A resin composition based on a supramolecular thixotropic network structure, its preparation method and application
By constructing a resin composition based on a supramolecular thixotropic network, the problems of insufficient shape retention and flowability of ultrathin adhesive lines at high temperatures were solved, achieving a balance between shape retention and flowability at high temperatures, and ensuring high toughness and edge wrapping effect of ultrathin dispensing.
Patent Information
- Application Number
- CN202611463717.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to maintain the shape of ultra-thin adhesive lines at high temperatures without collapsing, and they also cannot achieve both good flowability and high toughness, resulting in insufficient coverage of critical areas such as solder joints and corners with ultra-thin adhesive.
A resin composition based on a supramolecular thixotropic network structure is used, including epoxy resin, reactive diluent, multifunctional thiol curing agent, curing accelerator, thixotropic functional agent and silane coupling agent. A dynamic network is constructed by combining monomers with organic thixotropic agents through multiple hydrogen bond self-assembly to improve thixotropy and toughness.
It achieves a balance between shape retention and flowability at high temperatures, ensuring that the adhesive strip remains intact without collapsing after curing at 150℃, can withstand more than 100 bends at room temperature, and maintains good edge wrapping effect, thus solving the problem of dripping in ultra-thin adhesive application.
Smart Images

Figure CN123107597A_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of resin composition technology, and in particular to a resin composition based on a supramolecular thixotropic network structure, its preparation method, and its application. Background Technology
[0002] Flexible printed circuit boards (FPCs) are core components of flexible electronics such as wearable devices and foldable screen phones. Their encapsulation and protection require the encapsulation material to have good fluidity when applied in ultra-thin dispensing (thickness 30μm~90μm), to maintain its shape without collapsing during the thermosetting process, and to be flexible and bendable after curing.
[0003] To address the issue of high-temperature flow and ensure the material retains its shape during thermosetting, thixotropic agents are required. For example, current technologies often employ a thixotropic system composed of fumed silica and organobentonite. While this composite system exhibits some thixotropy at room temperature, the reliance on single hydrogen bonds and physical layer stacking weakens drastically at high temperatures, making it difficult to effectively maintain the colloidal shape during the curing heating phase. This results in insufficient coverage of critical areas such as solder joints and corners in the ultrathin adhesive wire.
[0004] Polyamide wax, a commonly used organic thixotropic agent, relies primarily on hydrogen bonding between molecular chains to form a three-dimensional network for thickening. However, the hydrogen bonds between conventional polyamide wax molecules are mostly non-specific and weak single or double hydrogen bonds, resulting in insufficient stability at high temperatures and easy destruction of the network structure. Consequently, it is difficult to meet the stringent requirements for high-temperature shape retention in ultra-thin precision dispensing.
[0005] Meanwhile, existing composition systems cannot achieve good flowability during ultra-thin dispensing, maintain shape without collapsing, and possess high toughness during thermosetting. Summary of the Invention
[0006] In view of this, this application provides a resin composition based on a supramolecular thixotropic network structure, its preparation method and application. When the resin composition provided in this application is used as an adhesive, it has good flowability in ultra-thin dispensing and high-temperature shape retention and high toughness during thermosetting.
[0007] This application provides a resin composition based on a supramolecular thixotropic network structure, comprising the following components: 40 to 60 parts by weight of epoxy resin; 5 to 15 parts by weight of reactive diluent; 30 to 40 parts by weight of multifunctional thiol curing agent; Curing accelerator: 0.1 to 3 parts by weight; Thixotropic functional agent: 2 to 8 parts by weight; 0.5 to 2 parts by weight of silane coupling agent; Defoamer 0 parts by weight to 0.5 parts by weight; Pigment 0 to 2 parts by weight; The thixotropic functional agent includes a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent; Alternatively, the thixotropic functional agent may be obtained by reacting a monomer containing isocyanate with an amino-containing organic thixotropic agent.
[0008] In some specific implementations, the weight ratio of the multi-hydrogen-bonded self-assembling monomer to the organic thixotropic agent is 1~2:1.
[0009] In some specific implementations, the isocyanate-containing multiple hydrogen bond assembly monomer is selected from formula (I) or formula (II). (I); (II); Wherein, R is a C1~C6 alkyl group.
[0010] In some specific implementations, the multiple hydrogen bond self-assembly monomer is selected from formula (III), formula (IV) or formula (V). (III); (Ⅳ); (V); Wherein, R is a C1~C6 alkyl group.
[0011] In some specific implementations, the multi-hydrogen-bonded self-assembled monomer is selected from formula (VI) and formula (VII). (VI); (VII).
[0012] In some specific implementations, the amino-containing organic thixotropic agent and the organic thixotropic agent are each independently selected from one or more of polyamide wax, polyamide solution and diamide.
[0013] In some specific implementations, the epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, alicyclic epoxy resin, trifunctional epoxy resin, and tetrafunctional epoxy resin. The reactive diluent is butyl glycidyl ether, glycerol epoxy resin, resorcinol diglycidyl ether, 1,4-butanediol diglycidyl ether, and C... 12 ~C 14 One or more of alkyl glycidyl ethers; The multifunctional thiol curing agent is one or both of trimethylolpropane tris(3-mercaptopropionic acid) ester or pentaerythritol tetra(3-mercaptopropionic acid) ester. The curing accelerator is one or both of imidazole accelerators and modified amine accelerators; The silane coupling agent is selected from one or more of 3-glycidyl etheroxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, titanate coupling agents, and aluminate coupling agents.
[0014] This application also provides a method for preparing a resin composition based on a supramolecular thixotropic network structure, comprising the following steps: a) Mix epoxy resin and reactive diluent to obtain the first component; b) Mix the first component with the thixotropic agent to obtain the second component; c) Mix the second component, the multifunctional thiol curing agent, the curing accelerator and the silane coupling agent to obtain the third component; d) The third component, defoamer, and pigment are mixed to obtain a resin composition.
[0015] In some specific implementations, in step a), the mixing temperature is 15℃~25℃ and the rotation speed is 300rpm / min~500rpm / min; In step b), the mixing temperature is 40℃~50℃, the rotation speed is 800rpm / min~1200rpm / min, and the time is 30min~60min; In step c), the mixing temperature is 0℃~25℃, the rotation speed is 400rpm / min~600rpm / min, and the time is 20min~30min.
[0016] This application also provides a single-component epoxy resin adhesive based on a supramolecular thixotropic network structure, comprising the resin composition described in any of the above technical solutions or the resin composition prepared by the preparation method described in any of the above technical solutions.
[0017] This application provides a resin composition based on a supramolecular thixotropic network structure, comprising the following components: 40-60 parts by weight of epoxy resin; 5-15 parts by weight of reactive diluent; 30-40 parts by weight of polyfunctional thiol curing agent; 0.1-3 parts by weight of curing accelerator; 2-8 parts by weight of thixotropic functional agent; 0.5-2 parts by weight of silane coupling agent; 0-0.5 parts by weight of defoamer; and 0-2 parts by weight of pigment. The thixotropic functional agent comprises a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent; or the thixotropic functional agent is obtained by reacting an isocyanate-containing multi-hydrogen-bonded self-assembly monomer with an amino-containing organic thixotropic agent. This application achieves a synergistic improvement in the thixotropy, shape retention, and toughness of the resin composition system by introducing a dynamic network constructed from specific multi-hydrogen-bonded supramolecular units and a flexible thiol network at the microscopic level. Experimental results show that when the resin composition provided in this application is used as an adhesive, the thixotropic viscosity ratio is ≥4.0, the sag length after standing on a vertical plane at 25℃ for 10 min is ≤1, the adhesive strip shape remains intact without collapse after curing at 150℃ for 15 min, and the number of bends at room temperature is >100; furthermore, while achieving ultra-thin dispensing process, the adhesive still maintains good edge and corner wrapping effect and no sag phenomenon. Attached Figure Description
[0018] Figure 1 These are schematic diagrams of dispensing cross-sections of the adhesives described in Comparative Examples 1 and 3 of this application after curing at 150°C. Figure 1 (a) is a schematic diagram of a slice after the adhesive described in Comparative Example 1 has been cured at 150°C. Figure 1 (b) is a schematic diagram of a cross-section of the adhesive described in Comparative Example 3 of this application after curing at 150°C; Figure 2 These are schematic diagrams of dispensing sections of the adhesives described in Examples 3 and 4 of this application after curing at 150°C. Figure 2 (a) is a schematic diagram of a slice after the adhesive described in Example 3 has been cured at 150°C and then applied. Figure 2 (b) is a schematic diagram of the adhesive slice after curing at 150°C according to Example 4 of this application. Detailed Implementation
[0019] It should be understood that the expression “one or more of…” individually includes each of the objects described after the expression, as well as various different combinations of two or more of the described objects, unless otherwise understood from the context and usage. The expression “and / or” combined with three or more described objects should be understood to have the same meaning, unless otherwise understood from the context.
[0020] The terms “including,” “having,” or “containing,” including the use of their grammatical synonyms, should generally be understood as open-ended and non-restrictive, for example, not excluding other unstated elements or steps, unless otherwise specifically stated or understood from the context.
[0021] It should be understood that the order of steps or the sequence of actions is not important as long as this application remains operational. Furthermore, two or more steps or actions may be performed simultaneously.
[0022] The use of any and all instances or exemplary language such as “e.g.” or “including” herein is merely intended to better illustrate the application and does not constitute a limitation on the scope of the application unless the claims are made. No language in this specification should be construed as indicating that any unclaimed element is essential to the practice of this application.
[0023] Furthermore, the numerical ranges and parameters used to define this application are approximate values, and the relevant values in the specific embodiments have been presented as precisely as possible. However, any numerical value inevitably contains standard deviations due to individual test methods. Therefore, unless otherwise explicitly stated, it should be understood that all ranges, quantities, values, and percentages used in this disclosure are modified with the word "approximately." Here, "approximately" generally means that the actual value is within plus or minus 10%, 5%, 1%, or 0.5% of a specific value or range.
[0024] This application provides a resin composition based on a supramolecular thixotropic network structure, comprising the following components: 40 to 60 parts by weight of epoxy resin; 5 to 15 parts by weight of reactive diluent; 30 to 40 parts by weight of multifunctional thiol curing agent; Curing accelerator: 0.1 to 3 parts by weight; Thixotropic functional agent: 2 to 8 parts by weight; 0.5 to 2 parts by weight of silane coupling agent; Defoamer 0 parts by weight to 0.5 parts by weight; Pigment 0 to 2 parts by weight; The thixotropic functional agent includes a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent; Alternatively, the thixotropic functional agent may be obtained by reacting a monomer containing isocyanate with an amino-containing organic thixotropic agent.
[0025] This application does not impose any special restrictions on the source of epoxy resin, reactive diluent, multifunctional thiol curing agent, curing accelerator and silane coupling agent, which can be purchased from commercial sources.
[0026] In this application, the resin composition includes an epoxy resin, which serves as the matrix resin constituting the main cross-linking skeleton of the cured material, imparting basic adhesive strength, mechanical properties, and chemical stability to the cured product, and adjusting the basic viscosity of the system. In some specific implementations, the epoxy resin is 40 to 60 parts by weight, preferably 45 to 55 parts by weight. In some specific implementations, the epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, alicyclic epoxy resin, trifunctional epoxy resin, and tetrafunctional epoxy resin, preferably bisphenol A epoxy resin.
[0027] In this application, the resin composition includes an active diluent, which reduces the viscosity of the system, improves the flowability and coating operability of the resin composition, and facilitates thorough mixing of the components. In some specific implementations, the active diluent is 5 to 15 parts by weight, preferably 8 to 12 parts by weight. In some specific implementations, the active diluent is butyl glycidyl ether, glycerol epoxy resin, resorcinol bisglycidyl ether, 1,4-butanediol diglycidyl ether, and C... 12 ~C 14 One or more of alkyl glycidyl ethers, preferably 1,4-butanediol diglycidyl ether.
[0028] In this application, the resin composition includes a polyfunctional thiol curing agent, which is used to achieve rapid, low-temperature curing of the resin and to form a high-performance crosslinking network. In some specific implementations, the polyfunctional thiol curing agent is present in an amount of 30 to 40 parts by weight, preferably 32 to 38 parts by weight. In some specific implementations, the polyfunctional thiol curing agent is one or both of trimethylolpropane tris(3-mercaptopropionic acid) ester or pentaerythritol tetra(3-mercaptopropionic acid) ester, preferably trimethylolpropane tris(3-mercaptopropionic acid) ester.
[0029] The multifunctional thiol curing agent is the core crosslinking and curing component of this system. Its molecules contain multiple highly active thiol groups, which can undergo efficient nucleophilic addition reactions with the epoxy groups of epoxy resin under heating conditions of 150℃, achieving rapid high-temperature curing. Compared to traditional amine and anhydride curing agents, the multifunctional thiol curing agent exhibits milder exothermic reactions during high-temperature curing, with a significantly lower exothermic peak. Under the combined effect of external heating and internal exothermic reactions, the lower exothermic peak effectively prevents excessive temperature rise, thus protecting the supramolecular thixotropic network constructed by multiple hydrogen bonds from thermal damage and maximizing the preservation of the composition's excellent thixotropic anti-sagging properties during high-temperature curing. Simultaneously, the molecular structure of the multifunctional thiol significantly increases the crosslinking density of the cured system, and the resulting thioether bonds exhibit good flexibility, endowing the cured product with excellent flexibility.
[0030] In this application, the resin composition includes a curing accelerator, which is used to precisely catalyze the thiol-epoxy crosslinking reaction between the epoxy resin and the multifunctional thiol curing agent, effectively reducing the activation energy of the curing reaction. Under high-temperature curing conditions of 150°C, the accelerator can significantly accelerate the ring-opening addition reaction rate of thiol and epoxy groups, solving the problem of slow reaction rate and long curing cycle when no accelerator is added. This allows the composition to achieve rapid and complete curing within 15 minutes, precisely controlling and significantly improving the high-temperature curing efficiency, while ensuring that the cured product has ideal crosslinking density and mechanical properties. In some specific implementations, the curing accelerator is 0.1 parts by weight to 3 parts by weight, preferably 0.5 parts by weight to 1.5 parts by weight. In some specific implementations, the curing accelerator is one or both of imidazole accelerators or modified amine accelerators, preferably modified amine accelerators.
[0031] In this application, the resin composition includes a thixotropic functional agent, which forms a reversible supramolecular network structure through intermolecular non-covalent interactions, thereby endowing the resin composition with excellent thixotropic properties. In some specific implementations, the thixotropic functional agent is present in an amount of 2 to 8 parts by weight, preferably 3 to 7 parts by weight.
[0032] The thixotropic functional agent described in this application can achieve a supramolecular network structure with multiple hydrogen bonds in the thixotropic agent system. Specifically, it is a compound or polymer that forms a supramolecular network structure through self-assembly of multiple hydrogen bonds (such as DADA·ADAD type, UPy type, tetrad hydrogen-bonded dimers based on triazine and pyrimidine derivatives, etc.). In some specific implementations, the thixotropic functional agent includes a multi-hydrogen-bonded self-assembling monomer and an organic thixotropic agent; or the thixotropic functional agent is obtained by reacting an isocyanate-containing multi-hydrogen-bonded self-assembling monomer with an amino-containing organic thixotropic agent.
[0033] The thixotropic functional agent can be prepared by chemical grafting modification. This preparation method involves reacting the active groups of a multi-hydrogen-bonded self-assembly monomer with the active groups of an organic thixotropic agent, thereby grafting the multi-hydrogen-bonded self-assembly monomer onto the organic thixotropic agent in the form of chemical bonds. This can include, but is not limited to: polymers with tetrahydrogen-bonded groups such as ureidopyrimidinone (UPy) and 2,7-diamino-1,8-naphthylpyridine (DAN) at the ends or sides (such as polyamide waxes, polyesters, polyethers, etc.); polymers with hexahydrogen-bonded groups at both ends (such as polyethylene glycol derivatives); and other small molecules or polymers that can form trimers or higher-order multihydrogen-bonded arrays.
[0034] This application does not specifically limit the types of active groups involved in the reaction of the multi-hydrogen-bonded self-assembly functional monomer and the organic thixotropic agent. In some specific implementations, the thixotropic functional agent is preferably obtained by reacting an isocyanate-containing multi-hydrogen-bonded assembly monomer with an amino-containing organic thixotropic agent, and the number-average molecular weight of the modified thixotropic functional agent is 1000 Da to 10000 Da, preferably 7500 Da.
[0035] In some specific implementations, the isocyanate-containing multiple hydrogen bond assembly monomer includes, but is not limited to, the structures shown in formula (I) or formula (II); (I); (II); Wherein, R is a C1 to C6 alkyl group, preferably a C1 to C3 alkyl group.
[0036] In some specific implementations, the amino-containing organic thixotropic agent is selected from one or more of polyamide wax, polyamide solution and diamide, preferably polyamide wax.
[0037] The isocyanate-containing multi-hydrogen bond assembly monomer described in this application can be prepared by reacting it with an amino-containing organic thixotropic agent according to the following preparation method: 1) Mix an amino-containing organic thixotropic agent with a solvent to obtain an amino-containing organic thixotropic agent solution; 2) Mix the isocyanate-containing multi-hydrogen bond assembly monomer with a solvent to obtain an isocyanate-containing multi-hydrogen bond assembly monomer solution; 3) The amino-containing organic thixotropic agent solution and the isocyanate-containing multi-hydrogen bond assembly monomer solution are reacted to obtain the thixotropic functional agent.
[0038] The types of amino-containing organic thixotropic agents and isocyanate-containing multi-hydrogen bond assembly monomers described in this application are as described above, and will not be repeated here. In some specific implementations, the amino-containing organic thixotropic agent solution is preferably prepared under nitrogen atmosphere, heated to 70°C, and stirred until completely dissolved. In some specific implementations, the solvent is preferably anhydrous N,N-dimethylformamide. In some specific implementations, the molar ratio of the terminal amino group of the amino-containing organic thixotropic agent to the isocyanate-containing multi-hydrogen bond assembly monomer is 1:1.02~1.1, preferably 1:1.04~1.06. In some specific implementations, the isocyanate-containing multi-hydrogen bond assembly monomer solution is preferably slowly added dropwise to the amino-containing organic thixotropic agent solution through a constant pressure dropping funnel, completing the addition in about 1 hour. In some specific implementations, the reaction temperature is 60°C~80°C, preferably 65°C~75°C; the reaction time is 5 hours~7 hours, preferably 5.5 hours~6.5 hours.
[0039] After the reaction is complete, the reaction solution is preferably cooled to room temperature and stirred in an ice-water bath to precipitate the product. The precipitate is then filtered and washed three times with ethanol to remove unreacted isocyanate-containing multi-hydrogen bonded monomers and solvent. Finally, the resulting white solid is vacuum dried at 45°C–55°C for 20–30 h to obtain the thixotropic functional agent.
[0040] The thixotropic functional agent may also include a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent. In some specific implementations, the weight ratio of the multi-hydrogen-bonded self-assembly monomer to the organic thixotropic agent is 1~2:1, preferably 1.4~1.6:1.
[0041] This application does not impose any special restrictions on the selection of the multi-hydrogen-bonded self-assembly functional monomer. In some specific implementations, the multi-hydrogen-bonded self-assembly monomer can be a single molecule, including but not limited to the structures shown in formula (III), formula (IV), or formula (V); (III); (Ⅳ); (V); Wherein, R is a C1 to C6 alkyl group, preferably a C1 to C3 alkyl group.
[0042] When R is a C2 alkyl group, the structure shown in formula (V) is 2-ureido-6-(4-aminophenyl)-4-pyrimidinone, possessing the DADA hydrogen bond sequence. This compound can self-assemble in a suitable solvent to form a dimer based on a DADA-ADAD quadruple hydrogen bond array. This dimer can further form a three-dimensional supramolecular network under static conditions. DADA and ADAD are two equivalent expressions of the same self-complementary dimer, reading the hydrogen bond sequence from opposite directions.
[0043] In some specific implementations, the multi-hydrogen-bonded self-assembly monomer can be a bimolecular monomer, including but not limited to formula (VI) and formula (VII). (VI); (VII).
[0044] In some specific implementations, the organic thixotropic agent is selected from one or more of polyamide wax, polyamide solution and diamide, preferably polyamide wax.
[0045] In this application, the resin composition includes a silane coupling agent, which can effectively improve the interfacial compatibility between the components. In some specific implementations, the silane coupling agent is 0.5 to 2 parts by weight, preferably 0.5 to 1.5 parts by weight. In some specific implementations, the silane coupling agent includes, but is not limited to, 3-glycidyl etheroxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, titanate coupling agents, or aluminate coupling agents, etc., and may be one or two of them. When the silane coupling agent is a combination of two substances, this application does not have a special limitation on the proportion of each specific substance. In some specific implementations, the silane coupling agent is preferably 3-glycidyl etheroxypropyltrimethoxysilane.
[0046] In this application, the resin composition includes a defoamer used to eliminate and inhibit the generation of bubbles in the resin composition, thereby improving the processing technology. In some specific implementations, the defoamer is present in an amount of 0 to 0.5 parts by weight, preferably 0 to 0.2 parts by weight. In some specific implementations, the defoamer is selected from one or more of polyether-modified polysiloxanes, fatty alcohol polyethers, polyvinyl ether copolymers, and fluorinated acrylate copolymers.
[0047] In this application, the resin composition includes a pigment used to impart the desired color to the resin composition, while also improving the weather resistance, opacity, and protective properties of the article. In some specific implementations, the pigment is 0 to 2 parts by weight, preferably 0 to 1 part by weight. In some specific implementations, the pigment is selected from one or both of inorganic and organic pigments.
[0048] In this application, the resin composition further includes a stabilizer. This application does not impose any particular limitation on the specific type and amount of the stabilizer; any type and amount commonly used by those skilled in the art can be used. In some specific implementations, the stabilizer is selected from one or more of salicylic acid, barbituric acid, lauric acid, and fumaric acid.
[0049] In the resin composition system provided in this application, the introduced supramolecular physical network based on multiple hydrogen bonds is highly compatible and functionally complementary to the chemical cross-linking network formed by the flexible multifunctional thiol curing agent in the formulation. Before curing, the physical network dominates the rheology, ensuring processability and shape retention; after curing, the chemical network provides strength and durability, while the remaining dynamic physical network and its flexible segments can effectively disperse stress and hinder crack propagation, thereby significantly improving the toughness of the cured product without significantly sacrificing modulus. In summary, the key to this application lies in introducing specific supramolecular units with multiple hydrogen bonds that can form a strong dynamic physical network and synergizing them with the flexible chemical network in a systematic manner, rather than simply physical blending of components.
[0050] This application does not impose any particular limitation on the preparation method of the resin composition, which can be prepared according to the following method: a) Mix epoxy resin and reactive diluent to obtain the first component; b) Mix the first component with the thixotropic agent to obtain the second component; c) Mix the second component, the multifunctional thiol curing agent, the curing accelerator and the silane coupling agent to obtain the third component; d) The third component, defoamer, and pigment are mixed to obtain a resin composition.
[0051] This application first mixes epoxy resin and reactive diluent. The specific types and amounts of epoxy resin and reactive diluent are as described above and will not be repeated here. In some specific implementations, the mixing temperature is 15℃~25℃, preferably 15℃~20℃; the rotation speed is 300rpm / min~500rpm / min, preferably 350rpm / min~450rpm / min. This application does not have a special limitation on the mixing time, as long as the mixing system is stirred evenly.
[0052] After obtaining the first component, the first component is mixed with a thixotropic agent. The specific type and amount of the thixotropic agent are as described above, and will not be repeated here. In some specific implementations, the mixing temperature is 40℃~50℃, preferably 42℃~48℃; the rotation speed is 800rpm / min~1200rpm / min, preferably 900rpm / min~1100rpm / min; and the time is 30min~60min, preferably 40min~50min.
[0053] After obtaining the second component, the second component, the polyfunctional thiol curing agent, the curing accelerator, and the silane coupling agent are mixed. The specific types and amounts of the polyfunctional thiol curing agent, the curing accelerator, and the silane coupling agent are as described above, and will not be repeated here. In some specific implementations, the mixing temperature is 0℃~25℃, preferably 10℃~20℃; the rotation speed is 400rpm / min~600rpm / min, preferably 450rpm / min~550rpm / min; and the time is 20min~30min, preferably 22min~28min.
[0054] After obtaining the third component, the third component, defoamer, and pigment are mixed. The specific types and amounts of the defoamer and pigment are as described above and will not be repeated here. In some specific implementations, the mixing is preferably carried out at 400 rpm / min to 600 rpm / min for 10 min to 15 min.
[0055] After mixing in step d), the mixture is preferably transferred to a vacuum degassing machine for degassing to obtain a resin composition. In some specific implementations, the vacuum degree of degassing is -0.085 MPa to -0.1 MPa, preferably -0.095 MPa; the time is 5 min to 10 min, preferably 6 min to 9 min.
[0056] Preferably, when the thixotropic functional agent comprises a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent, it is preferably prepared according to the following method: 1) Mix the multi-hydrogen-bonded self-assembly monomer and the reactive diluent to obtain a multi-hydrogen-bonded self-assembly system; 2) The epoxy resin and the multi-hydrogen bond self-assembly system were mixed to obtain the fourth component; 3) Mix the fourth component with the organic thixotropic agent to obtain the fifth component; 4) Mix the fifth component, the polyfunctional thiol curing agent, the curing accelerator, and the silane coupling agent to obtain the sixth component; 5) Mix the sixth component, defoamer, and pigment to obtain a resin composition.
[0057] This application first mixes a multi-hydrogen-bonded self-assembly monomer and a reactive diluent. The specific types and amounts of the multi-hydrogen-bonded self-assembly monomer and the reactive diluent are as described above and will not be repeated here. In some specific implementations, the mixing process specifically involves heating the reactive diluent to 65℃~75℃ and stirring, then slowly adding the multi-hydrogen-bonded self-assembly monomer to the reactive diluent in batches, and continuing stirring at 65℃~75℃ for 1h~2h. In some specific implementations, the addition time of the multi-hydrogen-bonded self-assembly monomer is preferably 25min~35min.
[0058] The parameters of the specific mixing process in steps 2) to 5) are as described in steps a) to d) above, and will not be repeated here.
[0059] This application also provides a single-component epoxy resin adhesive based on a supramolecular thixotropic network structure, comprising the resin composition described in any of the above technical solutions or the resin composition prepared by the preparation method described in any of the above technical solutions.
[0060] The single-component epoxy resin adhesive based on a supramolecular thixotropic network structure provided in this application has the following advantages: First, it achieves a balance between low viscosity application and high heat retention: Due to the dynamic reversible nature of the multi-hydrogen bonded supramolecular network, the colloid exhibits a low initial viscosity (2500 mPa·s~4500 mPa·s) under shear, facilitating precise dispensing; after standing, the network recovers rapidly, providing timely anti-sagging properties, and the thermosetting shape retention rate is >97%, completely solving the problem of flow of ultra-thin adhesive lines at high temperatures and ensuring effective encapsulation of critical parts of the FPC.
[0061] Secondly, a balance between high toughness and good strength was achieved: the flexible thiol curing agent contributed the intrinsic flexible network structure, while the dynamic reversibility of the multiple hydrogen-bonded supramolecular network and the synergy of its flexible segments further realized stress dispersion and crack prevention. The combined effect of these two factors enabled the cured product to maintain sufficient tensile strength while achieving an elongation at break exceeding 200%, fully meeting the reliability requirements of flexible electronic devices.
[0062] Third, this application is not a simple superposition of components, but rather achieves the two mutually restrictive properties of "low viscosity and high thermal conductivity" and "high toughness and high tensile strength" through the intrinsic synergy between the dynamic network constructed by introducing specific multiple hydrogen bond supramolecular units and the flexible thiol network at the microscopic level, thus providing an innovative solution for flexible electronic ultrathin packaging technology.
[0063] This application provides a resin composition based on a supramolecular thixotropic network structure, comprising the following components: 40-60 parts by weight of epoxy resin; 5-15 parts by weight of reactive diluent; 30-40 parts by weight of polyfunctional thiol curing agent; 0.1-3 parts by weight of curing accelerator; 2-8 parts by weight of thixotropic functional agent; 0.5-2 parts by weight of silane coupling agent; 0-0.5 parts by weight of defoamer; and 0-2 parts by weight of pigment. The thixotropic functional agent comprises a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent; or the thixotropic functional agent is obtained by reacting an isocyanate-containing multi-hydrogen-bonded self-assembly monomer with an amino-containing organic thixotropic agent. This application achieves a synergistic improvement in the thixotropy, shape retention, and toughness of the resin composition system by introducing a dynamic network constructed from specific multi-hydrogen-bonded supramolecular units and a flexible thiol network at the microscopic level. Experimental results show that when the resin composition provided in this application is used as an adhesive, the thixotropic viscosity ratio is ≥4.0, the sag length after standing on a vertical plane at 25℃ for 10 min is ≤1, the adhesive strip shape remains intact without collapse after curing at 150℃ for 15 min, and the number of bends at room temperature is >100; furthermore, while achieving ultra-thin dispensing process, the adhesive still maintains good edge and corner wrapping effect and no sag phenomenon.
[0064] The present invention is further illustrated below with reference to the embodiments. The scope of protection of the present invention is not limited to the following embodiments.
[0065] Example 1
[0066] This embodiment provides a UPy modified polyamide wax thixotropic agent, including the following steps: (1) In a dry, nitrogen-protected three-necked flask, add 10g of polyamide wax (hexamethylenediamine and dodecanoic acid condensation, with a number average molecular weight Mn of about 2500) and 100mL of anhydrous N,N-dimethylformamide (DMF), heat to 70°C and stir to dissolve completely.
[0067] (2) 20 mL of anhydrous DMF solution containing 2.2 g of ethyl isocyanate ureidopyrimidinone (UPy-NCO, see formula (I), the molar amount is about 1.05 times that of the terminal amino group of polyamide wax) was slowly added dropwise to the above solution through a constant pressure dropping funnel, and the addition was completed in about 1 hour.
[0068] (I).
[0069] (3) After the addition is completed, the reaction continues for 6 hours under nitrogen protection at 70°C.
[0070] (4) After the reaction is complete, the reaction solution is cooled to room temperature, and then stirred in an ice-water bath to precipitate the product. The product is then filtered and washed three times with ethanol to remove unreacted UPy-NCO and solvent. Finally, the obtained white solid is vacuum dried at 50°C for 24 hours and ground to obtain white powder of UPy modified polyamide wax (UPy-polyamide wax).
[0071] Example 2
[0072] (1) In a dry, nitrogen-protected three-necked flask, add 10g of polyamide wax and 100mL of anhydrous DMF, heat to 70°C and stir until completely dissolved.
[0073] (2) 20 mL of anhydrous DMF solution containing 2.0 g of 1,5-diaminonaphthalene-terminated isocyanate prepolymer (DAN-NCO, see formula (II), the molar amount is about 1.05 times that of the terminal amino group of polyamide wax) was slowly added dropwise to the above solution through a constant pressure dropping funnel, and the addition was completed in about 1 hour.
[0074] (II); Wherein, R is a C2 alkyl group.
[0075] (3) After the addition is completed, the reaction continues for 6 hours at 70°C under nitrogen protection. During the reaction, the isocyanate group (-NCO) of DAN-NCO undergoes a nucleophilic addition reaction with the amino group (-NH2) at the end of the polyamide wax to generate a urea bond, introducing the DAN group into the polyamide wax molecular chain.
[0076] (4) After the reaction is complete, the reaction solution is cooled to room temperature, and then stirred in an ice-water bath to precipitate the product. The product is filtered and washed three times with ethanol to remove unreacted DAN-NCO and solvent. The obtained solid is dried under vacuum at 50°C for 24 hours and then ground to obtain DAN-modified polyamide wax (DAN-polyamide wax) powder.
[0077] Example 3
[0078] The specific formula of the adhesive provided in this embodiment is as follows: (unit: parts by weight)
[0079] Epoxy resin (bisphenol A type): 50 parts by weight; Reactive diluent (1,4-butanediol diglycidyl ether): 10 parts by weight; Curing agent (trimethylolpropane tris(3-mercaptopropionic acid) ester TMPMP): 35 parts by weight; Curing accelerator (modified amine, EH-4357S): 1 part by weight; Thixotropic functional agent (UPy-polyamide wax): 5 parts by weight; Silane coupling agent (KH560): 1 part by weight; The preparation method is as follows: (1) Weigh the epoxy resin and reactive diluent and put them into the stirring reaction equipment. Control the system temperature to 18°C and set the stirring speed to 400 rpm / min. Continue stirring and mixing until the materials are completely uniform.
[0080] (2) Add thixotropic functional agent to the above mixture, slowly heat to 45°C, adjust the stirring speed to 1000 rpm / min, and disperse at high speed for 45 min.
[0081] (3) Cool the above mixture to 15°C, add curing agent, curing accelerator and coupling agent in sequence, adjust the stirring speed to 500 rpm / min and continue stirring for 25 min.
[0082] (4) Transfer the mixed adhesive to a vacuum degassing device and degas it for 8 minutes under a vacuum of -0.095MPa to completely remove the bubbles inside the system. After degassing is completed, the material is discharged to obtain the finished single-component epoxy resin adhesive.
[0083] Example 4
[0084] The only difference from Example 3 is that 5 parts by weight of UPy-polyamide wax are replaced with 5 parts by weight of DAN-polyamide wax, which was prepared in Example 2.
[0085] Example 5
[0086] The specific formula of the adhesive provided in this embodiment is as follows: (unit: parts by weight)
[0087] Epoxy resin (bisphenol A type): 50 parts by weight; Reactive diluent (C 12 ~C 14 Alkyl glycidyl ether (AGE): 10 parts by weight; Curing agent (trimethylolpropane tris(3-mercaptopropionic acid) ester TMPMP): 35 parts by weight; Curing accelerator (2-ethyl-4-methylimidazole): 1 part by weight; Thixotropic functional agent: 5 parts by weight; including 2 parts by weight of polyamide wax and 3 parts by weight of 2-ureido-6-(4-aminophenyl)-4-pyrimidinone; Silane coupling agent (KH560): 1 part by weight.
[0088] The preparation method is as follows: (1) Add 10 parts by weight of C to a dry three-necked flask. 12 ~C 14Alkyl glycidyl ether (AGE) was heated to 70°C and stirred. Three parts by weight of 2-ureido-6-(4-aminophenyl)-4-pyrimidinone (see formula (V), possessing the DADA hydrogen bond sequence) were slowly added to the above solution in portions, completing the addition over approximately 30 minutes. The mixture was then stirred at 70°C for 1.5 hours. During this process, the 2-ureido-6-(4-aminophenyl)-4-pyrimidinone molecules self-assembled (homogeneously dimerized) through complementary quadruple hydrogen bonds between DADA and ADAD, forming a uniformly dispersed supramolecular association system. After mixing, the system was cooled to room temperature to obtain the DADA / ADAD quadruple hydrogen bond supramolecular self-assembled system.
[0089] (2) Weigh the epoxy resin and DADA / ADAD quadruple hydrogen bond supramolecular self-assembly system and put them into the stirring reaction equipment. Control the system temperature to 18℃, set the stirring speed to 400rpm / min, and continue stirring and mixing until the materials are completely uniform.
[0090] (3) Add polyamide wax to the above mixture, slowly heat to 45°C, adjust the stirring speed to 1000 rpm / min, and disperse at high speed for 45 min.
[0091] (4) Cool the above mixture to 15°C, add curing agent, curing accelerator and coupling agent in sequence, adjust the stirring speed to 500 rpm / min and continue stirring for 25 min.
[0092] (5) Transfer the mixed adhesive to a vacuum degassing device and degas it for 8 minutes under a vacuum of -0.095MPa to completely remove the bubbles inside the system. After degassing is completed, the material is discharged to obtain the finished single-component epoxy resin adhesive.
[0093] (V); Wherein, R is a C2 alkyl group.
[0094] Comparative Example 1
[0095] The only difference from Example 3 is that 5 parts by weight of the thixotropic functional agent is replaced with 5 parts by weight of the inorganic thixotropic agent, which consists of 3 parts by weight of organic bentonite and 2 parts by weight of fumed silica.
[0096] Comparative Example 2
[0097] The only difference from Example 3 is that 35 parts by weight of trimethylolpropane tris(3-mercaptopropionic acid) ester (TMPMP) is replaced with 26 parts by weight of polyetheramine (D230).
[0098] Comparative Example 3
[0099] The only difference from Example 3 is that 5 parts by weight of the thixotropic functional agent is replaced with 5 parts by weight of an inorganic thixotropic agent, which is fumed silica.
[0100] Experimental Example 1
[0101] To verify the technical effect of this application, the above embodiments and comparative examples were set up. The specific formulas are shown in Table 1 (unit: parts by weight): Table 1 Formulations of the adhesives described in Examples 3-5 and Comparative Examples 1-3
[0102] The relevant performance of Examples 3-5 and Comparative Examples 1-3 were tested, and the results are shown in Table 2.
[0103] Table 2 Performance test results of the adhesives described in Examples 3-5 and Comparative Examples 1-3
[0104] As shown in Table 1, Examples 3-5 used different types of thixotropic functional agents, and all of them exhibited excellent and balanced performance, especially in shape retention at high temperatures and ultra-long bending life, demonstrating the universal superiority of the synergistic effect of supramolecular networks based on multiple hydrogen bonds and thiol curing agents.
[0105] In comparison, Comparative Example 1, using a traditional thixotropic system combining fumed silica and organobentonite, exhibited significantly insufficient shape retention at high temperatures, with sagging still occurring at the edges. Furthermore, compared to the thixotropic functional agent combined with a thiol-based curing agent in the examples, its toughness decreased. Comparative Example 3, using only fumed silica as the thixotropic agent, showed slightly worse high-temperature shape retention than Comparative Example 1, indicating that a single thixotropic agent offers limited performance improvement. In summary, regardless of whether it is a single agent or a combination, traditional inorganic thixotropic agent systems have significant shortcomings in high-temperature shape retention.
[0106] Comparative Example 2 used a conventional amine curing agent, and the resulting cured adhesive layer was extremely brittle and had very poor toughness, which completely failed to meet the basic toughness requirements of flexible electronics. Moreover, compared with the thixotropic functional agent combined with thiol curing agent in the examples, the high-temperature shape retention was reduced.
[0107] In summary, this comparative result clearly reveals that thixotropic functional agents and multifunctional thiol curing agents are indispensable core components that endow this system with high-temperature shape retention and excellent toughness. This application creatively solves the existing technical challenges by introducing thixotropic functional agents capable of forming multiple hydrogen bond networks and synergizing them with flexible thiol curing agents.
[0108] Experimental Example 2
[0109] Figure 1These are schematic diagrams of dispensing cross-sections of the adhesives described in Comparative Examples 1 and 3 of this application after curing at 150°C. Figure 1 (a) is a schematic diagram of a slice after the adhesive described in Comparative Example 1 has been cured at 150°C. Figure 1 (b) is a schematic diagram of a cross-section of the adhesive described in Comparative Example 3 of this application after curing at 150°C. Figure 1 It can be seen that, Figure 1 (a) and Figure 1 (b) Obvious glue flow was observed at the right corner, indicating that its high temperature shape retention was insufficient and could not meet the shape retention requirements of ultra-thin dispensing.
[0110] Figure 2 These are schematic diagrams of dispensing sections of the adhesives described in Examples 3 and 4 of this application after curing at 150°C. Figure 2 (a) is a schematic diagram of a slice after the adhesive described in Example 3 has been cured at 150°C and then applied. Figure 2 (b) is a schematic diagram of a cross-section of the adhesive strip after curing at 150°C according to Example 4 of this application. Figure 2 It can be seen that, Figure 2 (a) and Figure 2 (b) The thickness of the adhesive coating in the corner areas was controlled within the range of 30 μm to 90 μm. This result indicates that while achieving an ultra-thin dispensing process, the adhesive still maintains good corner coating effect without sagging.
[0111] The above description is merely a preferred embodiment of this application, but the scope of protection of this application is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in this application, based on the technical solution and inventive concept of this application, should be included within the scope of protection of this application.
Claims
1. A resin composition based on a supramolecular thixotropic network structure, characterized in that, Includes the following components: 40 to 60 parts by weight of epoxy resin; 5 to 15 parts by weight of reactive diluent; 30 to 40 parts by weight of multifunctional thiol curing agent; Curing accelerator: 0.1 to 3 parts by weight; Thixotropic functional agent: 2 to 8 parts by weight; 0.5 to 2 parts by weight of silane coupling agent; Defoamer 0 parts by weight to 0.5 parts by weight; Pigment 0 to 2 parts by weight; The thixotropic functional agent includes a multi-hydrogen-bonded self-assembly monomer and an organic thixotropic agent; Alternatively, the thixotropic functional agent may be obtained by reacting a monomer containing isocyanate with an amino-containing organic thixotropic agent.
2. The resin composition according to claim 1, characterized in that, The weight ratio of the multi-hydrogen-bonded self-assembled monomer to the organic thixotropic agent is 1~2:
1.
3. The resin composition according to claim 1, characterized in that, The isocyanate-containing multiple hydrogen bond assembly monomer is selected from formula (I) or formula (II); (Ⅰ); (Ⅱ); Wherein, R is a C1~C6 alkyl group.
4. The resin composition according to claim 1, characterized in that, The multi-hydrogen bond self-assembly monomer is selected from formula (III), formula (IV) or formula (V). (Ⅲ); (Ⅳ); (Ⅴ); Wherein, R is a C1~C6 alkyl group.
5. The resin composition according to claim 1, characterized in that, The multi-hydrogen bond self-assembly monomer is selected from formula (VI) and formula (VII). (Ⅵ); (Ⅶ)。 6. The resin composition according to claim 1, characterized in that, The amino-containing organic thixotropic agent and the organic thixotropic agent are each independently selected from one or more of polyamide waxes, polyamide solutions, and diamides.
7. The resin composition according to claim 1, characterized in that, The epoxy resin is one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, alicyclic epoxy resin, trifunctional epoxy resin, and tetrafunctional epoxy resin. The reactive diluent is butyl glycidyl ether, glycerol epoxy resin, resorcinol diglycidyl ether, 1,4-butanediol diglycidyl ether, and C... 12 ~C 14 One or more of alkyl glycidyl ethers; The multifunctional thiol curing agent is one or both of trimethylolpropane tris(3-mercaptopropionic acid) ester or pentaerythritol tetra(3-mercaptopropionic acid) ester. The curing accelerator is one or both of imidazole accelerators and modified amine accelerators; The silane coupling agent is selected from one or more of 3-glycidyl etheroxypropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, titanate coupling agents, and aluminate coupling agents.
8. A method for preparing a resin composition based on a supramolecular thixotropic network structure, characterized in that, Includes the following steps: a) Mix epoxy resin and reactive diluent to obtain the first component; b) Mix the first component with the thixotropic agent to obtain the second component; c) Mix the second component, the multifunctional thiol curing agent, the curing accelerator and the silane coupling agent to obtain the third component; d) The third component, defoamer, and pigment are mixed to obtain a resin composition.
9. The preparation method according to claim 8, characterized in that, In step a), the mixing temperature is 15℃~25℃, and the rotation speed is 300rpm / min~500rpm / min; In step b), the mixing temperature is 40℃~50℃, the rotation speed is 800rpm / min~1200rpm / min, and the time is 30min~60min; In step c), the mixing temperature is 0℃~25℃, the rotation speed is 400rpm / min~600rpm / min, and the time is 20min~30min.
10. A one-component epoxy resin adhesive based on a supramolecular thixotropic network structure, characterized in that, The resin composition includes any one of claims 1 to 7 or the resin composition prepared by the preparation method of claim 8 or 9.