A high and low temperature resistant hot melt adhesive, its preparation method and application

By using blended coupling type SIS and SESBS hot melt adhesives, combined with specific additives, the sealing problem of refrigerator VIP panels under extreme temperatures was solved, achieving high efficiency in low-temperature toughness and high-temperature creep resistance, and reducing processing energy consumption.

CN123107592APending Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202510618503.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2025-05-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing hot melt adhesives cannot simultaneously meet the requirements of low-temperature toughness and high-temperature creep resistance in the application of refrigerator VIP panels, resulting in poor sealing performance, high processing viscosity, and high energy consumption.

Method used

A star-shaped structure is formed by using a coupled SIS and SESBS blend hot melt adhesive, combined with naphthenic oil, tackifying resin, crosslinking agent and antioxidant, which improves low temperature flexibility and high temperature stability, reduces melt viscosity and enhances bonding performance.

Benefits of technology

It achieves high peel strength and long-term adhesion in the range of -18℃ to 50℃, reduces processing energy consumption, and improves production efficiency and sealing performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a high- and low-temperature resistant hot melt adhesive, its preparation method, and its applications, belonging to the field of polymer composite materials. The high- and low-temperature resistant hot melt adhesive mainly comprises coupled polystyrene-isoprene-styrene block copolymers and polystyrene-(ethylene-styrene-butene)-styrene block copolymers, as well as filler oils, tackifying resins, crosslinking agents, antioxidants, and other components. It exhibits good high- and low-temperature resistance and is particularly suitable for core material composites in refrigerator vacuum insulation panels or for long-term edge sealing of vacuum insulation panels.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a hot melt adhesive, particularly to a styrene-isoprene-styrene block copolymer (SIS) and a styrene-(ethylene-styrene-butene)-styrene copolymer (SESBS) blended hot melt adhesive modified by dynamic vulcanization, and also to its preparation method, as well as to the application of a high and low temperature resistant hot melt adhesive in the composite of refrigerator vacuum insulation panel core material or in the sealing of vacuum insulation panel edges, belonging to the field of polymer composite material technology. Background Technology

[0002] VIP panels (vacuum insulation panels) for refrigerators demonstrate unique application value in multiple fields due to their ultra-thin structure and high-efficiency thermal insulation performance. In household refrigerators, they increase internal volume by reducing the thickness of the insulation layer while maintaining a more stable low-temperature environment, making them particularly suitable for high-end energy-saving refrigerator designs. During refrigerator manufacturing, to achieve an aesthetically pleasing effect, VIP panels are not directly exposed but are bonded to metal materials such as side panels and back panels using hot melt adhesive. Because the internal temperature of refrigerators is low, the hot melt adhesive used for bonding must have low-temperature resistance to ensure long-term bonding. Domestic refrigerators exported overseas are generally shipped via container shipping, where temperatures can reach over 50°C; therefore, the hot melt adhesive used for bonding also needs to have certain high-temperature resistance.

[0003] Existing technologies have the following drawbacks: traditional EVA-based hot melt adhesives exhibit high low-temperature brittleness, with peel strength decreasing by more than 60% at -20℃; polyolefin-based hot melt adhesives have poor permeability to porous core materials, and the adhesive layer is prone to creep in high-temperature environments, leading to VIP board deformation or decreased tack, adhesive layer detachment, and loss of sealing effect. Chinese patent (publication number: CN106867429B) relates to a low-temperature resistant hot melt adhesive and its preparation method, using butyl rubber as the main component. The adhesive sheet has good flexibility, ensuring that the heat shrink tape does not crack during unwinding even at -30℃, thus ensuring the feasibility of construction in cold regions. Furthermore, the preparation method is simple and low-cost, and the resulting low-temperature resistant hot melt adhesive exhibits excellent performance; however, its high-temperature resistance has not been evaluated. Chinese patent (publication number: CN117844416A) discloses a high-temperature resistant, high-tack hot melt adhesive for tapes and its preparation method. Using SIS and SEBS as base materials, the prepared hot melt adhesive is less prone to overflow and exhibits high softening point, high temperature resistance, high bonding strength, and high holding power. However, its viscosity is high, reaching nearly 30,000 cps at 200°C, leading to increased energy consumption during application and hindering energy conservation. Furthermore, SIS can age within 1-2 hours at high temperatures, affecting the quality and bonding performance of the hot melt adhesive. Therefore, there is an urgent need to develop a hot melt adhesive that combines low-temperature toughness, high-temperature creep resistance, and low processing viscosity to adapt to the extreme working conditions of refrigerator VIP panels. Summary of the Invention

[0004] To address the issue that existing hot melt adhesives cannot meet the requirements for bonding refrigerator VIP panels:

[0005] The first objective of this invention is to provide a hot melt adhesive resistant to high and low temperatures, which can meet the requirements of refrigerator VIP panels in applications requiring resistance to high and low temperatures (-18℃~50℃). In everyday household use, it remains non-brittle at low temperatures, with a steel sheet peel strength (-18℃) > 20 N / inch at a coating strength of 70 g / m². For export by sea, it maintains high-temperature peel strength and long-term adhesion, with a high-temperature peel strength (50℃) > 30 N / inch, a high-temperature holding time (1000 g / inch, 50℃) > 24 h, a room-temperature peel strength > 43 N / inch, and a softening point > 100℃, exhibiting excellent adhesion.

[0006] The second objective of this invention is to provide a method for preparing a high- and low-temperature resistant hot melt adhesive, which is simple, low-cost, and meets the requirements of industrial production.

[0007] The third objective of this invention is to provide an application of a high- and low-temperature resistant hot melt adhesive for use in the composite of core materials of refrigerator vacuum insulation panels or for sealing the edges of vacuum insulation panels (with the side or back panel), meeting the high and low temperature (-18℃~50℃) application scenarios for daily household use and marine export.

[0008] To achieve the above-mentioned technical objectives, the present invention provides a hot melt adhesive resistant to high and low temperatures, comprising the following components by weight percentage: 5-10% coupled polystyrene-isoprene-styrene block copolymer; 5-10% polystyrene-(ethylene-styrene-butene)-styrene block copolymer; 20-40% filler oil; 30-60% tackifying resin; 0.4-0.8% crosslinking agent; and 0.5-1% antioxidant. The melt index of the coupled polystyrene-isoprene-styrene block copolymer is 15-30 g / 10 min. (200℃,5kg) The styrene unit content is 15-25% by mass; the polystyrene-isoprene diblock copolymer accounts for 70-80% by mass in the coupled polystyrene-isoprene-styrene block copolymer; the melt index of the polystyrene-(ethylene-styrene-butene)-styrene block copolymer is 5-30 g / 10 min. (200℃,5kg) It contains 15-50% styrene units by mass, and the styrene units in the intermediate polyethylene-styrene-butene block account for 20-60% of the total styrene units in the copolymer.

[0009] The key components of the high and low temperature resistant hot melt adhesive of this invention are coupled SIS (styrene-isoprene-styrene triblock copolymer) and SESBS (styrene-(ethylene-styrene-butene)-styrene block copolymer). The combination of these two components imparts low-temperature flexibility, high-temperature peel strength, and long-term tack to the hot melt adhesive. More specifically, the coupled SIS has a star-shaped radial branched molecular structure and contains a high proportion of uncoupled styrene-isoprene diblock structures, resulting in significant performance advantages: 1) Low melt viscosity and excellent processing performance: The star-shaped radial branches of the coupled SIS are more easily unentangled in the molten state, resulting in stronger melt flow and a significantly lower melt viscosity than linear SIS. This allows for processing at lower temperatures (e.g., 120~150℃), reducing energy consumption and the risk of material thermal degradation due to high temperatures, thus improving production efficiency. 2) High cohesive strength and mechanical properties; for example, enhanced physical cross-linking: the star-shaped molecular chains form more physical cross-linking points (aggregation of styrene hard segments), giving the hot melt adhesive higher tensile strength, elasticity, and creep resistance; also, excellent peel resistance: it is not easy to crack under dynamic stress (such as repeated bending) or long-term load, making it suitable for durable applications such as shoe materials and automotive sealing strips. 3) Wide temperature range adaptability; high temperature stability: the hard segment has a higher glass transition temperature (Tg), which increases the softening point of the hot melt adhesive at high temperatures, reducing adhesion problems during summer storage or transportation; low temperature toughness: the isoprene soft segment maintains flexibility, allowing the adhesive to remain elastic at low temperatures (such as -30℃), avoiding brittleness (such as in frozen packaging applications). 4) Excellent adhesion performance; strong initial tack: quickly wets the substrate surface (such as low surface energy materials such as PE and PP), shortening the bonding and pressing time and improving production line efficiency; long-lasting tack: high long-term adhesion stability, especially suitable for applications that need to withstand continuous loads (such as building joint sealing). In summary, this invention selects a coupled star-shaped SIS, which improves high-temperature resistance. Furthermore, because it contains a diblock copolymer, it enhances both viscosity and low-temperature performance. Additionally, its high melt index significantly improves processing fluidity. Linear SESBS, through hydrogenation, converts unsaturated double bonds into a saturated structure, significantly improving its resistance to oxidation and thermal degradation, allowing for long-term use at temperatures up to 100-120°C (higher than SIS's 80-100°C). In high-temperature environments, the hot melt adhesive does not easily soften or flow, maintaining bond strength. The soft segment (ethylene-styrene-butene) remains flexible at -40°C, preventing low-temperature brittleness (e.g., in frozen logistics packaging). However, SESBS has a high melt viscosity and poor fluidity; even at low molecular weights, it is difficult to achieve high fluidity at processing temperatures above 160°C, limiting its widespread application in the hot melt adhesive field. It is well known in the industry that by adding a portion of styrene units to the middle of the soft segment (EB) to form an ethylene-styrene-butene soft segment, its fluidity can be significantly improved, which can greatly broaden the application range of SESBS in the field of hot melt adhesives.In summary, the present invention introduces SESBS into hot melt adhesives to improve the temperature resistance and aging resistance of hot melt adhesives while satisfying processability requirements.

[0010] The coupled polystyrene-isoprene-styrene block copolymer of the present invention is obtained by coupling a polystyrene-isoprene diblock copolymer with a coupling agent having three or more active functional groups. Common coupling agents with three or more active functional groups include trichlorosilane, tetrachlorosilane, etc., which are common coupling agents in the industry, and can respectively obtain coupled polystyrene-isoprene-styrene block copolymers with three or four arms, exhibiting a star-shaped structure.

[0011] As a preferred embodiment, the melt index of the coupled polystyrene-isoprene-styrene block copolymer is 15~25 g / 10 min. (200℃,5kg) The styrene-isoprene-styrene block copolymer contains 18-22% styrene units by mass; the polystyrene-isoprene diblock copolymer accounts for 70-75% of the total mass of the coupled polystyrene-isoprene block copolymer. Preferred coupled polystyrene-isoprene-styrene block copolymers include, for example, the commercially available YH-4016 (styrene unit content 18-20%, diblock content 70-75%, melt index 19-24 g / 10 min), or the commercially available YH-4018 (styrene unit content 20-22%, diblock content 70-75%, melt index 16-24 g / 10 min). These preferred coupled polystyrene-isoprene-styrene block copolymers are characterized by low styrene content, high diblock content, and high melt index, giving the hot melt adhesive good flexibility and excellent low-temperature resistance.

[0012] As a preferred embodiment, the melt index of the polystyrene-(ethylene-styrene-butene)-styrene block copolymer is 10~20 g / 10 min. (200℃,5kg)The styrene content of the polystyrene-(ethylene-styrene-butene)-styrene block copolymer is 25-45%. Preferred options include commercially available YH-530 (styrene content 30-32%, with styrene units in the soft segments accounting for 33-35% of the total styrene content in the copolymer, melt index: 10-20 g / 10 min) or commercially available YH-516 (styrene content 40-43%, with styrene units in the soft segments accounting for 48-50% of the total styrene content in the copolymer, melt index: 10-20 g / 10 min). Preferred SESBS has a high styrene content, a high melt index, and is free of unsaturated double bonds. Its long-term operating temperature is 100-120°C, giving the hot melt adhesive excellent high-temperature resistance. After introducing a crosslinking agent for micro-crosslinking, a reversible three-dimensional network is formed, further enhancing the hot melt adhesive's high-temperature resistance and creep resistance.

[0013] As a preferred embodiment, the filler oil comprises naphthenic oil and / or white oil. A further preferred naphthenic oil is 4010, and a further preferred white oil is 36#. It is well known in the industry that naphthenic oil and white oil act as plasticizers and softeners in the preparation of hot melt adhesives, playing a crucial role in adjusting colloidal viscosity, improving processing fluidity, enhancing low-temperature performance, and optimizing costs. The cyclic structure of naphthenic oil has better compatibility with highly polar SBS and SIS, reducing the risk of oil precipitation, making it particularly suitable for coupled SIS-based hot melt adhesives. Furthermore, its outstanding low-temperature performance, with a low pour point (below -30°C), imparts excellent low-temperature flexibility to the hot melt adhesive, making it suitable for applications such as cold chain packaging. White oil, with its straight-chain alkane structure, can effectively reduce melt viscosity, but its compatibility is only good in non-polar systems, i.e., it has good compatibility with SESBS.

[0014] As a preferred option, the tackifying resin is a petroleum resin. Petroleum resins include C5 petroleum resin, C9 petroleum resin, hydrogenated C5, hydrogenated C9 petroleum resin, terpene resin, rosin resin, hydrogenated rosin resin, etc. The performance of hot melt adhesives is highly dependent on their resin composition. Tackifying resins mainly provide adhesion, hardness, temperature resistance, and compatibility with the substrate. The advantages of C5 petroleum resin are: low cost, good processing fluidity, and better aging resistance than rosin resin; the disadvantages are: moderate high-temperature resistance and poor adhesion to polar materials. The advantages of C9 petroleum resin are high bonding strength, suitable for high-load applications; the disadvantages are: dark color, prone to yellowing, and poor compatibility with polar materials. Hydrogenated C5 or hydrogenated C9 petroleum resins have very light color, are compatible with polar / non-polar elastomers, and have good temperature resistance; the disadvantage is that they are relatively expensive. Terpene resins are bio-based, biodegradable, and environmentally friendly; the disadvantages are poor temperature resistance and high price. Taking all factors into consideration, as a preferred option, the present invention selects hydrogenated C5 or C9 resin.

[0015] As a preferred embodiment, the crosslinking agent includes at least one of dicumyl peroxide, di-tert-butyl cumyl peroxide, and di-tert-butyl peroxide. In hot melt adhesives, the crosslinking agent induces the formation of chemical bonds (covalent or ionic bonds) between polymer molecular chains, transforming linear or branched structures into three-dimensional network structures. This promotes the formation of stable crosslinking points between polymer chains (such as SBS and SESBS), significantly improving the cohesive strength of the adhesive and reducing molecular chain slippage under stress. This, in turn, significantly enhances the physicochemical properties of the hot melt adhesive, strengthening its cohesive strength and durability. Furthermore, the crosslinking network restricts molecular chain movement, increasing the softening point of the hot melt adhesive and preventing surface softening that could lead to bonding failure. Crosslinking agents used for SBS and SESBS include DCP (dicumyl peroxide), BIPB (di-tert-butyl cumyl peroxide), and DTBP (di-tert-butyl peroxide). DCP has a decomposition temperature of approximately 170°C, BIPB has a higher decomposition temperature (approximately 175°C to 185°C), and DTPB has an even higher decomposition temperature, making it suitable for high-temperature processing. Considering that the melt temperature of the present invention is around 175°C, DCP is preferred as the crosslinking agent.

[0016] As a preferred embodiment, the antioxidant comprises 1076 and / or 168. To prevent the hot melt adhesive from oxidizing and deteriorating at high temperatures, thus compromising the bond strength, a certain amount of antioxidant needs to be added. The present invention preferably uses a combination of 1076 and 168.

[0017] This invention also provides a method for preparing a high- and low-temperature resistant hot melt adhesive. The method involves preheating the filler oil, then adding a coupled polystyrene-isoprene-styrene block copolymer and a polystyrene-(ethylene-styrene-butene)-styrene block copolymer and stirring until completely dissolved. Next, a tackifying resin is added and stirring is continued until the system becomes transparent. Then, a crosslinking agent is added to carry out a crosslinking reaction. Finally, an antioxidant is added and stirred evenly before being discharged and cooled.

[0018] The present invention also provides an application of a high and low temperature resistant hot melt adhesive, which is used for the composite of the core material of a refrigerator vacuum insulation panel, or for the edge sealing of a refrigerator vacuum insulation panel.

[0019] The present invention also provides a method for preparing a hot melt adhesive resistant to high and low temperatures: (1) Premixing stage: Under nitrogen protection, the filler oil is heated to 150°C; (2) Melt blending: SIS and SESBS are added in sequence and stirred at 500 rpm until completely melted (about 30 min); (3) Resin dispersion: Resin is added, the temperature is raised to 170°C, and stirring is continued until the system is transparent (about 1 h); (4) Dynamic crosslinking: The temperature is raised to 175°C, a crosslinking agent is added, and the crosslinking reaction is completed after maintaining for 10 min; (5) Stabilization treatment: Antioxidant is added, and the material is discharged and cooled after stirring for 5 min.

[0020] Compared with existing technologies, the advantages of the technical solution of this invention are as follows:

[0021] The high and low temperature resistant hot melt adhesive of this invention uses coupled SIS and SESBS as the base material. The star-shaped SIS exhibits better high-temperature resistance compared to the linear SIS. The SIS used in this invention features low styrene content, a high proportion of diblock segments, and a high melt index. The low styrene content of the SIS imparts good flexibility to the hot melt adhesive, giving it excellent low-temperature resistance. Simultaneously, the flexibility of the soft segments enhances low-temperature resistance, ensuring it remains non-brittle at low temperatures. The viscosity range at 190°C is 5000±1500 mPa·s, but with a 70 g / m² coating, the peel strength of the steel sheet (-18°C) is >20 N / inch. Furthermore, the high styrene content and high melt index of the SESBS, which does not contain unsaturated double bonds, allows for long-term use at 100~120°C, giving the hot melt adhesive excellent high-temperature resistance. The introduction of a crosslinking agent for micro-crosslinking forms a reversible three-dimensional network, further improving the hot melt adhesive's high-temperature resistance and creep resistance. During sea transport, it can maintain peel strength at high temperatures and long-term adhesion. High temperature peel strength (50℃) > 30N / inch, high temperature adhesion time (1000g / inch, 50℃) > 24h, room temperature peel strength > 43N / inch, softening point > 100℃, and has good adhesion. Detailed Implementation

[0022] To facilitate understanding of the present invention, the present invention will be described more fully and in detail below with reference to preferred embodiments, but the scope of protection of the present invention is not limited to the following specific embodiments.

[0023] Unless otherwise defined, all technical terms used herein have the same meaning as commonly understood by those skilled in the art. The technical terms used herein are for the purpose of describing particular embodiments only and are not intended to limit the scope of the invention.

[0024] In the following embodiments, unless otherwise specified, all raw materials, reagents, instruments and equipment used in this invention can be purchased from the market or prepared by existing methods.

[0025] Peel strength: according to GB / T2790-1995 standard.

[0026] Low temperature test: Heat the hot melt adhesive to 175℃, pour it out, let it flow naturally into the test steel plate, place it in a refrigerator at -18℃ for 24 hours, take it out, and place it parallel to a height of 1.5 meters for free drop, repeat three times, and observe whether the adhesive is brittle.

[0027] High temperature test: Heat the hot melt adhesive to 175℃, pour it out, let it flow naturally into the test steel plate, place it in an 80℃ oven for 12 hours, and observe whether it shifts or tilts.

[0028] Viscosity: Measured using a Borelfeld viscometer.

[0029] Holding time: Tested according to ASTM D3654 standard.

[0030] Softening point test: Globe and ring method.

[0031] Unless otherwise specified, the chemical reagents and raw materials used in the following specific embodiments are all conventional commercially available materials.

[0032] The present invention will be further described in detail below through specific examples:

[0033] Preparation method of hot melt adhesive: (1) Premixing stage: Under nitrogen protection, heat the filler oil to 150°C; (2) Melt blending: Add SIS and SESBS in sequence, and stir at 500 rpm until completely melted (about 30 min); (3) Tackifying resin dispersion: Add tackifying resin, heat to 170°C, and continue stirring until the system is transparent (about 1 h); (4) Dynamic crosslinking: Heat to 175°C, add crosslinking agent, and maintain for 10 min to complete the crosslinking reaction; (5) Stabilization treatment: Add antioxidant 1076+168 (1:1), stir for 5 min, and then discharge and cool.

[0034] The formulations of high and low temperature resistant hot melt adhesives are shown in Table 1:

[0035]

[0036]

[0037] Notes: (1) Examples 1 and 2 use coupled star-shaped SIS, SIS-4016 and SIS-4018 alone, and compare the differences between the two. (2) Examples 3 and 4 use SESBS, YH-530 and YH-516 alone, and compare the differences between the two. (3) Examples 5 and 6 use a mixed formulation of coupled star-shaped SIS and SESBS (1:1). Example 5 uses YH-530 and SIS-4016, and Example 6 uses YH-516 and SIS-4018. Compare the differences between the two. (4) Example 7 changes the naphthenic oil in Example 6 to white oil and compare the differences between the two. (5) Example 8 changes the hydrogenated C9 petroleum resin in Example 7 to hydrogenated C5 petroleum resin and compare the differences between the two. (6) Example 9 increases the crosslinking agent content in Example 7 from 0.4 to 1.0 and compares the differences between the two. (7) Example 10 reduced SIS-4018 from 10 parts to 5 parts and YH-516 from 10 parts to 15 parts in Example 7, comparing the performance differences between the two. (8) Example 11 increased YH-4018 from 10 parts to 15 parts and reduced YH-516 from 10 parts to 5 parts in Example 7, comparing the differences between the two. (8) Example 12 increased the antioxidant from 0.5 parts to 1 part in Example 7, comparing the differences between the two. The test results are shown in Table 2:

[0038]

[0039] Comparing Examples 1 and 2, the coupled star-shaped SIS alone did not crack at low temperatures, but tilted at high temperatures. While the low-temperature peel strength met requirements, the peel strength at both room temperature and high temperatures was low. The softening point, viscosity, and high-temperature holding time were also low, failing to meet the requirements. The experiments show that YH-4018 exhibits higher peel strength, softening point, and holding time than YH-4016, and also has lower viscosity.

[0040] Comparing Examples 3 and 4, SESBS alone did not crack at low temperatures or tilt at high temperatures, and its low-temperature peel strength was below 20 N / inch. However, it exhibited higher peel strength and softening point at both room and high temperatures, and its viscosity exceeded the specifications. The high-temperature holding time was improved compared to using star-shaped SIS alone, but still <24 hours, failing to meet the requirements. The test results show that YH-516 has higher peel strength, softening point, and holding time than YH-530, and also has lower viscosity.

[0041] Comparing Examples 5 and 6, the novel SIS and SESBS blend formulation showed no brittleness at low temperatures, no tilting at high temperatures, a low-temperature peel strength >20 N / inch, a room-temperature peel strength >43 N / inch, a softening point >100°C, and a viscosity within 5000 ± 1500 mPa·s, meeting all requirements. The test results show that YH-4018 / YH-516 exhibits higher peel strength, softening point, and holding time, and lower viscosity than YH-4016 / YH-530.

[0042] Comparing Examples 6 and 7, replacing the naphthenic oil with white oil resulted in essentially the same low-temperature and high-temperature tests and low-temperature peel strength, but the high-temperature peel strength and softening point increased significantly. This is mainly because white oil has better compatibility with SESBS, which makes the high-temperature performance of SESBS stand out. The viscosity and holding time are slightly lower, but they basically meet the requirements.

[0043] Comparing Examples 7 and 8, replacing C9 hydrogenated petroleum resin with C5 hydrogenated petroleum resin resulted in varying degrees of decline in all properties, but all remained within the acceptable range.

[0044] Compared with Example 7 and Example 9, increasing the crosslinking agent from 0.4 parts to 1.0 parts resulted in a slight decrease in low-temperature peel strength, while the high-temperature peel strength, softening point, viscosity, and holding time all increased significantly.

[0045] Comparing Example 7 and Example 10, the amount of SIS-4018 in Example 7 was reduced from 10 parts to 5 parts, and the amount of YH-516 was increased from 10 parts to 15 parts. The low-temperature peel strength was reduced, while the high-temperature peel strength, softening point, viscosity and holding time were significantly improved, but all were within the specified range.

[0046] Comparing Example 7 and Example 11, the amount of SIS-4018 in Example 7 was increased from 10 parts to 15 parts, and the amount of YH-516 was reduced from 10 parts to 5 parts. The low-temperature peel strength was improved, while the high-temperature peel strength, softening point, viscosity and holding time were significantly reduced, but all were within the specified range.

[0047] Comparing Example 7 and Example 12, increasing the antioxidant from 0.5 parts to 1 part did not significantly alter the performance of the samples.

[0048] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A high and low temperature resistant hot melt adhesive, characterized in that: The raw materials include the following components by weight percentage: Coupled polystyrene-isoprene-styrene block copolymer 5~10%; 5-10% polystyrene-(ethylene-styrene-butene)-styrene block copolymer; Filler oil 20~40%; Tackifying resin 30-60%; Crosslinking agent 0.4~0.8%; Antioxidant 0.5-1%; The melt index of the coupled polystyrene-isoprene-styrene block copolymer is 15~30 g / 10min. (200℃,5kg) It contains 15-25% styrene units by mass; The mass percentage of polystyrene-isoprene-styrene diblock copolymer in the coupled polystyrene-isoprene-styrene block copolymer is 70-80%. The melt index of the polystyrene-(ethylene-styrene-butene)-styrene block copolymer is 5~30 g / 10 min. (200℃,5kg) It contains 15-50% styrene units by mass, and the styrene units in the intermediate polyethylene-styrene-butene block account for 20-60% of the total styrene units in the copolymer.

2. The high and low temperature resistant hot melt adhesive according to claim 1, characterized in that: The melt index of the coupled polystyrene-isoprene-styrene block copolymer is 15~25 g / 10min. (200℃,5kg) It contains 18-22% styrene units by mass.

3. A high and low temperature resistant hot melt adhesive according to claim 1 or 2, characterized in that: The mass percentage of polystyrene-isoprene-styrene diblock copolymer in the coupled polystyrene-isoprene-styrene block copolymer is 70-75%.

4. The high and low temperature resistant hot melt adhesive according to claim 1, characterized in that: The melt index of the polystyrene-(ethylene-styrene-butene)-styrene block copolymer is 10~20 g / 10 min. (200℃,5kg) It contains 25-45% styrene units by mass.

5. A high and low temperature resistant hot melt adhesive according to claim 1, 2 or 4, characterized in that: The filler oil includes naphthenic oil and / or white oil.

6. A high and low temperature resistant hot melt adhesive according to claim 1, 2 or 4, characterized in that: The tackifying resin is a petroleum resin.

7. A high and low temperature resistant hot melt adhesive according to claim 1, 2 or 4, characterized in that: The crosslinking agent includes at least one of dicumyl peroxide, di-tert-butyl peroxide, and di-tert-butyl peroxide.

8. A high and low temperature resistant hot melt adhesive according to claim 1, 2 or 4, characterized in that: The antioxidants include 1076 and / or 168.

9. A method for preparing a high and low temperature resistant hot melt adhesive according to any one of claims 1 to 8, characterized in that: After preheating the filler oil, first add the coupled polystyrene-isoprene-styrene block copolymer and polystyrene-(ethylene-styrene-butene)-styrene block copolymer and stir until completely dissolved. Then add the tackifying resin and continue stirring until the system is transparent. Next, add the crosslinking agent to carry out the crosslinking reaction. Finally, add the antioxidant and stir evenly before discharging and cooling.

10. The application of the high and low temperature resistant hot melt adhesive according to any one of claims 1 to 8, characterized in that: Used for composite materials of core materials in refrigerator vacuum insulation panels, or for edge sealing of refrigerator vacuum insulation panels.

Citation Information

Patent Citations

  • A low-temperature resistant hot melt adhesive and its preparation method

    CN106867429B

  • High-temperature-resistant and high-persistent-adhesion hot melt adhesive for adhesive tape and preparation method of hot melt adhesive

    CN117844416A