A one-component underfill adhesive with high glass transition temperature and its preparation method

By preparing a single-component underfill adhesive with a high glass transition temperature, the problems of high curing temperature, low glass transition temperature and poor storage stability in the existing technology are solved. It achieves medium-temperature rapid curing and excellent storage stability, is suitable for high-precision packaging processes, and extends the life of electronic devices.

CN123107598APending Publication Date: 2026-11-17广东省博翔新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611483743.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-22
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing single-component underfill adhesives suffer from problems such as high curing temperature, low glass transition temperature, poor storage stability, and insufficient narrow gap filling ability, making it difficult to meet the requirements of high-precision, high-volume automated packaging.

Method used

A single-component underfill adhesive with a high glass transition temperature is prepared by using multifunctional epoxy resin, silane coupling agent, latent curing agent and curing accelerator, etc., through specific mixing and processing technology, so as to achieve medium-temperature rapid curing and excellent storage stability.

Benefits of technology

It enables convenient operation without on-site mixing, reduces energy consumption, improves packaging yield and operation efficiency, adapts to advanced packaging processes, and extends the life of electronic devices.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention relates to the field of polymer materials technology for electronic packaging, and discloses a single-component underfill adhesive with a high glass transition temperature and its preparation method. The underfill adhesive is composed of a multifunctional epoxy resin, a silane coupling agent, a latent curing agent, and a curing accelerator, forming a homogeneous single-component system. Reactive diluents, toughening agents, spherical fused silica, and antioxidants can also be added as needed. This invention achieves a long storage period of ≥6 months at -20°C through a latent curing system and rapid curing at a medium temperature of 120–150°C. The multifunctional epoxy resin constructs a high cross-linking density network, resulting in a glass transition temperature ≥120°C after curing, while also exhibiting a low coefficient of thermal expansion and excellent narrow-gap flow and filling properties. This product requires no on-site mixing, has a wide process window, and is suitable for large-scale automated packaging processes such as flip-chip bonding, BGA, and CSP. It can effectively alleviate thermal mismatch stress, improve the high-temperature reliability and service life of packaged devices, and has broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polymer materials technology for electronic packaging, specifically a single-component underfill adhesive with a high glass transition temperature and its preparation method. Background Technology

[0002] Underfill is an adhesive primarily composed of epoxy resin, used to fill the gaps between chips in BGA, CSP, and Flip Chip packages. Through heat curing, it fills the tiny voids between the chip and the substrate over a large area, thereby dispersing stress on solder joints, protecting the chip and solder joints, and extending the lifespan of electronic products. With the increasing demands for high performance, multifunctionality, and portability in electronic components, and the continuous improvement in packaging density, higher requirements are being placed on the heat resistance, storage stability, filling capacity, and process adaptability of underfill adhesives.

[0003] Currently, underfill adhesives are mainly divided into two categories: two-component systems and one-component systems. Two-component systems require mixing in a specific ratio before use, which has drawbacks such as cumbersome operation, performance fluctuations due to mixing ratio deviations, short pot life, and susceptibility to air bubble inclusion. These drawbacks make it difficult to meet the requirements of high-precision, high-volume automated packaging production lines for process stability and operational consistency. In contrast, one-component underfill adhesives, due to their elimination of on-site mixing, simple application process, and stable dispensing quality, have become the mainstream development direction in the packaging industry.

[0004] However, existing single-component underfill adhesives still have many technical bottlenecks: First, the curing temperature is generally too high, often requiring long-term baking at temperatures above 180°C, which can easily damage thermistor devices and consume a lot of energy; Second, the glass transition temperature (Tg) after curing is too low, with most products having a Tg of less than 100°C, making it difficult to withstand the high-temperature impact of 260°C during lead-free reflow soldering, and the adhesive layer is prone to softening and failure at high temperatures; Third, it is difficult to balance storage stability and curing activity, as premature gelation is likely to occur at room temperature, and the low-temperature storage period is generally less than 3 months; Fourth, the narrow gap filling capability is insufficient, making it difficult to adapt to high-end micro-pitch encapsulation processes below 50μm. Summary of the Invention

[0005] This invention provides a single-component bottom filler with a high glass transition temperature and its preparation method, which solves the problems mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] A single-component underfill adhesive with a high glass transition temperature, comprising, by weight, 30-80 parts of multifunctional epoxy resin, 0.5-3 parts of silane coupling agent, 3-15 parts of latent curing agent, and 0.5-3 parts of curing accelerator.

[0008] As a preferred embodiment of the present invention, the multifunctional epoxy resin is at least one of alicyclic epoxy, phenolic epoxy, cresol-formaldehyde epoxy, dicyclopentadiene epoxy, and tetrafunctional glycidylamine epoxy resin, with an epoxy equivalent of 160-250 g / eq.

[0009] As a preferred embodiment of the present invention, the silane coupling agent is at least one of γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

[0010] As a preferred embodiment of the present invention, the latent curing agent is at least one of dicyandiamide, adipic acid dihydrazide, microcapsule-coated imidazole, and boron trifluoride monoethylamine complex, wherein the microcapsule-coated imidazole includes 2-ethyl-4-methylimidazolium microcapsules and 2-phenylimidazolium microcapsules, and the curing accelerator is at least one of 2-methylimidazolium, 1-benzyl-2-methylimidazolium, and organic urea accelerators.

[0011] As a preferred embodiment of the present invention, the raw materials further include, by weight parts: 5-20 parts of reactive diluent, 5-15 parts of toughening agent, 100-200 parts of spherical fused silica, and 0.5-3 parts of antioxidant.

[0012] As a preferred embodiment of the present invention, the reactive diluent is at least one of p-tert-butylphenyl glycidyl ether, o-tolyl glycidyl ether, and 1,4-butanediol diglycidyl ether; the toughening agent is at least one of carboxyl-terminated nitrile rubber, core-shell rubber, and polyethersulfone; and the antioxidant is a hindered phenolic antioxidant.

[0013] As a preferred embodiment of the present invention, the average particle size of the spherical molten silica is 1 to 3 μm.

[0014] A method for preparing a one-component underfill adhesive with a high glass transition temperature includes the following steps:

[0015] S1. Add the multifunctional epoxy resin and silane coupling agent to the reactor and stir and mix at 25-70°C for 30-60 minutes until homogeneous and transparent to obtain the resin matrix premix.

[0016] S2. Cool the resin matrix premix to room temperature, add the curing accelerator, and stir and mix for 20 to 80 minutes under vacuum conditions of -0.09 to -0.1 MPa and 15 to 25°C until homogeneous. During the stirring process, control the material temperature to ≤40°C.

[0017] S3. Add the latent curing agent to the above well dispersed mixture and stir at low speed for 20-30 minutes at ≤25℃ to fully disperse the curing agent system.

[0018] S4. Degas the final mixture under vacuum for 1-15 minutes, filter the mixture, seal it in a moisture-proof container, and store it at -20°C.

[0019] As a preferred embodiment of the present invention, in step S3, the ambient humidity of all operations is ≤50%RH.

[0020] The present invention has the following advantages:

[0021] 1. Convenience of single components: No on-site mixing required, ready to use after opening the can, eliminating the risk of mixing errors and air bubble encapsulation, significantly improving packaging yield and operational efficiency, and suitable for large-scale automated production lines.

[0022] 2. Excellent storage stability: It can be stored at -20℃ for more than 6 months, which greatly reduces transportation and storage requirements and facilitates production line scheduling.

[0023] 3. Medium-temperature rapid curing: It can be fully cured in 45 to 90 minutes at 120 to 150℃, without the need for long-term baking at temperatures above 180℃, thus reducing energy consumption and ensuring compatibility with heat-sensitive devices.

[0024] 4. High heat resistance and reliability: After curing, the Tg reaches above 120℃, which can withstand the high temperature impact of 260℃ in lead-free reflow soldering, avoiding the softening and failure of the adhesive layer at high temperature; at the same time, the low coefficient of thermal expansion in the glass state has a small thermal mismatch with silicon chips and organic substrates, which can effectively buffer the interface stress during temperature cycling, reduce the risk of fatigue cracking of solder joints, and extend the service life of electronic devices.

[0025] 5. Excellent narrow gap filling performance: It can completely fill the bottom gap of chips of 50μm and below, and is compatible with advanced packaging processes such as fine-pitch flip-chip bonding and high-end BGA / CSP, ensuring the consistency and yield of batch packaging. Detailed Implementation

[0026] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0027] Example 1

[0028] A one-component underfill adhesive with a high glass transition temperature, the formulation of which is as follows (by parts by weight):

[0029] 70 parts of multifunctional epoxy resin (phenolic epoxy, epoxy equivalent 200g / eq), 10 parts of p-tert-butylphenyl glycidyl ether, 8 parts of CTBN (carboxyl-terminated butadiene-acrylonitrile rubber) toughening agent, 1.5 parts of KH-560 silane coupling agent, 150 parts of spherical fused silica (average particle size 2μm), 8 parts of microencapsulated 2-ethyl-4-methylimidazole (latent curing agent), 0.5 parts of 2-methylimidazole (curing accelerator), and 1 part of antioxidant 1010.

[0030] Preparation method:

[0031] S1. Add phenolic epoxy resin, reactive diluent, toughening agent and coupling agent to the reactor, and stir at 70℃ for 45 minutes until homogeneous;

[0032] S2. Cool to room temperature, add 2-methylimidazole and silica in three batches, disperse under vacuum of -0.095MPa and rotation speed of 1000r / min for 75min, and control the material temperature ≤38℃;

[0033] S3. Under nitrogen protection or strict dehumidification environment (ambient humidity ≤50%RH), premix the curing accelerator (2-methylimidazole) and antioxidant evenly, add them to the above system, and stir at low speed (400r / min) for 25min at 25℃ until completely dispersed to prevent latent curing agent from absorbing moisture and failing.

[0034] S4. Vacuum degassing for 15 minutes, filter out the material, seal it in an aluminum-plastic composite bag, and refrigerate at -20℃.

[0035] Performance test results:

[0036] 1. Storage period (-20℃): >8 months (viscosity increase ≤15%);

[0037] 2. Curing conditions: Thaw and warm to room temperature, apply adhesive to fill 40μm gaps, and cure at 140℃ for 60min;

[0038] 3. Tg (DSC): 163℃; CTE (TMA, <Tg):26ppm / ℃;

[0039] 4. Viscosity at 25℃: 4800 mPa・s; completely filled with no voids;

[0040] 5. Shear strength (Al-Al): 23.0 MPa; no cracks after reflow soldering at 260℃.

[0041] Example 2

[0042] A one-component underfill adhesive with a high glass transition temperature, the formulation of which is as follows (by parts by weight):

[0043] 80 parts of cresol-formaldehyde epoxy resin (epoxy equivalent 210), 5 parts of o-tolyl glycidyl ether, 12 parts of core-shell rubber (butadiene core / PMMA shell), 2 parts of KH-560, 180 parts of spherical fused silica (average particle size 3μm), 10 parts of dicyandiamide (latent curing agent), 1.5 parts of organic urea accelerator (UR-500), and 1.5 parts of antioxidant 1076.

[0044] The preparation method is the same as in Example 1, with the temperature controlled at ≤30℃ during the mixing stage.

[0045] Curing conditions: 150℃ / 45min.

[0046] Performance test results: Tg=170℃, CTE=24ppm / ℃, viscosity=5900mPa・s, shear strength=24.5MPa, no defects in the 50μm gap, storage period at -20℃>7 months.

[0047] Example 3

[0048] A one-component underfill adhesive with a high glass transition temperature, the formulation of which is as follows (by parts by weight):

[0049] 60 parts of dicyclopentadiene epoxy resin (epoxy equivalent 230), 20 parts of 1,4-butanediol diglycidyl ether, 5 parts of polyethersulfone (toughening agent), 3 parts of KH-550, 200 parts of spherical fused silica (average particle size 1μm), 12 parts of adipic acid dihydrazide (latent curing agent), 2 parts of 1-benzyl-2-methylimidazolium, and 2 parts of antioxidant 168.

[0050] The preparation method is the same as in Example 1, with the temperature controlled at ≤35℃ during the mixing stage.

[0051] Curing conditions: 130℃ / 90min.

[0052] Performance test results: Tg=157℃, CTE=28ppm / ℃, viscosity=7300mPa・s, shear strength=21.2MPa, gap 35μm fully filled, storage period at -20℃>6 months.

[0053] Comparative Example 1 (Non-latent system)

[0054] The microcapsule curing agent was replaced with an equal amount of unencapsulated 2-ethyl-4-methylimidazole, and the rest of the formulation and process were the same as in Example 1.

[0055] Performance results: The viscosity increased sharply during the mixing process, making it impossible to achieve uniform dispersion at 25°C. The adhesive gelled and solidified within 2 hours, making it impossible to prepare a storable single-component product.

[0056] Comparative Example 2 (Using ordinary bisphenol A epoxy resin instead of multifunctional resin)

[0057] The phenolic epoxy was replaced with bisphenol A epoxy resin E51, and the rest of the formulation, process and curing conditions were the same as in Example 1.

[0058] Performance results: The Tg after curing was only 92℃, and microcracks appeared after reflow soldering at 260℃.

[0059] Comparative Example 3 (Insufficient amount of latent curing agent)

[0060] The rest is the same as in Example 1, except that the amount of microcapsule curing agent is reduced to 2 parts.

[0061] Performance results: After curing at 140℃ for 60min, the residual exothermic peak of DSC was obvious, the crosslinking was incomplete, and the Tg was only 98℃, which could not meet the usage requirements.

[0062] The comparative analysis of the above embodiments and comparative examples shows that the present invention successfully resolves the contradiction between storage stability and curing activity in a single-component system by introducing microcapsules or a dicyandiamide-based latent curing system; the use of multifunctional epoxy resin is key to achieving a high Tg (≥120℃). The organic combination of these two factors results in the single-component underfill adhesive of the present invention exhibiting significantly better overall performance than conventional solutions, fully meeting the requirements of advanced encapsulation for highly reliable underfill materials.

[0063] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, it is intended that all variations falling within the meaning and scope of equivalents of the claims be included within the present invention.

Claims

1. A high glass transition temperature one-part underfill adhesive characterized in that, By weight, the raw materials include: 30-80 parts of multifunctional epoxy resin, 0.5-3 parts of silane coupling agent, 3-15 parts of latent curing agent, and 0.5-3 parts of curing accelerator.

2. The high glass transition temperature single component underfill adhesive of claim 1, wherein, The multifunctional epoxy resin is at least one of alicyclic epoxy, phenolic epoxy, cresol-formaldehyde epoxy, dicyclopentadiene epoxy, and tetrafunctional glycidylamine epoxy resin, with an epoxy equivalent of 160-250 g / eq.

3. The high glass transition temperature single component underfill adhesive of claim 1, wherein, The silane coupling agent is at least one of γ-glycidoxypropyltrimethoxysilane and γ-aminopropyltriethoxysilane.

4. The high glass transition temperature single component underfill adhesive of claim 1, wherein, The latent curing agent is at least one of dicyandiamide, adipic acid dihydrazide, microencapsulated imidazole, and boron trifluoride monoethylamine complex, wherein the microencapsulated imidazole includes 2-ethyl-4-methylimidazolium microcapsules and 2-phenylimidazolium microcapsules, and the curing accelerator is at least one of 2-methylimidazolium, 1-benzyl-2-methylimidazolium, and organic urea accelerators.

5. The high glass transition temperature single component underfill adhesive of claim 1, wherein, By weight, the raw materials also include: 5-20 parts of reactive diluent, 5-15 parts of toughening agent, 100-200 parts of spherical fused silica, and 0.5-3 parts of antioxidant.

6. The high glass transition temperature, one-part underfill adhesive of claim 5, wherein, The active diluent is at least one of p-tert-butylphenyl glycidyl ether, o-tolyl glycidyl ether, and 1,4-butanediol diglycidyl ether; the toughening agent is at least one of carboxyl-terminated nitrile rubber, core-shell rubber, and polyethersulfone; and the antioxidant is a hindered phenolic antioxidant.

7. The high glass transition temperature one-component underfill adhesive according to claim 5, characterized in that, The average particle size of the spherical molten silica is 1–3 μm.

8. A process for the preparation of a high glass transition temperature, one component underfill adhesive according to any one of claims 1 to 7, characterized in that, Includes the following steps: S1. Add the multifunctional epoxy resin and silane coupling agent to the reactor and stir and mix at 25-70°C for 30-60 minutes until homogeneous and transparent to obtain the resin matrix premix. S2. Cool the resin matrix premix to room temperature, add the curing accelerator, and stir and mix for 20 to 80 minutes under vacuum conditions of -0.09 to -0.1 MPa and 15 to 25°C until homogeneous. During the stirring process, control the material temperature to ≤40°C. S3. Add the latent curing agent to the above well dispersed mixture and stir at low speed for 20-30 minutes at ≤25℃ to fully disperse the curing agent system. S4. Degas the final mixture under vacuum for 1-15 minutes, filter the mixture, seal it in a moisture-proof container, and store it at -20°C.

9. The method for preparing a high glass transition temperature single-component bottom filler according to claim 8, characterized in that, The ambient humidity for all operations in step S3 is ≤50%RH.