film 1) / an ultraviolet light-absorbing carrier layer 2 / an interfacial interpenetration transition region 3 / a transparent heat-resistant pressure-sensitive adhesive layer 4 / a second PET release film (second release film 5).
[0111] (8) Rolling up and cutting The composite functional film obtained in step (7) was placed stably at room temperature for 12 hours, and then wound up using a roll-to-roll method, controlling the winding speed at 2 m / min and maintaining appropriate tension to ensure the film layer was flat and free of obvious wrinkles and bubbles. After winding, it was cut according to the actual usage size using a slitting device, with the cutting speed controlled at 1 m / min, to obtain the UV-absorbing heat-resistant adhesive functional film of this embodiment. Since the interpenetrating transition region 3 is formed by the interpenetration of two adjacent layers rather than an independent film layer, its thickness is not included separately; excluding the release protective layers on both sides, the main body thickness of the functional film in this embodiment is approximately 58 μm, of which the UV-absorbing carrier layer 2 is approximately 8 μm and the transparent heat-resistant adhesive layer 4 is approximately 50 μm. The functional film obtained in this embodiment was used for back lamination of a quartz substrate.
[0112] In actual use, first peel off the second release layer 5 on one side of the transparent heat-resistant pressure-sensitive adhesive layer 4, and then attach the pressure-sensitive adhesive layer to the surface of the quartz substrate; then peel off the first release layer 1 to expose the ultraviolet light-absorbing carrier layer.
[0113] 1. Thermal viscosity reduction properties The peel force between the functional film and the quartz substrate was measured to be 7.2 N / cm without heat treatment.
[0114] The quartz substrate with the functional film attached was then treated at 100°C for 90 seconds.
[0115] After heat treatment, its peel strength was measured to be 1.1 N / cm.
[0116] Compared to before heat treatment, the peel strength decreased by approximately 84.7%.
[0117] After heat treatment, the functional film can be peeled off from the surface of the quartz substrate as a whole. No obvious residual adhesive was observed during the peeling process, and no obvious interlayer separation occurred between the ultraviolet light-absorbing carrier layer and the transparent heat-resistant pressure-sensitive adhesive layer.
[0118] The results show that the functional film of this embodiment can maintain a high adhesion ability at room temperature and achieve a significant reduction in adhesion after short-term heat treatment at 100°C.
[0119] 2. Ultraviolet reflectance The reflectivity of a quartz substrate was tested at a wavelength of 365 nm.
[0120] Without the functional film of this embodiment, the 365nm reflectance of the quartz substrate is 5.3%.
[0121] After the functional film of this embodiment is bonded to the back of the quartz substrate, the 365nm reflectivity is reduced to 0.52%.
[0122] Compared to an uncoated quartz substrate, the reflectivity decreased by approximately 90.2%.
[0123] This embodiment demonstrates that by employing a composite light-absorbing carrier layer composed of benzotriazole UV absorbers and nano-carbon black, the back reflection of the quartz substrate in the 365nm exposure band can be significantly reduced.
[0124] 3. Microsphere distribution and interfacial interpenetration transition zone The cross-sectional morphology of the UV-absorbing thermal anti-adhesion functional film prepared in Example 1 was observed by scanning electron microscopy as follows: Figure 6 As shown in the SEM cross-sectional image, a large number of approximately spherical thermally expanded microspheres 11 are present inside the transparent thermally anti-adhesive pressure-sensitive adhesive layer 4. Along the thickness direction of the functional film, the microsphere distribution is relatively sparse near the ultraviolet light-absorbing carrier layer 2, the microsphere distribution density is significantly increased in the middle region, and the microsphere distribution decreases again near the transparent substrate bonding side, showing an overall spatial distribution characteristic of a first low-concentration region 8 – a middle high-concentration region 9 – a second low-concentration region 10. Figure 7 Cross-sectional SEM observations showed that there was a continuous interface morphology transition region 3 between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4, with a width of approximately 4 μm.
[0125] Table 3 below summarizes the test results of Example 1. The UV-absorbing thermally de-adhesive functional film prepared in this example simultaneously achieves: (1) effective back reflection suppression in the 365nm exposure band; (2) reliable bonding to the quartz substrate at room temperature; (3) significant de-adhesion and overall peeling after heat treatment; (4) effective construction of the thermal expansion microsphere gradient distribution structure; and (5) formation of a stable interface transition structure between the UV-absorbing carrier layer and the transparent thermally de-adhesive pressure-sensitive adhesive layer. Therefore, this example can effectively verify the feasibility of the technical solution of the present invention and its comprehensive technical effects.
[0126] Table 3 Summary of Results from Example 1
[0127] Example 2 The preparation methods of Example 2 and Example 1 are basically the same, except that the addition ratio of benzotriazole UV absorber to nano carbon black in the UV absorber carrier layer 2 is different.
[0128] Specifically, as shown in Table 4, with a total mass of 100 parts by mass of the solid components of the UV-absorbing coating, Example 2 uses the following formulation: Table 4
[0129] In Example 1, the amounts of 2-(5-chloro-2H-benzotriazole-2-yl)-6-(1,1-dimethylethyl)-4-methylphenol and nano-carbon black added were 4 parts and 3 parts, respectively. In this example, the amounts were adjusted to 3 parts and 4 parts, respectively. While maintaining the total amount of the two light-absorbing components at 7 parts, the proportion of black light-absorbing material was increased and the proportion of benzotriazole UV absorbers was reduced accordingly.
[0130] Except for the different formulation of the ultraviolet light-absorbing carrier layer, the first release protective substrate, the thickness of the ultraviolet light-absorbing carrier layer 2, the composition of the acrylic copolymer, the amount of poly(dodecyl acrylate) added, the type of thermally expanding microspheres and their gradient distribution of 1wt%-6wt%-1wt%, the thickness of the transparent heat-reducing pressure-sensitive adhesive layer 4, the thermal curing conditions, and the second release protective layer are all the same as in Example 1.
[0131] Table 5 Performance test results of Example 2
[0132] The performance test results of Example 2 are shown in Table 5. As shown in Table 5, under the quartz substrate bonding condition, the 365nm reflectance of the functional film in this example is 0.68%, which is approximately 87.2% lower than the 5.3% of the quartz substrate without the functional film. The peel force of the functional film before heat treatment was 7.3 N / cm, which decreased to 1.1 N / cm after treatment at 100℃ for 90 s, a decrease of approximately 84.9%. No obvious residual adhesive or interlayer separation was observed after heat treatment, and the functional film could be peeled off the quartz substrate surface as a whole. The results indicate that after adjusting the ratio of benzotriazole UV absorber to nano-carbon black, this example still exhibits good 365nm back reflection suppression capability and thermal de-adhesion performance.
[0133] Example 3 The preparation methods of Example 3 and Example 1 are basically the same, except that the proportion of thermally expanding microspheres added along the thickness direction in the transparent heat-reducing pressure-sensitive adhesive layer is different.
[0134] Specifically, this embodiment still uses the same thermally expandable microspheres 11 as in Example 1, and divides the basic thermally viscous pressure-sensitive adhesive liquid into three parts. Based on the total solid mass of acrylic copolymer and polydodecyl acrylate, different amounts of thermally expandable microspheres 11 are added to form a first pressure-sensitive adhesive composition, a second pressure-sensitive adhesive composition, and a third pressure-sensitive adhesive composition. The formulations are shown in Table 6 below: Table 6
[0135] Using the same multi-stage roller coating method as in Example 1, the above three pressure-sensitive adhesive compositions were sequentially coated onto the surface of the pre-cured ultraviolet light-absorbing carrier layer 2, resulting in a non-uniform distribution structure of the thermally expanding microspheres 11 along the thickness direction of the transparent thermally reducing pressure-sensitive adhesive layer 4: a first low-concentration region 8 (2wt%-8wt%-2wt%), an intermediate high-concentration region 9, and a second low-concentration region 10. The total thickness of the transparent thermally reducing pressure-sensitive adhesive layer 4 in this embodiment remains approximately 50 μm.
[0136] Compared with Example 1, this example increases the amount of thermally expandable microspheres 11 added in the three regions, while maintaining a significantly higher microsphere concentration in the middle region than in the regions near the UV-absorbing carrier layer 2 and the bonding surface of the quartz substrate. This is to examine the adaptability of the low-concentration-high-concentration-low-concentration non-uniform distribution structure to room temperature adhesion, heat treatment de-adhesion, and overall peeling performance when the overall thermal response component content is increased.
[0137] Except for the different addition amount of thermally expanded microspheres 11, the composition and thickness of the first and second release protective layers, the ultraviolet light-absorbing carrier layer, the composition of the acrylic copolymer, the addition amount of poly(dodecyl acrylate), the total thickness of the transparent heat-reducing pressure-sensitive adhesive layer, the interfacial interpenetration structure formation process, and the thermal curing conditions in this embodiment are all the same as in Example 1.
[0138] Example 3 Verification Results The optical and thermal anti-adhesion properties of the UV-absorbing thermal anti-adhesion functional film prepared in Example 3 were tested, and the test results are shown in Table 7.
[0139] Table 7 Performance test results of Example 3
[0140] As shown in Table 7, after attaching the functional film of this embodiment to the back of the quartz substrate, the reflectivity at 365nm wavelength decreased from 5.3% without the functional film to 0.52%, a relative decrease of about 90.2%. This indicates that changing the thermal expansion microsphere gradient content did not have a significant adverse effect on the back reflection suppression performance of the ultraviolet light absorption carrier layer 2.
[0141] In this embodiment, the peel strength of the functional film before heat treatment was 6.3 N / cm, which decreased to 0.9 N / cm after treatment at 100℃ for 90 s, a reduction of approximately 85.7%. No significant residue or interlayer separation was observed after heat treatment, and the functional film could be peeled off entirely from the quartz substrate surface. Compared to the 1wt%-6wt%-1wt% gradient structure of Example 1, this embodiment increased the content of thermally expanded microspheres to 2wt%-8wt%-2wt%. Increasing the content of thermally expanded microspheres further reduced the peel strength of the functional film after heat treatment, while still maintaining whole-film peeling without significant residue or interlayer separation. This indicates that the thermally expanded microsphere distribution structure of the first low-concentration region 8-intermediate high-concentration region 9-second low-concentration region 10 adopted in this invention can achieve effective thermal de-adhesion response within a certain concentration range.
[0142] On the other hand, the peel force before heat treatment in this embodiment decreased from 7.2 N / cm in Example 1 to 6.3 N / cm, indicating that the increase in the amount of thermally expanded microspheres 11 may have a certain impact on the initial adhesion performance of the functional film. Therefore, while taking into account both the room temperature adhesion capability and the anti-adhesion effect after heat treatment, the content of thermally expanded microspheres 11 in different regions can be adjusted according to the actual application requirements.
[0143] Comparative Example 1 The preparation methods of Comparative Example 1 and Example 1 are basically the same, except that the curing state of the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 before they are combined is different.
[0144] Specifically, in Example 1, the UV-absorbing coating is kept in a pre-cured state after the first stage of curing, and then a transparent heat-resistant pressure-sensitive adhesive composition is directly coated on its surface. This allows the organic solvent in the subsequent pressure-sensitive adhesive system to produce limited swelling on the surface of the UV-absorbing carrier layer and promotes the diffusion and entanglement of chain segments in the interface region during the thermal curing process.
[0145] In this comparative example, after the ultraviolet light-absorbing coating is applied to the first PET release film, it is fully cured to form a relatively complete and stable cured structure of the ultraviolet light-absorbing carrier layer. Then, a transparent heat-resistant pressure-sensitive adhesive composition is applied to its surface in the same manner as in Example 1.
[0146] The curing process utilizes a 365nm UV light source with a light intensity of 50mW / cm². 2 The irradiation time was 50 seconds, corresponding to a UV irradiation energy of approximately 2500 mJ / cm². 2 This allows the UV-absorbing coating to reach a fully cured state where the surface has no obvious stickiness and the structure is stable.
[0147] Except for the different curing degree of the ultraviolet light-absorbing carrier layer mentioned above, the composition and thickness of the ultraviolet light-absorbing carrier layer 2, the composition of the acrylic copolymer, the amount of poly(dodecyl acrylate) added, the type of thermally expanding microspheres 11 and their gradient distribution of 1wt%-6wt%-1wt%, the total thickness of the transparent heat-reducing pressure-sensitive adhesive layer, the thermal curing conditions, the first and second release protective layers, and the subsequent winding and cutting processes in this comparative example are all the same as in Example 1.
[0148] This comparative example is used to investigate the changes in interface morphology and interlayer stability between the UV-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 under the conditions of fully cured UV-absorbing carrier layer, limited interface swelling, and suppressed chain segment diffusion, in order to evaluate the role of the interfacial interpenetration transition structure in the overall peel stability of the composite functional membrane.
[0149] The cross-sectional morphology and peel performance of the functional membrane prepared in Comparative Example 1 were observed and tested. The test results are shown in Table 8.
[0150] Table 8 shows the test results of Comparative Example 1.
[0151] Cross-sectional SEM, such as Figure 8 As shown, the observation results indicate that there is a relatively clear interlayer boundary between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4 in Comparative Example 1. Under ×1000 magnification, the cross-sectional morphology of the two materials undergoes a significant abrupt change near the interface. The continuous interface morphology transition region with a width of approximately 4 μm, as seen in Example 1, is not observed. Narrow linear interface dark areas can also be observed in some locations.
[0152] The peel strength of the functional film in Comparative Example 1 before heat treatment was 7.4 N / cm, close to 7.2 N / cm in Example 1, indicating that the full curing of the UV-absorbing carrier layer 2 did not significantly affect the initial adhesion of the functional film to the quartz substrate. However, when peeling was performed after treatment at 100°C for 90 s, significant interlayer separation occurred between the UV-absorbing carrier layer and the transparent heat-resistant pressure-sensitive adhesive layer 4, with some pressure-sensitive adhesive remaining on the surface of the quartz substrate. The functional film could not be peeled off as a whole, thus failing to obtain a comparable full-film peel strength after heat treatment. Compared with Example 1, the main difference between Comparative Example 1 and Example 1 is that the UV-absorbing carrier layer 2 was fully cured before coating the transparent heat-resistant pressure-sensitive adhesive layer 4. Example 1 used a pre-cured carrier layer, which, after subsequent pressure-sensitive adhesive coating and heat curing, formed a continuous interface morphology transition region of approximately 4 μm between the two layers; the functional film could be peeled off as a whole after heat treatment, and no obvious residual adhesive or interlayer separation was observed. Comparative Example 1 did not form the aforementioned obvious continuous morphological transition region and underwent interlayer damage during the peeling process after heat treatment.
[0153] The above results indicate that in the system of the present invention, the use of a pre-cured ultraviolet light-absorbing carrier layer 2 and the formation of a continuous interface transition structure through subsequent limited swelling and thermal curing are beneficial to improving the interlayer bonding stability between the ultraviolet light-absorbing carrier layer 2 and the transparent heat-resistant pressure-sensitive adhesive layer 4. This makes the peeling failure location after heat treatment preferentially occur between the quartz substrate and the pressure-sensitive adhesive layer, thereby reducing the risk of interlayer separation and pressure-sensitive adhesive residue, and facilitating the overall peeling of the functional film.
[0154] Comparative Example 2 The preparation methods of Comparative Example 2 and Example 1 are basically the same, except that the distribution of thermally expanding microspheres 11 along the thickness direction in the transparent thermally de-adhesive pressure-sensitive adhesive layer 4 is different.
[0155] In Example 1, thermally expandable microspheres were added at 1 wt%, 6 wt%, and 1 wt% along the thickness direction of the transparent thermally de-adhesive pressure-sensitive adhesive layer, respectively, corresponding to the first low-concentration region 8 near the ultraviolet light-absorbing carrier layer, the middle high-concentration region 9, and the second low-concentration region 10 near the quartz substrate bonding surface. The dry film thickness of each region was approximately 15 μm, 20 μm, and 15 μm, respectively.
[0156] In this comparative example, the content of thermally expandable microspheres in the three transparent heat-resistant pressure-sensitive adhesive compositions used for three-stage coating was adjusted to 3 wt%, and the dry film thicknesses in each region were maintained at 15 μm, 20 μm, and 15 μm, respectively. The same three-stage roller coating method as in Example 1 was used to coat the adhesives sequentially, resulting in a transparent heat-resistant pressure-sensitive adhesive layer approximately 50 μm thick where the thermally expandable microspheres were distributed substantially uniformly along the thickness direction.
[0157] The nominal thickness-weighted average amount of thermally expandable microspheres added in Example 1 is: (15×1%+20×6%+15×1%) / 50=3wt%.
[0158] Therefore, this comparative example uses a uniform addition method of 3wt% to make it basically consistent with the nominal total addition level of thermally expanded microspheres 11 in Example 1. The main difference is that Example 1 forms a non-uniform distribution structure of the first low concentration region 8 - the intermediate high concentration region 9 - the second low concentration region 10, while this comparative example forms a basically uniform microsphere distribution structure along the thickness direction of the adhesive layer.
[0159] Except for the different spatial distribution of the thermally expanding microspheres 11, the composition and thickness of the ultraviolet light-absorbing carrier layer 2, the pre-curing process, the formation method of the interface transition structure, the composition of the acrylic copolymer, the amount of poly(dodecyl acrylate) added, the type of thermally expanding microspheres, the total thickness of the transparent heat-reducing pressure-sensitive adhesive layer, the thickness of each coating layer, the heat curing conditions, and the first and second release protective layers in this comparative example are all the same as in Example 1.
[0160] This comparative example is used to investigate the effect of the spatial distribution of thermally expanded microspheres 11 along the thickness direction of the adhesive layer on the initial adhesion performance, heat treatment de-tack performance, peel interface state, and overall peel performance of the functional film under the condition that the total addition level of thermally expanded microspheres 11 is basically the same.
[0161] The optical properties and thermal de-adhesion properties of the functional film prepared in Comparative Example 2 were tested, and the results are shown in Table 9.
[0162] Table 9 Performance test results of Comparative Example 2
[0163] As shown in Table 9, the reflectance of the functional film in Comparative Example 2 at a wavelength of 365 nm is 0.57%, which is about 89.2% lower than that of the quartz substrate without the functional film. This indicates that the change in the spatial distribution of the thermally expanded microspheres 11 did not significantly affect the back reflection suppression effect of the ultraviolet light-absorbing carrier layer 2.
[0164] Under quartz substrate bonding conditions, the peel force of Comparative Example 2 before heat treatment was 5.1 N / cm; after treatment at 100℃ for 90 s, the peel force decreased to 1 N / cm, a decrease of approximately 80.4%, indicating that the use of 3 wt% uniformly distributed thermally expanded microspheres 11 can still produce a significant thermal de-adhesion response. No obvious adhesive residue was observed after heat treatment, but slight interlayer separation occurred during the peeling process. The functional film could be peeled off almost entirely, but the peeling integrity was significantly lower than that of Example 1.
[0165] Comparative Example 2 and Example 1 had essentially the same nominal total addition level of thermally expanded microspheres. Example 1 used a low-concentration-high-concentration-low-concentration distribution structure of 1wt%-6wt%-1wt%, with a peel force of 7.2 N / cm before heat treatment and 1.1 N / cm after treatment at 100°C for 90 s, a decrease of approximately 84.7%, and no obvious residual adhesive or interlayer separation was observed after heat treatment, achieving whole-film peeling; Comparative Example 2 used a 3wt% uniform distribution, and the peel force before heat treatment decreased to 5.1 N / cm, while slight interlayer separation occurred after heat treatment.
[0166] The above results indicate that, under the condition that the total addition level of thermally expandable microspheres 11 is basically consistent, their spatial distribution along the thickness direction of the pressure-sensitive adhesive layer affects the initial adhesion performance of the functional film and the structural integrity after heat treatment. Reducing the content of microspheres near the quartz substrate bonding surface is beneficial to maintaining effective adhesion at the bonding interface; reducing the content of microspheres near the UV-absorbing carrier layer is beneficial to reducing local deformation and stress concentration near the interface during thermal expansion; at the same time, concentrating a higher concentration of thermally expandable microspheres in the middle of the adhesive layer can still provide effective thermal response.
[0167] Therefore, compared with a uniform distribution at the same nominal total addition level, the low-concentration-high-concentration-low-concentration thermal expansion microsphere distribution structure adopted in this invention can better balance room temperature adhesion ability and the integrity of the composite structure after heat treatment while maintaining an effective thermal de-adhesion response.
[0168] Numerous specific details are set forth in this specification. However, it will be understood that embodiments of the invention may be practiced without these specific details. In some embodiments, well-known methods, structures, and techniques have not been shown in detail so as not to obscure the understanding of this specification.
[0169] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.
[0170] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.
[0171] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Any simple modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention shall still fall within the scope of the technical solution of the present invention.
Claims
1. A UV-absorbing thermally de-adhesive functional film with an interface transition structure, characterized in that, It includes an ultraviolet light-absorbing carrier layer and a transparent heat-resistant pressure-sensitive adhesive layer disposed on one side of the ultraviolet light-absorbing carrier layer; The ultraviolet light-absorbing support layer comprises a UV-curable acrylic resin matrix, a benzotriazole ultraviolet absorber, and a black light-absorbing material; The transparent heat-resistant pressure-sensitive adhesive layer comprises an acrylic copolymer, poly(docosahexamethicone) and thermally expandable microspheres. A continuous interfacial interpenetration transition region is provided between the ultraviolet light-absorbing carrier layer and the transparent heat-resistant pressure-sensitive adhesive layer. The continuous interfacial interpenetration transition region is formed by the mutual penetration of the UV-cured acrylic resin matrix and the acrylic copolymer at the interface. Along the thickness direction of the transparent heat-resistant pressure-sensitive adhesive layer, the concentration of the thermally expanded microspheres in the middle region is higher than that in the region near the ultraviolet light-absorbing carrier layer and the region near the substrate bonding side, exhibiting a non-uniform distribution with low concentrations on both sides and high concentrations in the middle.
2. The ultraviolet light-absorbing thermal anti-adhesion functional film according to claim 1, characterized in that, The thickness of the ultraviolet light-absorbing support layer is 3–15 μm; Based on a total solid component mass of 100 parts by mass of the ultraviolet light-absorbing support layer, the ultraviolet light-absorbing support layer comprises: 70-82 parts by weight of UV-curable acrylic resin; 10-18 parts by weight of reactive diluent; 2-5 parts by weight of benzotriazole UV absorber; 2-5 parts by weight of black light-absorbing material; Photoinitiator 1.5–3 parts by weight; Dispersant 0.5 to 1.5 parts by weight.
3. The ultraviolet light-absorbing thermal anti-adhesion functional film according to claim 1, characterized in that, The black light-absorbing material is carbon black; The acrylic copolymer is obtained by polymerization of a monomer composition comprising isooctyl acrylate, lauryl acrylate, methyl methacrylate and acrylamide; Based on a total mass of 100 parts by mass of monomer composition, isooctyl acrylate comprises 40-70 parts by mass, lauryl acrylate comprises 5-25 parts by mass, methyl methacrylate comprises 10-35 parts by mass, and acrylamide comprises 0.5-10 parts by mass. Based on 100 parts by weight of the solids of the acrylic copolymer, the amount of poly(2-diethyl acrylate) added is 3 to 15 parts by weight, and it is dispersed in the transparent heat-resistant pressure-sensitive adhesive layer by physical blending.
4. The ultraviolet light-absorbing thermal anti-adhesion functional film according to claim 1, characterized in that, The transparent heat-resistant pressure-sensitive adhesive layer is divided into a first low-concentration region, an intermediate high-concentration region, and a second low-concentration region along its thickness direction. The thermal expansion microsphere content in the first low concentration region and the second low concentration region is based on the total solid mass of acrylic copolymer and poly(2-diethyl acrylate) in the corresponding region, and is 0.5 to 2 wt% respectively. The thermal expansion microsphere content in the intermediate high concentration region is based on the total solid mass of acrylic copolymer and poly(2-diethyl acrylate) in the corresponding region, and is 4 to 8 wt%.
5. The ultraviolet light-absorbing thermal anti-adhesion functional film according to claim 4, characterized in that, The thermal expansion microsphere content of the first low concentration region, the intermediate high concentration region and the second low concentration region are 1wt%, 6wt% and 1wt% respectively, based on the total solid mass of acrylic copolymer and poly(2-diethyl acrylate) in the corresponding regions, and the thickness of the corresponding regions is 15μm, 20μm and 15μm respectively.
6. The ultraviolet light-absorbing thermal anti-adhesion functional film according to any one of claims 1 to 5, characterized in that, It also includes a first release protective layer and a second release protective layer; the first release protective layer is disposed on the side of the ultraviolet light-absorbing carrier layer away from the transparent heat-resistant pressure-sensitive adhesive layer, and the second release protective layer is disposed on the side of the transparent heat-resistant pressure-sensitive adhesive layer away from the ultraviolet light-absorbing carrier layer. Both the first release protective layer and the second release protective layer are removable protective layers.
7. A method for preparing the ultraviolet light-absorbing thermal anti-adhesion functional film according to any one of claims 1 to 6, characterized in that, Includes the following steps: (1) Provide a first release protective substrate; (2) A UV-curable acrylic resin, a benzotriazole UV absorber, a black light-absorbing material and a photoinitiator are mixed to obtain a UV-absorbing coating composition; (3) The ultraviolet light-absorbing coating composition is coated on the surface of the first release protective substrate and UV curing is performed in the first stage to obtain a pre-cured ultraviolet light-absorbing carrier layer that maintains the complete film shape and has the ability to be swollen by organic solvents. (4) The acrylic copolymer was physically blended with poly(2-diethyl acrylate), and organic solvent and thermally expandable microspheres with different contents were added to prepare multiple transparent heat-reducing pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres. (5) Transparent thermally resistant pressure-sensitive adhesive compositions with different contents of thermally expandable microspheres are sequentially coated onto the surface of the pre-cured ultraviolet light-absorbing carrier layer; when the first layer of pressure-sensitive adhesive composition is coated, the organic solvent contained therein causes limited swelling on the surface of the pre-cured ultraviolet light-absorbing carrier layer; by sequentially coating compositions with different contents of microspheres, the thermally expandable microspheres are uniformly distributed along the thickness direction of the formed transparent thermally resistant pressure-sensitive adhesive layer, with low concentration on both sides and high concentration in the middle; (6) Thermal curing is carried out under conditions lower than the initial expansion temperature of the thermal expansion microspheres to evaporate the organic solvent and form a continuous interfacial interpenetration transition region at the interface between the ultraviolet light-absorbing carrier layer and the transparent thermally reducing pressure-sensitive adhesive layer, while stabilizing the spatial distribution of the thermal expansion microspheres along the thickness direction of the transparent thermally reducing pressure-sensitive adhesive layer. (7) A second release protective layer is laminated on the side of the transparent heat-resistant pressure-sensitive adhesive layer away from the ultraviolet light-absorbing carrier layer; (8) Roll up and cut to obtain the ultraviolet light-absorbing heat-reducing functional film.
8. The preparation method according to claim 7, characterized in that, In step (5), transparent heat-reducing pressure-sensitive adhesive compositions with low thermal expansion microsphere content, high thermal expansion microsphere content, and low thermal expansion microsphere content are coated sequentially, with the thermal expansion microsphere content in the corresponding regions being 0.5-2 wt%, 4-8 wt%, and 0.5-2 wt%, respectively.
9. The preparation method according to claim 7 or 8, characterized in that, The organic solvent includes ethyl acetate; the thermal curing temperature is 50–80°C, the thermal curing time is 10–60 min, and the thermal curing temperature is lower than the initial expansion temperature of the thermally expanding microspheres.
10. A method for suppressing back reflection during ultraviolet exposure of the front side of a transparent substrate, characterized in that, Using the ultraviolet light-absorbing thermal anti-adhesion functional film according to any one of claims 1 to 6, the following steps are included: S1. The second release protective layer for peeling off the functional film is used to attach a transparent heat-resistant pressure-sensitive adhesive layer to the back of a transparent substrate with photoresist on the front side. S2. Peel off the first release protective layer. The ultraviolet light-absorbing carrier layer is on the outside. Ultraviolet exposure is performed from the front of the transparent substrate. The ultraviolet light-absorbing carrier layer suppresses back reflection caused by exposure. S3. After exposure, heat treatment is performed to reduce the peeling force of the transparent heat-resistant pressure-sensitive adhesive layer, and then the functional film is peeled off from the surface of the transparent substrate.