A two-component addition-curing flame-retardant silicone containing fire-extinguishing microcapsules and its preparation method
By modifying the surface treatment of perfluorohexanone microcapsules and using composite flame retardants, the problems of catalyst poisoning and weak interfacial adhesion of microcapsules in liquid silica gel were solved, thus achieving the stability and effective fire extinguishing performance of the finished silica gel.
Patent Information
- Application Number
- CN202611198672.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-08
- Publication Date
- 2026-11-17
AI Technical Summary
In existing technologies, the curing of liquid silicone relies on a platinum catalyst. Residual nitrogen elements and free formaldehyde in the wall material of fire extinguishing microcapsules cause the catalyst to be implicitly poisoned. Furthermore, there are weak adhesion defects at the interface between the fire extinguishing microcapsules and the organosilicon matrix, which leads to premature leakage of the microcapsules during the mixing and vulcanization stages, thus failing to effectively exert their fire extinguishing and flame retardant effects.
Modified perfluorohexanone microcapsules were used, and a passivation capping layer was constructed on the surface of the microcapsules by a silane modifier. The microcapsules were then modified by secondary coating with low-viscosity vinyl silicone oil and MQ silicone resin to improve the interfacial bonding strength. At the same time, a composite flame retardant was used to form a dense glassy barrier layer to reduce the probability of microcapsule breakage during processing.
This ensures the effective loading of perfluorohexanone microcapsules in the finished silicone, achieving sufficient fire extinguishing and flame retardant effects in fire situations, while maintaining stability and mechanical properties under normal conditions, thus meeting the needs of all-area protection.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of flame retardant materials technology, and in particular to a two-component addition-type flame retardant silicone containing fire extinguishing microcapsules and its preparation method. Background Technology
[0002] Perfluorohexanone is a colorless, odorless, transparent, and non-conductive liquid at room temperature and pressure, with a boiling point of only 49.2℃. It possesses excellent fire extinguishing properties, but its low boiling point and high volatility present challenges in storage and application. To overcome this limitation, researchers have attempted to microencapsulate perfluorohexanone into solid microcapsules and then disperse them within a polymer matrix, aiming to achieve stable storage at room temperature and high-temperature trigger release of the fire extinguishing agent.
[0003] Among them, fire extinguishing microcapsules are prepared by coating perfluorohexanone with melamine-formaldehyde (MF) resin and / or urea-formaldehyde (UF) resin as wall materials. The fire extinguishing microcapsules are then incorporated into liquid silicone and used as sealants or potting compounds in the field of electronic packaging, which has already achieved a certain degree of application.
[0004] However, existing solutions still have pressing problems: On the one hand, the curing of liquid silicone relies on a hydrosilylation reaction catalyzed by a platinum catalyst. The wall material of the fire extinguishing microcapsule contains nitrogen and free formaldehyde residues, and nitrogen-containing compounds are typical poisons of platinum catalysts. When the wall material comes into contact with the platinum catalyst, a latent poisoning effect can easily occur, resulting in incomplete curing of the silicone. On the other hand, there is a "weak adhesion defect" at the interface between the fire extinguishing microcapsule and the silicone matrix. The fire extinguishing microcapsule may be uncontrolled pre-ruptured during the mixing or exothermic vulcanization stage of the adhesive, causing perfluorohexanone to leak prematurely before the finished silicone is exposed to fire. Ultimately, this results in a severe shortage of the number of effectively loaded perfluorohexanone microcapsules in the finished flame-retardant silicone, which cannot play the expected fire extinguishing and flame-retardant role when a fire breaks out. Summary of the Invention
[0005] In order to reduce the probability of pre-breakage of microcapsules during the mixing and vulcanization stages, ensure the retention rate of effective fire extinguishing components in the product, and give full play to the fire extinguishing and flame retardant effects, this application provides a two-component addition-type flame retardant silicone containing fire extinguishing microcapsules and its preparation method.
[0006] In the first aspect, this application provides a two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, which adopts the following technical solution: A two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, comprising the following raw materials by weight: Component A: 100 parts vinyl-terminated polydimethylsiloxane, 6-16 parts reinforcing agent, 6-26 parts composite flame retardant, 0.09-0.3 parts catalyst, 0.08-0.25 parts inhibitor, 0.1-0.8 parts anti-settling agent, and 0-2 parts color paste; Component B: 1-10 parts of hydrogen-containing silicone oil, 15-50 parts of modified perfluorohexanone microcapsules, 0.5-3 parts of adhesion promoter, and 0.1-0.8 parts of processing aid.
[0007] By employing the above-mentioned technical solution to coat and modify perfluorohexanone microcapsules, on the one hand, it can prevent nitrogen-containing residues in the wall material from contacting the platinum catalyst in the system, avoiding the catalyst from being poisoned, ensuring that the silicone system can achieve complete curing, and stabilizing the molding quality and basic mechanical properties of the finished product; on the other hand, the modification treatment can effectively improve the interfacial bonding strength between the microcapsules and the organosilicon matrix, improve the original weak interfacial bonding defects, significantly reduce the probability of uncontrolled pre-breakage of microcapsules during the mixing and vulcanization stages, reduce the premature leakage of perfluorohexanone before the finished product is molded, and ensure the number of perfluorohexanone microcapsules effectively loaded in the finished flame-retardant silicone, thereby ensuring that the finished silicone can fully exert the expected fire extinguishing and flame retardant effect when encountering fire, and obtain a finished flame-retardant silicone with stable and reliable flame retardant performance.
[0008] Under normal conditions (temperature < 100℃), the modified perfluorohexanone microcapsules are in a stable state. When a fire occurs (temperature ≥ 150℃), the composite flame retardant plays a passive flame retardant role, forming a dense, glassy barrier layer that slows down the conduction of oxygen and heat; the modified perfluorohexanone microcapsules begin to rupture, releasing perfluorohexanone vapor, which plays an active fire extinguishing role. With its excellent fluidity and dispersibility, it can easily penetrate narrow gaps, crevices, and other hidden corners to achieve all-round coverage and meet the needs of comprehensive protection.
[0009] Optionally, the preparation method of the modified perfluorohexanone microcapsules includes the following steps: (1) Mix the silane modifier with an ethanol solution and heat to hydrolyze to obtain a silane mixture; mix the perfluorohexanone microcapsules with a solvent, disperse evenly, add the silane mixture, stir evenly, add the catalyst, heat to react, filter, wash and dry after the reaction is complete to obtain closed microcapsules; (2) The sealed microcapsules are mixed with low-viscosity vinyl silicone oil and MQ silicone resin and stirred evenly to obtain modified perfluorohexanone microcapsules.
[0010] By employing the above technical solution, a silane modifier is grafted onto the surface of perfluorohexanone microcapsules through in-situ liquid-phase condensation to construct an organosiloxane passivation end-cap layer. This effectively seals the active nitrogen-containing groups on the original wall material surface of the microcapsules, blocking the poisoning effect of nitrogen-containing groups on the platinum catalyst in the system from the source. Simultaneously, it initially improves the surface hydrophobicity of the microcapsules and enhances their compatibility with the organosilicon matrix. Subsequent secondary coating modification with low-viscosity vinyl silicone oil and MQ silicone resin further constructs an organosilicon coating layer similar in composition to the silicone rubber matrix outside the passivation end-cap layer. The vinyl groups in this layer participate in the matrix crosslinking network during the subsequent mixing and vulcanization of components A and B, further optimizing the surface properties of the microcapsules, weakening the interfacial difference between the microcapsules as filler phase and the matrix, allowing for better dispersion in the silicone rubber system, avoiding local performance defects caused by uneven dispersion, and further reducing the risk of premature breakage and leakage of the microcapsules during processing. This ensures the stability of the microcapsules during long-term storage in the finished silicone and their reliable response to fire.
[0011] Optionally, the low-viscosity vinyl silicone oil has a viscosity of 200–800 mPa·s and a vinyl content of 3%–5%; the MQ silicone resin has an M / Q value of 0.6–0.8.
[0012] By adopting the above technical solution, controlling the viscosity and vinyl content of the low-viscosity vinyl silicone oil within this range ensures that the silicone oil has good fluidity, fully impregnates and disperses the closed microcapsule particles, and guarantees a uniform encapsulation process. It also provides sufficient vinyl sites to participate in the cross-linking reaction, allowing the microcapsule surface coating layer to firmly bond to the cross-linking network of the silicone rubber matrix. Furthermore, controlling the M / Q value of the MQ silicone resin within the range of 0.6 to 0.8 allows the MQ silicone resin to possess both suitable structural stability and reactivity, enabling it to synergistically form a uniform and dense coating layer with the vinyl silicone oil. This avoids insufficient structural strength due to an excessively high M / Q value, and also prevents decreased compatibility and the precipitation of free components that could affect the performance of the finished silicone product due to an excessively low M / Q value, effectively ensuring the secondary modification effect of the closed microcapsules.
[0013] Optionally, in step (1), the mass ratio of perfluorohexanone microcapsules to silane modifier is (20~40):1; in step (2), the mass ratio of blocked microcapsules, low-viscosity vinyl silicone oil and MQ silicone resin is 20:(4~7):(0.1~0.3).
[0014] By adopting the above technical solution, in step (1), the silane modifier at this ratio can form a complete, uniform, and appropriately thick passivated end-capping layer on the surface of the perfluorohexanone microcapsules. In step (2), the low-viscosity vinyl silicone oil and MQ silicone resin at this ratio can form a moderately thick and dense secondary modified coating layer on the surface of the sealed microcapsules, which can fully exert the effect of coating modification on improving interfacial compatibility and storage stability.
[0015] Optionally, the silane modifier includes one or more of perfluorooctyltriethoxysilane, vinyltriethoxysilane, and hexamethyldisilazane.
[0016] Preferably, the silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:(2~4).
[0017] By adopting the above technical solution, perfluorooctyltriethoxysilane can effectively reduce the surface energy of perfluorohexanone microcapsules, improve the interfacial compatibility between microcapsules and the silicone rubber matrix, reduce the probability of microcapsule particle aggregation, and enable them to be uniformly dispersed in the system. The vinyl groups carried by vinyltriethoxysilane can participate in the vulcanization and crosslinking reaction of addition-type silicone rubber, covalently anchoring the microcapsules in the crosslinked network structure of the silicone, effectively preventing microcapsule migration and precipitation during use, and improving the structural stability of the finished silicone. At this ratio, the two modified components can fully exert their synergistic effect, effectively improving the dispersion stability of the modified microcapsules in the silicone matrix without affecting the fire extinguishing performance of perfluorohexanone, and ensuring the uniformity of the finished silicone's properties.
[0018] Optionally, the composite flame retardant comprises polysiloxane and cyclic arylphosphazene derivatives in a mass ratio of (8~14):(2~4).
[0019] Preferably, the polysiloxane has a number-average molecular weight of 800–2500, a viscosity of 2000–8000 mPa·s, and a B content of 4 wt%–9 wt%; the cyclic arylphosphazene derivative is hexaphenoxycyclotriphosphazene.
[0020] By adopting the above technical solution, polysiloxane and hexaphenoxycyclotriphosphazene exert a synergistic flame-retardant effect. When heated, polysiloxane forms a continuous and dense high-strength borosilicate ceramic insulating carbon layer, covering the surface of the silicone matrix, isolating oxygen and heat transfer, and simultaneously preventing the outward diffusion of combustible small molecules generated by the thermal decomposition of the substrate. When cyclic arylphosphazene decomposes upon heating, it releases non-flammable gases, diluting the concentration of combustible gases. At the same time, the phosphorus-based component can capture active free radicals in the condensed phase, interrupting the combustion chain reaction. The combined effect of these two components further enhances the flame-retardant effect. Compared with the traditional aluminum hydroxide flame-retardant phase, the composite flame retardant used in this application requires only a lower addition amount to achieve the same or even better flame-retardant rating, reducing the negative impact of high-filling-content inorganic flame retardants on the mechanical and processing properties of silicone, and balancing the flame-retardant performance and physical processing properties of the material.
[0021] Optionally, the adhesion promoter includes one or both of KH-560 and vinyl MQ tackifying resin.
[0022] By adopting the above technical solution and adding an appropriate amount of adhesion promoter, the interfacial compatibility between the flame-retardant silicone matrix and the substrate being bonded can be effectively improved, enhancing the bonding strength between the two and broadening the application scenarios of the flame-retardant silicone to meet the needs of applications requiring fixed bonding. Specifically, KH-560 can form chemical bonds with the active sites on the substrate surface through the silanol groups generated by hydrolysis, while the vinyl MQ tackifying resin can carry its own vinyl groups to participate in the vulcanization crosslinking network of the silicone rubber. Both can function individually or synergistically to improve bonding stability.
[0023] Secondly, this application provides a method for preparing a two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules, which adopts the following technical solution: A method for preparing a two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules includes the following steps: S1.A component preparation: Mix vinyl-terminated polydimethylsiloxane with reinforcing agent, stir evenly, add composite flame retardant and anti-settling agent, continue stirring, vacuum, add catalyst, inhibitor and color paste, stir evenly and then seal and store. Preparation of S2.B component: Mix the hydrogen-containing silicone oil, adhesion promoter and processing aid evenly, add the modified perfluorohexanone microcapsules, stir at low temperature, disperse evenly and then seal and store. S3. Mixed use: Mix component A and component B evenly to obtain flame-retardant silicone, then use it for injection molding / potting / dispensing and staged vulcanization.
[0024] Preferably, in step S3, the mass ratio of component A to component B is 10:1.
[0025] By adopting the above technical solution, preparing components A and B separately and then sealing them for storage can prevent premature cross-linking reactions, effectively improving the storage stability of the finished raw materials and extending the storage period. After mixing components A and B, vulcanization allows the cross-linking reaction to proceed fully. The segmented vulcanization process enables the system to gradually complete cross-linking, reducing internal stress and porosity, ultimately resulting in a finished flame-retardant silicone product with a uniform structure and stable performance.
[0026] This application has the following beneficial effects: 1. Encapsulating and modifying perfluorohexanone microcapsules can, on the one hand, prevent nitrogen-containing residues in the wall material from contacting the platinum catalyst in the system, avoiding latent poisoning of the catalyst, ensuring complete curing of the silicone system, and stabilizing the molding quality and basic mechanical properties of the finished product; on the other hand, the modification treatment can effectively improve the interfacial bonding strength between the microcapsules and the organosilicon matrix, improve the original weak interfacial adhesion defects, significantly reduce the probability of uncontrolled pre-breakage of microcapsules during mixing and vulcanization, reduce premature leakage of perfluorohexanone before the finished product is molded, and ensure the number of perfluorohexanone microcapsules effectively loaded in the finished flame-retardant silicone, thereby ensuring that the finished silicone can fully exert the expected fire extinguishing and flame retardant effect when encountering fire, and obtain a finished flame-retardant silicone with stable and reliable flame retardant performance.
[0027] Under normal conditions, the modified perfluorohexanone microcapsules are in a stable state. When a fire occurs, the composite flame retardant plays a passive flame-retardant role, forming a dense, glassy barrier layer that slows down the conduction of oxygen and heat; the modified perfluorohexanone microcapsules begin to rupture, releasing perfluorohexanone vapor, which plays an active fire-extinguishing role. With its excellent fluidity and dispersibility, it can easily penetrate narrow gaps, crevices, and other hidden corners, achieving all-round coverage and meeting the needs of comprehensive protection.
[0028] 2. A silane modifier is grafted onto the surface of perfluorohexanone microcapsules via in-situ liquid-phase condensation to construct an organosiloxane passivation end-cap layer. This effectively seals the active nitrogen-containing groups on the original wall material surface of the microcapsules, blocking the poisoning effect of nitrogen-containing groups on the platinum catalyst from the source. Simultaneously, it initially improves the surface hydrophobicity of the microcapsules and enhances their compatibility with the organosilicon matrix. Subsequent secondary coating modification with low-viscosity vinyl silicone oil and MQ silicone resin further constructs an organosilicon coating layer similar in composition to the silicone rubber matrix outside the passivation end-cap layer. The vinyl groups in this layer participate in the matrix crosslinking network during the subsequent mixing and vulcanization of components A and B, further optimizing the surface properties of the microcapsules, weakening the interfacial difference between the microcapsules as a filler phase and the matrix, allowing for better dispersion in the silicone rubber system, avoiding local performance defects caused by uneven dispersion, and further reducing the risk of premature breakage and leakage during processing. This ensures the stability of the microcapsules during long-term storage in the finished silicone and their reliable response to fire. Detailed Implementation
[0029] The present application will be further described in detail below with reference to the embodiments.
[0030] Preparation Example 1 The preparation method of perfluorohexanone microcapsules includes the following steps: S1. Mix 7.5g melamine, 7.3g urea, and 30g formaldehyde aqueous solution (concentration of 37%), adjust the pH to 8.5 with triethanolamine, and stir at 300rpm for 1h under water bath heating at 70℃ to obtain melamine urea-formaldehyde resin prepolymer. S2. Dissolve 0.2g OP-10 and 0.2g Tween 20 in 10mL N,N-dimethylacetamide to obtain an emulsifier solution; mix 5mL perfluorohexanone and 5mL methyl nonafluorobutyl ether, add the emulsifier solution under stirring, and continue stirring and emulsifying at 2000rpm for 20min to form a core material emulsion; S3. Melamine urea-formaldehyde resin prepolymer was slowly added dropwise to the core material emulsion. After the addition was complete, the pH value was adjusted to 6 with citric acid. The temperature was slowly raised to 45°C and reacted for 2 hours. A 10% sodium carbonate solution was added and the mixture was stirred at 300 rpm for 15 minutes to remove residual free formaldehyde from the solution. After the reaction product cooled, it was washed with deionized water, filtered, and vacuum dried to obtain perfluorohexanone microcapsules.
[0031] Preparation Example 2-1 The preparation method of modified perfluorohexanone microcapsules includes the following steps: (1) Weigh perfluorohexanone microcapsules and silane modifier at a mass ratio of 40:1. Mix silane modifier with 95wt% ethanol solution at a mass ratio of 1:5 and heat in a water bath to 50℃ for 40 min to hydrolyze and obtain silane mixture. Mix perfluorohexanone microcapsules with solvent (solvent is a mixture of anhydrous ethanol and isopropanol at a mass ratio of 3:2) at a mass ratio of 1:9. After dispersing evenly, add silane mixture and stir evenly. Then add acetic acid to adjust pH to 4.5 and heat to 45℃ for 1.5 h. After the reaction is completed, filter, wash and dry to obtain closed microcapsules.
[0032] The perfluorohexanone microcapsules were prepared in Preparation Example 1.
[0033] The silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:2.
[0034] (2) Weigh the closed microcapsules, low viscosity vinyl silicone oil and MQ silicone resin according to the mass ratio of 20:4:0.1, and mix the closed microcapsules with the low viscosity vinyl silicone oil and MQ silicone resin. Stir evenly at 100 rpm to obtain modified perfluorohexanone microcapsules.
[0035] The low-viscosity vinyl silicone has a viscosity of 200 mPa·s and a vinyl content of 3%.
[0036] The M / Q value of MQ silicone resin is 0.6.
[0037] Preparation Example 2-2 The preparation method of modified perfluorohexanone microcapsules includes the following steps: (1) Weigh perfluorohexanone microcapsules and silane modifier at a mass ratio of 30:1. Mix silane modifier with 95wt% ethanol solution at a mass ratio of 1:5 and heat in a water bath to 50℃ for 40 min to hydrolyze and obtain silane mixture. Mix perfluorohexanone microcapsules with solvent (solvent is a mixture of anhydrous ethanol and isopropanol at a mass ratio of 3:2) at a mass ratio of 1:9. After dispersing evenly, add silane mixture, stir evenly, add acetic acid to adjust pH to 5, heat to 55℃ for 2 h, filter, wash and dry after reaction to obtain closed microcapsules.
[0038] The perfluorohexanone microcapsules were prepared in Preparation Example 1.
[0039] The silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:4.
[0040] (2) Weigh the closed microcapsules, low viscosity vinyl silicone oil and MQ silicone resin according to the mass ratio of 20:5:0.2, and mix the closed microcapsules with the low viscosity vinyl silicone oil and MQ silicone resin. Stir evenly at 200 rpm to obtain modified perfluorohexanone microcapsules.
[0041] The low-viscosity vinyl silicone has a viscosity of 600 mPa·s and a vinyl content of 5%.
[0042] The M / Q value of MQ silicone resin is 0.8.
[0043] Preparation Examples 2-3 The preparation method of modified perfluorohexanone microcapsules includes the following steps: (1) Weigh perfluorohexanone microcapsules and silane modifier at a mass ratio of 20:1. Mix silane modifier with 95wt% ethanol solution at a mass ratio of 1:5 and heat in a water bath to 50℃ for 40 min to hydrolyze and obtain silane mixture. Mix perfluorohexanone microcapsules with solvent (solvent is a mixture of anhydrous ethanol and isopropanol at a mass ratio of 3:2) at a mass ratio of 1:9. After dispersing evenly, add silane mixture and stir evenly. Then add acetic acid to adjust pH to 4.5 and heat to 65℃ for 2.5 h. After the reaction is completed, filter, wash and dry to obtain closed microcapsules.
[0044] The perfluorohexanone microcapsules were prepared in Preparation Example 1.
[0045] The silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:3.
[0046] (2) Weigh the closed microcapsules, low viscosity vinyl silicone oil and MQ silicone resin according to the mass ratio of 20:7:0.3, and mix the closed microcapsules with the low viscosity vinyl silicone oil and MQ silicone resin. Stir evenly at 300 rpm to obtain modified perfluorohexanone microcapsules.
[0047] The low-viscosity vinyl silicone has a viscosity of 400 mPa·s and a vinyl content of 4%.
[0048] The M / Q value of MQ silicone resin is 0.7.
[0049] Preparation Examples 2-4 The difference between this preparation example and Preparation Examples 2-3 is that the silane modifier used in this example is vinyltriethoxysilane alone. That is, perfluorooctyltriethoxysilane is replaced by vinyltriethoxysilane in equal mass.
[0050] Preparation Examples 2-5 The difference between this preparation example and preparation examples 2-3 is that the low viscosity vinyl silicone oil in step (2) is replaced by a low viscosity vinyl silicone oil with a vinyl content of 0.5 wt%.
[0051] Preparation Examples 2-6 The difference between this preparation example and preparation examples 2-3 is that the preparation method of the modified perfluorohexanone microcapsules includes the following steps: Weigh perfluorohexanone microcapsules and silane modifier separately at a mass ratio of 20:1. Mix the silane modifier with a 95wt% ethanol solution at a mass ratio of 1:5 and heat in a water bath to 50℃ for 40 min to hydrolyze, obtaining a silane mixture. Mix the perfluorohexanone microcapsules with a solvent (the solvent is a mixture of anhydrous ethanol and isopropanol at a mass ratio of 3:2) at a mass ratio of 1:9. After dispersing evenly, add the silane mixture, stir evenly, add acetic acid to adjust the pH to 4.5, heat to 65℃ and react for 2.5 h. After the reaction is complete, filter, wash and dry to obtain modified perfluorohexanone microcapsules.
[0052] The perfluorohexanone microcapsules were prepared in Preparation Example 1.
[0053] The silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:3.
[0054] Example
[0055] Example 1 A two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, comprising the following raw materials: Component A: 100 parts vinyl-terminated polydimethylsiloxane, 8 parts reinforcing agent, 8 parts polysiloxane, 2 parts hexaphenoxycyclotriphosphazene, 0.12 parts catalyst, 0.1 parts 1-ethynyl-1-cyclohexanol, 0.02 parts triphenylphosphine, 0.3 parts anti-settling agent, and 1 part color paste; Component B: 3 parts of hydrogen-containing silicone oil, 25 parts of modified perfluorohexanone microcapsules, 1 part of KH-560, and 0.2 parts of BYK-085 defoamer.
[0056] The vinyl-terminated polydimethylsiloxane has a viscosity of 10,000 mPa·s and a vinyl content of 0.15 wt%.
[0057] The reinforcing agent was hydrophobic fumed silica, purchased from Hubei Huifu Nanomaterials Co., Ltd., model number HB-630.
[0058] The polysiloxane has a number average molecular weight of 1000, a viscosity of 2000 mPa∙s, and a boron content of 4 wt%.
[0059] The catalyst was a platinum catalyst, purchased from Shenzhen Tianqi New Materials Technology Co., Ltd., model SK-P050, with a platinum content of 5000ppm.
[0060] The antisettling agent is BENTONE 27 bentonite.
[0061] The color paste is a commercially available product, purchased from Dongguan Caimijia Electronic Technology Co., Ltd., CAS No. 1333-86-4.
[0062] The viscosity of the hydrogen-containing silicone oil is 30 mPa∙s, and the hydrogen content is 1 wt%.
[0063] The modified perfluorohexanone microcapsules were prepared according to Preparation Example 2-1.
[0064] The preparation method of the two-component addition-curing flame-retardant silicone for fire extinguishing microcapsules includes the following steps: Preparation of S1.A component: Vinyl-terminated polydimethylsiloxane was mixed with hydrophobic fumed silica and stirred evenly. Polysiloxane, hexaphenoxycyclotriphosphazene and BENTONE 27 bentonite were added and stirred. Vacuum degassing was carried out at -0.095 MPa for 20 min. Platinum catalyst, 1-ethynyl-1-cyclohexanol, triphenylphosphine and color paste were added. After stirring evenly, the mixture was sealed and stored. Preparation of S2.B component: Mix hydrogen-containing silicone oil, KH-560 and BYK-085 defoamer evenly, add modified perfluorohexanone microcapsules, stir at 25°C, disperse evenly, and then seal and store. S3. Mixed use: Add component A and component B to a double planetary mixer at a mass ratio of 10:1, stir evenly at 25°C to obtain flame-retardant silicone. After injection molding / potting / dispensing, cure at 80°C for 30 minutes, and then heat to 120°C for 60 minutes.
[0065] Example 2 A two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, comprising the following raw materials: Component A: 100 parts vinyl-terminated polydimethylsiloxane, 10 parts reinforcing agent, 11 parts polysiloxane, 3 parts hexaphenoxycyclotriphosphazene, 0.15 parts catalyst, 0.11 parts 1-ethynyl-1-cyclohexanol, 0.04 parts triphenylphosphine, and 0.4 parts anti-settling agent; Component B: 5 parts of hydrogen-containing silicone oil, 30 parts of modified perfluorohexanone microcapsules, 1.5 parts of KH-560, and 0.3 parts of BYK-085 defoamer.
[0066] The vinyl-terminated polydimethylsiloxane has a viscosity of 15000 mPa·s and a vinyl content of 0.15 wt%.
[0067] The reinforcing agent was hydrophobic fumed silica, purchased from Hubei Huifu Nanomaterials Co., Ltd., model number HB-630.
[0068] The polysiloxane has a number average molecular weight of 1500, a viscosity of 5000 mPa∙s, and a boron content of 7 wt%.
[0069] The catalyst was a platinum catalyst, purchased from Shenzhen Tianqi New Materials Technology Co., Ltd., model SK-P050, with a platinum content of 5000ppm.
[0070] The antisettling agent is BENTONE 27 bentonite.
[0071] The viscosity of the hydrogen-containing silicone oil is 50 mPa∙s, and the hydrogen content is 1 wt%.
[0072] The modified perfluorohexanone microcapsules were prepared according to Preparation Example 2-2.
[0073] The preparation method of the two-component addition-curing flame-retardant silicone for fire extinguishing microcapsules includes the following steps: Preparation of S1.A component: Vinyl-terminated polydimethylsiloxane was mixed with hydrophobic fumed silica and stirred evenly. Polysiloxane, hexaphenoxycyclotriphosphazene and BENTONE 27 bentonite were added and stirred. Vacuum degassing was carried out at -0.095 MPa for 20 min. Platinum catalyst, 1-ethynyl-1-cyclohexanol and triphenylphosphine were added. After stirring evenly, the mixture was sealed and stored. Preparation of S2.B component: Mix hydrogen-containing silicone oil, KH-560 and BYK-085 defoamer evenly, add modified perfluorohexanone microcapsules, stir at 25°C, disperse evenly, and then seal and store. S3. Mixed use: Add component A and component B to a double planetary mixer at a mass ratio of 10:1, stir evenly at 25°C to obtain flame-retardant silicone. After injection molding / potting / dispensing, cure at 80°C for 30 minutes, and then heat to 120°C for 60 minutes.
[0074] Example 3 A two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, comprising the following raw materials: Component A: 100 parts vinyl-terminated polydimethylsiloxane, 12 parts reinforcing agent, 14 parts polysiloxane, 4 parts hexaphenoxycyclotriphosphazene, 0.18 parts catalyst, 0.13 parts 1-ethynyl-1-cyclohexanol, 0.05 parts triphenylphosphine, and 0.5 parts anti-settling agent; Component B: 8 parts of hydrogen-containing silicone oil, 35 parts of modified perfluorohexanone microcapsules, 2 parts of KH-560, and 0.4 parts of BYK-085 defoamer.
[0075] The vinyl-terminated polydimethylsiloxane has a viscosity of 18000 mPa·s and a vinyl content of 0.15 wt%.
[0076] The reinforcing agent was hydrophobic fumed silica, purchased from Hubei Huifu Nanomaterials Co., Ltd., model number HB-630.
[0077] The polysiloxane has a number average molecular weight of 2000, a viscosity of 8000 mPa∙s, and a boron content of 9 wt%.
[0078] The catalyst was a platinum catalyst, purchased from Shenzhen Tianqi New Materials Technology Co., Ltd., model SK-P050, with a platinum content of 5000ppm.
[0079] The antisettling agent is BENTONE 27 bentonite.
[0080] The viscosity of the hydrogen-containing silicone oil is 70 mPa∙s, and the hydrogen content is 1 wt%.
[0081] The modified perfluorohexanone microcapsules were prepared in Preparation Examples 2-3.
[0082] The preparation method of the two-component addition-curing flame-retardant silicone for fire extinguishing microcapsules includes the following steps: Preparation of S1.A component: Vinyl-terminated polydimethylsiloxane was mixed with hydrophobic fumed silica and stirred evenly. Polysiloxane, hexaphenoxycyclotriphosphazene and BENTONE 27 bentonite were added and stirred. Vacuum degassing was carried out at -0.095 MPa for 20 min. Platinum catalyst, 1-ethynyl-1-cyclohexanol and triphenylphosphine were added. After stirring evenly, the mixture was sealed and stored. Preparation of S2.B component: Mix hydrogen-containing silicone oil, KH-560 and BYK-085 defoamer evenly, add modified perfluorohexanone microcapsules, stir at 25°C, disperse evenly, and then seal and store. S3. Mixed use: Add component A and component B to a double planetary mixer at a mass ratio of 10:1, stir evenly at 25°C to obtain flame-retardant silicone. After injection molding / potting / dispensing, cure at 80°C for 30 minutes, and then heat to 120°C for 60 minutes.
[0083] Example 4 The difference between this embodiment and Embodiment 3 is that the polysiloxane is replaced by a polysiloxane with a B content of 0.5 wt%.
[0084] Example 5 The difference between this embodiment and Example 3 is that the modified perfluorohexanone microcapsules prepared in Examples 2-4 are used.
[0085] Example 6 The difference between this embodiment and Example 3 is that the modified perfluorohexanone microcapsules prepared in Examples 2-5 are used.
[0086] Example 7 The difference between this embodiment and Example 3 is that the modified perfluorohexanone microcapsules prepared in Examples 2-6 are used.
[0087] Comparative Example Comparative Example 1 A two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules differs from Example 3 in that the polysiloxane is replaced by hexaphenoxycyclotriphosphazene by mass.
[0088] Comparative Example 2 A two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules differs from Example 3 in that the hexaphenoxycyclotriphosphazene is replaced by polysiloxane by mass. The polysiloxane has a number-average molecular weight of 2000, a viscosity of 8000 mPa∙s, and a B content of 9 wt%.
[0089] Comparative Example 3 A two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules differs from Example 3 in that the composite flame retardant is replaced by aluminum hydroxide by mass.
[0090] Comparative Example 4 A two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules differs from Example 3 in that the modified perfluorohexanone microcapsules are replaced by the perfluorohexanone microcapsules prepared in Preparation Example 1. Performance testing
[0091] 1. Oxygen Index Determination: According to GB / T 10707-2088 "Determination of Burning Performance of Rubber", the sample size is 120mm×6.5mm (±0.5mm)×3mm (±0.25mm), with 5 samples in each group, and the average value is calculated.
[0092] 2. Vertical burning test: According to GB / T 2408-2008 "Determination of the flammability of plastics - Horizontal and vertical methods", the sample size is 100mm×13mm×3mm (±0.2mm), with 5 samples in each group, and the average value is calculated.
[0093] 3. The combustion behavior of flame-retardant silicone was tested according to GB / T 16172-2007 "Test Method for Heat Release Rate of Building Materials". The radiation power was 35kW, the sample size was 100mm×100mm×6mm (±0.5mm), and there were 3 samples in each group. The average value was calculated.
[0094] 4. Long-term environmental stability test: Components A and B in each example and comparative example were placed in a constant temperature and humidity chamber, and the conditions were set at 60°C and 90% RH for continuous storage for 6 months (simulating a long-term harsh environment). After the samples were taken out and restored to room temperature, step S3 was performed, and the combustion behavior test described above was repeated.
[0095] 5. Mechanical property testing: The tensile strength was tested according to GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber". The tensile strength was tested using a DL-D5000N rubber tensile testing machine with a tensile speed of 10 mm / min and a sample shape of 10 mm dumbbell.
[0096] Table 1
[0097] Based on the comparison between Examples 3 and 4 and the data in Table 1, it can be seen that increasing the boron content in polysiloxane helps improve the overall flame-retardant properties of the flame-retardant silicone. Higher boron content results in a higher oxygen index, a higher UL94 rating, a longer ignition time during combustion, and a shorter duration of open flame, while without significantly negatively impacting tensile strength. It is speculated that boron can promote the migration and enrichment of silicon elements to the surface of the flame-retardant silicone during combustion, forming a denser and more continuous barrier char layer, better blocking heat and oxygen transfer, and exhibiting superior condensed-phase flame-retardant effects without damaging the cross-linked structure of the silicone, thus maintaining good mechanical properties. Conversely, low boron content leads to discontinuous or insufficiently thick molten capping layers, failing to effectively isolate oxygen and heat transfer.
[0098] Based on the comparison between Examples 3 and 5 and the data in Table 1, it can be seen that: Example 3 involves in-situ condensation grafting of perfluorooctyltriethoxysilane and vinyltriethoxysilane onto the surface of perfluorohexanone microcapsules to construct a passivated end-capping layer, resulting in surface-inert microcapsules. This can block the implicit poisoning effect on the platinum catalyst, ensuring the normal progress of the curing reaction of the two-component addition-type silicone rubber. Simultaneously, the vinyl groups grafted onto the microcapsule surface can participate in the crosslinking reaction of the silicone rubber, covalently binding the microcapsules to the crosslinking network of the silicone rubber, significantly improving the interfacial bonding force between the microcapsules and the matrix, and preventing microcapsule aggregation, sedimentation, and leakage. In contrast, the perfluorohexanone microcapsules in Example 5 lack the modification effect of perfluorooctyltriethoxysilane on their surface. Therefore, active sites on the microcapsule surface may still exist, potentially poisoning the platinum catalyst, leading to insufficient crosslinking and curing of the system, and consequently, a decrease in flame retardant and mechanical properties.
[0099] Based on the comparison between Examples 3 and 6-7 and the data in Table 1, it can be seen that: since the vinyl groups grafted onto the surface of the microcapsules are the key sites for the vulcanization bonding between the microcapsules and the silicone rubber matrix, the less vinyl groups are grafted, the fewer active sites can participate in the cross-linking reaction, the looser the bonding between the microcapsules and the silicone rubber cross-linking network, and the significantly reduced interfacial bonding force. This not only makes it easier for the microcapsules to aggregate and settle, but also increases the number of defect points on the surface of the microcapsules, making it easier for perfluorohexanone inside the microcapsules to migrate outward, thus affecting the flame retardant stability of the silicone material.
[0100] According to the comparison between Example 3 and Comparative Examples 1 and 2, the flame retardant effect of polysiloxane and hexaphenoxycyclotriphosphazene compound is better than that of using either flame retardant component alone. The two can play a synergistic flame retardant role. Polysiloxane promotes the formation of a dense barrier char layer, while hexaphenoxycyclotriphosphazene can capture active free radicals during combustion and interrupt the combustion chain reaction. The combination of the two further improves the flame retardant efficiency.
[0101] Based on the comparison between Example 3 and Comparative Example 3, and the data in Table 1, it can be seen that the flame-retardant silicone rubber using aluminum hydroxide as a single flame retardant exhibits significantly lower performance in all aspects compared to Example 3, which uses a multi-component compound flame-retardant system. This indicates that, at the same addition amount, the flame-retardant efficiency of aluminum hydroxide is far lower than that of the ternary synergistic flame-retardant system composed of polysiloxane, hexaphenoxycyclotriphosphazene, and modified perfluorohexanone microcapsules. Aluminum hydroxide only relies on thermal decomposition to absorb heat and release water vapor to dilute combustibles, thus failing to adequately block oxygen and heat transfer in the condensed phase. It cannot achieve the multi-level protection effect of blocking heat transfer in the condensed phase, interrupting the chain reaction in the gas phase, and actively extinguishing the fire using microcapsules. Ultimately, this results in both flame-retardant and mechanical properties failing to meet the application requirements of this invention.
[0102] The comparison between Example 3 and Comparative Example 4 shows that the unmodified perfluorohexanone microcapsules have poor interfacial bonding with the silicone rubber matrix. The microcapsules are prone to sedimentation and aggregation, and premature leakage of perfluorohexanone. As a result, the flame retardant performance is far lower than that of Example 3 using modified microcapsules. In addition, the performance data after 180 days of long-term storage shows that the flame retardant performance of the unmodified sample decreases more after long-term storage, indicating that the microcapsule modification method used in this invention can effectively improve the long-term storage stability of flame-retardant silicone.
[0103] This specific embodiment is merely an explanation of this application and is not intended to limit it. After reading this specification, those skilled in the art can make modifications to this specific embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they fall within the scope of the claims of this application.
Claims
1. A two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules, characterized in that, By weight, it includes the following ingredients: Component A: 100 parts vinyl-terminated polydimethylsiloxane, 6-16 parts reinforcing agent, 6-26 parts composite flame retardant, 0.09-0.3 parts catalyst, 0.08-0.25 parts inhibitor, 0.1-0.8 parts anti-settling agent, and 0-2 parts color paste; Component B: 1-10 parts of hydrogen-containing silicone oil, 15-50 parts of modified perfluorohexanone microcapsules, 0.5-3 parts of adhesion promoter, and 0.1-0.8 parts of processing aid.
2. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 1, characterized in that, The preparation method of the modified perfluorohexanone microcapsules includes the following steps: (1) Mix the silane modifier with an ethanol solution and heat to hydrolyze to obtain a silane mixture; mix the perfluorohexanone microcapsules with a solvent, disperse evenly, add the silane mixture, stir evenly, add the catalyst, heat to react, filter, wash and dry after the reaction is complete to obtain closed microcapsules; (2) The closed microcapsules were mixed with low-viscosity vinyl silicone oil and MQ silicone resin and stirred evenly to obtain modified perfluorohexanone microcapsules.
3. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 2, characterized in that, The low-viscosity vinyl silicone oil has a viscosity of 200–800 mPa·s and a vinyl content of 3%–5%; the MQ silicone resin has an M / Q value of 0.6–0.
8.
4. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 2, characterized in that, In step (1), the mass ratio of perfluorohexanone microcapsules to silane modifier is (20~40):1; in step (2), the mass ratio of blocked microcapsules, low viscosity vinyl silicone oil and MQ silicone resin is 20:(4~7):(0.1~0.3).
5. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 2, characterized in that, The silane modifier includes one or more of perfluorooctyltriethoxysilane, vinyltriethoxysilane, and hexamethyldisilazane.
6. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 5, characterized in that, The silane modifier is a mixture of perfluorooctyltriethoxysilane and vinyltriethoxysilane in a molar ratio of 1:(2~4).
7. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 1, characterized in that, The composite flame retardant comprises polysiloxane and cyclic arylphosphazene derivatives in a mass ratio of (8~14):(2~4).
8. The two-component addition-cured flame-retardant silicone containing fire-extinguishing microcapsules according to claim 1, characterized in that, The adhesion promoter includes one or both of KH-560 and vinyl MQ tackifying resin.
9. A method for preparing a two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules according to any one of claims 1-8, characterized in that, Includes the following steps: S1.A component preparation: Mix vinyl-terminated polydimethylsiloxane with reinforcing agent, stir evenly, add composite flame retardant and anti-settling agent, continue stirring, vacuum, add catalyst, inhibitor and color paste, stir evenly and then seal and store. Preparation of S2.B component: Mix hydrogen-containing silicone oil, adhesion promoter and processing aid evenly, add modified perfluorohexanone microcapsules, stir at low temperature, disperse evenly and then seal and store. S3. Mixing: Mix component A and component B evenly to obtain flame-retardant silicone.
10. The method for preparing a two-component addition-type flame-retardant silicone containing fire-extinguishing microcapsules according to claim 9, characterized in that, In step S3, the mass ratio of component A to component B is 10:1.