High-leveling silicone thermally conductive potting compound based on filler compounding and anion / cation modification and its preparation method

By compounding fillers and modifying them with anions and cations, the contradiction between high thermal conductivity, high filling capacity, high leveling capacity, and low viscosity in existing technologies has been resolved, achieving a synergistic improvement in both thermal conductivity and leveling properties, and significantly improving the stability and flowability of the potting compound.

CN123107618APending Publication Date: 2026-11-17SHENZHEN AOCHUAN TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611568433.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicone thermally conductive potting compounds present irreconcilable contradictions in terms of synergistic effects on key indicators such as high thermal conductivity, high filler content, high leveling, and low viscosity. Specific problems include high filler content leading to a sharp increase in viscosity and poor flowability, easy agglomeration of fillers, weak interfacial bonding, and difficulty in forming a continuous and efficient thermally conductive network.

Method used

By employing filler compounding and anionic/cationic modification, modified silica powder and modified alumina are compounded with different particle sizes, and the powder surface is treated with cationic and anionic modifiers to form electrostatic adsorption aggregates, thereby improving the packing density and flowability of the filler and reducing viscosity.

Benefits of technology

It significantly improves the thermal conductivity and mechanical strength of the potting compound, maintains a low system viscosity and excellent leveling properties, and enhances the mechanical properties and long-term stability of the potting compound.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107618A_ABST
    Figure CN123107618A_ABST
Patent Text Reader

Abstract

This application provides a high-leveling silicone thermally conductive potting compound based on filler compounding and anion / cation modification, and its preparation method, relating to the field of thermally conductive potting compounds. It includes a first potting compound and a second potting compound with a mass ratio of 1:1. The first potting compound comprises 70-80 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-0.3 parts platinum catalyst, and 400-600 parts modified thermally conductive filler. The second potting compound comprises 70-80 parts vinyl silicone oil, 3-8 parts hydrogen-containing silicone oil, 0.1-0.3 parts inhibitor, and 400-600 parts modified thermally conductive filler. The modified thermally conductive filler comprises modified silica powder of a first particle size, modified alumina of a second particle size, and modified alumina of a third particle size. By compounding the modified thermally conductive filler with a multi-level particle size of modified silica powder of the first particle size, modified alumina of the second particle size, and modified alumina of the third particle size, the overall packing density of the filler is increased, significantly improving the thermal conductivity and mechanical strength of the potting compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of thermally conductive potting compounds, specifically to high-level silicone thermally conductive potting compounds based on filler compounding and anion-cation modification, and their preparation methods. Background Technology

[0002] Silicone thermally conductive potting compounds have become key encapsulation materials for high heat flux density electronic devices such as new energy vehicle electronic controls, power modules, and LED driver power supplies due to their excellent high and low temperature resistance, electrical insulation, chemical stability, and low stress characteristics. Their core function is to provide physical protection, moisture resistance, insulation, stress buffering, and efficient thermal conductivity and dissipation for electronic components through potting and curing, thereby ensuring the long-term reliability of devices under complex operating conditions.

[0003] Existing silicone thermally conductive potting compounds generally include fillers, and conventional surface treatment agents such as silane coupling agents and titanates are used to improve the interfacial compatibility between the fillers and the silicone matrix, thereby enhancing dispersibility and processability, and ultimately achieving the integration of curing, bonding, insulation and thermal conductivity.

[0004] Although existing technologies have been applied on a large scale, there are still irreconcilable contradictions in the synergy of key indicators such as high thermal conductivity, high filling capacity, high flow level, and low viscosity. Summary of the Invention

[0005] In view of the aforementioned problems, this application is made to provide a high-leveling silicone thermally conductive potting compound based on filler compounding and anion-cation modification, and a method for preparing the same, which overcomes or at least partially solves the aforementioned problems, comprising: A high-leveling silicone thermally conductive potting compound based on filler compounding and anion-cation modification, comprising a first potting compound and a second potting compound in a mass ratio of 1:1; By weight, the first potting compound comprises 70-80 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-0.3 parts platinum catalyst, and 400-600 parts modified thermally conductive filler; The second potting compound comprises 70-80 parts vinyl silicone oil, 3-8 parts hydrogen-containing silicone oil, 0.1-0.3 parts inhibitor, and 400-600 parts modified thermally conductive filler; The modified conductive filler includes modified silicon micropowder with a first particle size, modified alumina with a second particle size, and modified alumina with a third particle size.

[0006] Furthermore, the mass ratio of the modified silica powder of the first particle size, the modified alumina of the second particle size, and the modified alumina of the third particle size is (40-50)%: (30-40)%: (15-25)%.

[0007] Furthermore, the modified silicon micropowder is modified by a cationic modifier to obtain the modified silicon micropowder with cationic surface.

[0008] Furthermore, the cationic modifier is hexadecyltrimethylammonium bromide.

[0009] Furthermore, the modified alumina is modified by an anionic modifier to obtain the modified alumina with anionic surface.

[0010] Furthermore, the anionic modifier is aluminum stearate.

[0011] Furthermore, the first particle size is 30-50 μm, the second particle size is 4-6 μm, and the third particle size is 1-3 μm.

[0012] A method for preparing a high-leveling silicone thermally conductive potting compound based on filler compounding and anion / cation modification, comprising the following steps: Vinyl silicone oil, color paste, platinum catalyst and modified conductive and thermally conductive filler in a first specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000rpm, and the mixing temperature is 20-30℃ to obtain the first potting compound. The vinyl silicone oil, hydrogen-containing silicone oil, inhibitor, and the modified conductive and thermally conductive filler in the second specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000 rpm, and the mixing temperature is 20-30℃ to obtain the second potting compound. The first potting compound and the second potting compound are mixed and stirred at a mass ratio of 1:1, with a vacuum degree of -0.1MPa, a mixing time of 5-15 min, a stirring speed of 1000-2000 rpm, and a stirring temperature of 20-30℃. The potting compound is injected into the mold and cured at 70-90℃ for 0.5-2 h to obtain the target silicone potting compound material.

[0013] Furthermore, the preparation steps of the modified silica powder include: Disperse hexadecyltrimethylammonium bromide in anhydrous ethanol; Add silica powder, heat to 100℃, add hexadecyltrimethylammonium bromide anhydrous ethanol solution, stir evenly, and dry at 100~110℃ for 2-4 hours to obtain modified silica powder with cations on the surface.

[0014] Furthermore, the preparation steps of the modified alumina include: Disperse aluminum stearate in anhydrous ethanol; Alumina filler was added, the temperature was raised to 100℃, and anhydrous ethanol solution of aluminum stearate was added. After stirring evenly, the mixture was dried at 100~110℃ for 2-4 hours to obtain modified alumina with anionic surface.

[0015] This application has the following advantages: In the embodiments of this application, addressing the inherent contradiction of unresolved synergy between high thermal conductivity, high filling capacity, high leveling, and low viscosity in the prior art, this application provides a solution for modifying and compounding thermally conductive fillers. Specifically, it comprises a first potting compound and a second potting compound in a 1:1 mass ratio. By weight, the first potting compound comprises 70-80 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-0.3 parts platinum catalyst, and 400-600 parts modified thermally conductive filler; the second potting compound comprises 70-80 parts vinyl silicone oil, 3-8 parts hydrogen-containing silicone oil, 0.1-0.3 parts inhibitor, and 400-600 parts modified thermally conductive filler; wherein the modified thermally conductive filler comprises modified silica powder with a first particle size, modified alumina with a second particle size, and modified alumina with a third particle size. By using a multi-stage particle size compound of modified silica powder (first particle size), modified alumina (second particle size), and modified alumina (third particle size) to form a modified thermally conductive filler, the overall packing density of the filler is increased, significantly improving the thermal conductivity and mechanical strength of the potting compound. By using modified silica powder and modified alumina to form a modified conductive filler, the system viscosity remains low and the leveling properties are excellent even at high filler contents. At the same time, the mechanical properties and long-term stability of the potting compound are improved. The two-component system of the first and second potting compounds ensures uniform filler distribution after mixing by pre-dispersing the filler in both components. Attached Figure Description

[0016] To more clearly illustrate the technical solution of this application, the drawings used in the description of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figure 1 This is a flowchart of the preparation method of a high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification according to an embodiment of this application; Figure 2 This is a schematic flowchart of a method for preparing a high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification, according to an embodiment of this application. Detailed Implementation

[0018] To make the objectives, features, and advantages of this application more apparent and understandable, the application will be further described in detail below with reference to the accompanying drawings and specific embodiments. Obviously, the described embodiments are only some, not all, of the embodiments of this application. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0019] The inventors, through analysis of existing technologies, discovered that while these technologies have achieved large-scale application, there are still irreconcilable contradictions in the synergy of key indicators such as high thermal conductivity, high filling capacity, high leveling, and low viscosity. The specific problems and their causes are as follows: (1) High filler content leads to a sharp increase in viscosity and poor flowability. High proportion of thermally conductive filler is commonly used to meet the high thermal conductivity requirements. However, after adding a large amount of filler, the frictional resistance between particles is large and the free volume of the system is reduced, which leads to an increase in the viscosity of the potting compound and a decrease in the leveling speed. Defects such as incomplete potting and insufficient glue are prone to occur, which seriously affect the heat dissipation efficiency and insulation reliability.

[0020] (2) The filler is prone to agglomeration and the interfacial bonding is weak. Traditional surface treatment techniques cannot effectively eliminate the polarity difference between the high polarity of the filler surface and the low polarity of the organosilicon. After curing, the filler is prone to debonding from the matrix, resulting in interruption of the heat conduction path and a decrease in mechanical properties.

[0021] (3) Easy to agglomerate, many voids, and poor thermal conductivity network. The existing particles have high porosity, making it difficult to form a continuous and efficient thermal conductivity network. If the proportion of large particles is simply increased to improve thermal conductivity, it will further affect the anti-settling performance; if the proportion of small particles is increased to improve rheology, it will lead to a surge in viscosity and poor leveling.

[0022] Reference Figure 1 This application illustrates an embodiment of a high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification, characterized in that it comprises a first potting compound and a second potting compound in a mass ratio of 1:1; By weight, the first potting compound comprises 70-80 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-0.3 parts platinum catalyst, and 400-600 parts modified thermally conductive filler; The second potting compound comprises 70-80 parts vinyl silicone oil, 3-8 parts hydrogen-containing silicone oil, 0.1-0.3 parts inhibitor, and 400-600 parts modified thermally conductive filler; The modified conductive filler includes modified silicon micropowder with a first particle size, modified alumina with a second particle size, and modified alumina with a third particle size.

[0023] It should be noted that vinyl silicone oil, as an organosilicon matrix resin, provides basic properties such as matrix flexibility, resistance to high and low temperatures, and insulation. As an example, vinyl silicone oil can be at least one of α,ω-divinyl polydimethylsiloxane, terminal vinyl polydimethylsiloxane, side vinyl polydimethylsiloxane, vinyl MQ silicone resin modified silicone oil, and highly compliant vinyl polysiloxane.

[0024] Color pastes are used to adjust the appearance color of potting compounds; as an example, color pastes may be at least one of carbon black paste, silicone black paste, silicone white paste, silicone gray paste, and inorganic paste.

[0025] Platinum catalysts, acting as catalysts for addition curing reactions, trigger the addition reaction between vinyl groups and silane groups; as an example, platinum catalysts may be at least one of the following: a complex of chloroplatinic acid and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane, a chloroplatinic acid isopropanol complex, a platinum-tetramethyldivinyldisiloxane complex, a platinum-vinylsiloxane complex, and a caster platinum catalyst.

[0026] Hydrogen-containing silicone oil is a crosslinking agent that can undergo hydrosilylation curing with vinyl silicone oil under platinum catalysis. As an example, the hydrogen-containing silicone oil can be at least one of the following: end-hydrogen-containing polydimethylsiloxane, side-hydrogen-containing polydimethylsiloxane, high-hydrogen-containing polysiloxane, and low-hydrogen-containing crosslinked silicone oil.

[0027] Inhibitors are used to suppress the activity of platinum catalysts at room temperature and prolong the working time of rubber compounds; as an example, the inhibitor can be at least one of 1-ethynylcyclohexanol, 3-methyl-1-butyn-3-ol, tetramethyltetravinylcyclotetrasiloxane, and alkynol silane inhibitors.

[0028] In the embodiments of this application, addressing the inherent contradiction in the synergy of high thermal conductivity, high filler content, high leveling properties, and low viscosity in existing technologies, this application provides a solution for modifying and compounding thermally conductive fillers. By compounding modified thermally conductive fillers with a multi-level particle size profile consisting of modified silica powder of a first particle size, modified alumina of a second particle size, and modified alumina of a third particle size, the overall packing density of the filler is increased, significantly improving the thermal conductivity and mechanical strength of the potting compound. By using modified silica powder and modified alumina to form a modified conductive filler, low system viscosity and excellent leveling properties are maintained even at high filler contents. Simultaneously, the mechanical properties and long-term stability of the potting compound are improved. Through a two-component system of first and second potting compounds, the two components are pre-dispersed uniformly to ensure a uniform overall filler distribution after mixing.

[0029] The following will further describe a high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification in this exemplary embodiment.

[0030] In one embodiment of the present invention, the mass ratio of the modified silica powder of the first particle size, the modified alumina of the second particle size, and the modified alumina of the third particle size is (40-50)%: (30-40)%: (15-25)%.

[0031] Specifically, the smaller the filler particle size, the higher the viscosity of the prepared potting compound. This is because smaller-sized thermally conductive fillers have a larger specific surface area, which can adsorb more silicone oil, resulting in less freely flowing silicone oil in the system and thus increasing viscosity. As the filler particle size increases, the buoyancy provided by the silicone oil gradually becomes insufficient to overcome the weight of the filler itself, leading to increased sedimentation. This invention uses a blend of fillers with different particle sizes to fill the gaps between coarse-sized powders with fine-sized powders. This not only effectively improves the powder dispersion state but also increases the filler packing density, effectively improving the thermal conductivity and stability of the potting compound. As an example, the first particle size is 30-50 μm, the second particle size is 4-6 μm, and the third particle size is 1-3 μm. Large-particle silica powder serves as a framework, medium-sized alumina fills the gaps between large particles, and small-particle alumina further fills the remaining voids, increasing the filler packing density and constructing a continuous thermally conductive network while simultaneously considering the system's viscosity and leveling properties.

[0032] In one embodiment of the present invention, the modified silicon micropowder is modified by a cationic modifier to obtain the modified silicon micropowder with a cationic surface. Specifically, a cationic modifier is used to modify the surface of the silicon micropowder, so that the surface of the silicon micropowder carries cationic ions for electrostatic interaction with anionic modified alumina. As an example, the cationic modifier can be a quaternary ammonium salt cationic surfactant.

[0033] In one specific implementation, the cationic modifier is hexadecyltrimethylammonium bromide (CTAB).

[0034] In one embodiment of the present invention, the modified alumina is obtained by modifying the alumina with an anionic modifier to obtain the modified alumina with anionic surfaces. Specifically, an anionic modifier is used to modify the surface of the alumina powder, so that the alumina surface carries anions. As an example, the anionic modifier is aluminum stearate.

[0035] Inorganic fillers are prone to secondary agglomeration in organosilicon matrices due to van der Waals forces. In this embodiment, anionic and cationic modification is used to promote particle aggregation by utilizing the electrostatic interaction between anionic and cationic particles to form aggregates of a certain degree. The free flow space of silicone oil outside the aggregates is increased, reducing collision and friction resistance during the flow process, and significantly improving the problems of high viscosity and poor leveling properties of organosilicon potting compounds.

[0036] Powder particles treated with cationic surface modifiers carry a positive charge. These particles, along with negatively charged powder particles treated with anionic surface modifiers, attract each other electrostatically, forming partially compact aggregates. In this case, the number of individually dispersed particles in the system is small, while the aggregates provide ample free flow space for the vinyl silicone oil, effectively reducing particle collisions and frictional resistance during silicone oil flow, ultimately significantly lowering the viscosity of the silicone potting compound. In contrast, when unmodified powder is filled into vinyl silicone oil, the degree of particle aggregation is lower and the distribution is relatively uniform, but the free flow space for the silicone oil is reduced, resulting in a significantly higher system viscosity and poor leveling properties.

[0037] Reference Figure 1 and Figure 2 This paper illustrates a method for preparing a high-leveling silicone thermally conductive potting compound based on filler compounding and anion / cation modification, including the following steps: S110. Add the vinyl silicone oil, color paste, platinum catalyst and modified conductive and thermally conductive filler in the first specified mass ratio to a double planetary vacuum mixer for mixing and stirring. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the stirring speed is 1000-2000rpm, and the stirring temperature is 20-30℃ to obtain the first potting compound. S120. Add the vinyl silicone oil, hydrogen-containing silicone oil, inhibitor, and the modified conductive and thermally conductive filler in the second specified mass ratio to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000 rpm, and the mixing temperature is 20-30℃ to obtain the second potting compound. S130. Mix the first potting compound and the second potting compound at a mass ratio of 1:1, with a vacuum degree of -0.1MPa, a mixing time of 5-15 min, a mixing speed of 1000-2000 rpm, and a mixing temperature of 20-30℃. S140. Inject the potting compound into the mold and cure it at 70-90℃ for 0.5-2 h to obtain the target silicone potting compound material.

[0038] The following will further illustrate a method for preparing a high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification in this exemplary embodiment.

[0039] As described in step S110, the vinyl silicone oil, color paste, platinum catalyst and modified conductive and thermally conductive filler in the first specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000rpm, and the mixing temperature is 20-30℃ to obtain the first potting compound.

[0040] The first potting compound comprises, by weight, the following raw materials: 70-90 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-1 parts platinum catalyst, and 500-600 parts modified thermally conductive filler. The raw material components of the first potting compound are mixed using a dual planetary vacuum mixer with a vacuum degree ≤-0.1 MPa, a mixing time of 5-10 min, a mixing speed of 1500-2000 rpm, and a mixing temperature of 20-40℃ to obtain the first potting compound.

[0041] As described in step S120, the vinyl silicone oil, hydrogen-containing silicone oil, inhibitor, and the modified conductive and thermally conductive filler in the second specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000 rpm, and the mixing temperature is 20-30℃ to obtain the second potting compound.

[0042] The second potting compound comprises, by weight, the following raw materials: 70-90 parts vinyl silicone oil, 2-10 parts hydrogen-containing silicone oil, 0.1-1 parts inhibitor, and 500-600 parts modified thermally conductive filler. The raw material components of the second potting compound are mixed using a dual planetary vacuum mixer at a vacuum degree ≤-0.1 MPa, a mixing time of 5-10 min, a mixing speed of 1500-2000 rpm, and a mixing temperature of 20-40℃ to obtain the second potting compound.

[0043] As described in step S130, the first potting compound and the second potting compound are mixed and stirred at a mass ratio of 1:1, with a vacuum degree of -0.1MPa, a mixing time of 5-15 min, a stirring speed of 1000-2000 rpm, and a stirring temperature of 20-30℃.

[0044] The first potting compound and the second potting compound are mixed and stirred at a mass ratio of 1:1, with a vacuum degree of ≤-0.1MPa, a stirring time of 5~10 min, a stirring speed of 1500~2000 rpm, and a stirring temperature of 20~40℃.

[0045] As described in step S140, the potting compound is injected into the mold and cured at 70-90℃ for 0.5-2 h to obtain the target silicone potting compound material.

[0046] The potting compound is injected into a mold and cured at 80°C for 0.5–3 hours to obtain the silicone potting compound material. In this step, the hydrogen-containing silicone oil undergoes a hydrosilylation reaction with the vinyl group of the vinyl silicone oil under catalysis, forming a cross-linked network. The catalyst catalyzes the hydrosilylation reaction; the inhibitor complexes with the catalyst to inhibit the reaction and control the curing speed; and the colorant is used for coloring.

[0047] In one embodiment of the present invention, the preparation steps of the modified silicon micropowder include: Disperse hexadecyltrimethylammonium bromide in anhydrous ethanol; Add silica powder, heat to 100℃, add hexadecyltrimethylammonium bromide anhydrous ethanol solution, stir evenly, and dry at 100~110℃ for 2-4 hours to obtain modified silica powder with cations on the surface.

[0048] Specifically, an anhydrous ethanol solution (5-20 wt%) of the cationic modifier hexadecyltrimethylammonium bromide (CTAB) is prepared, and silica micropowder filler is added in a high-speed mixer (1000-1500 rpm). The mixture is heated to 100°C, and the anionic modifier anhydrous ethanol solution (0.5-3 wt% of the thermally conductive filler) is added. The mixture is stirred for 0.5-1 h. The mixture is then dried at 100-110°C for 3-5 h to obtain modified silica micropowder thermally conductive filler with cationic surface.

[0049] In this step, the main component of the silicon micropowder is SiO2, and its surface contains a large number of silanol groups (Si-OH), which dissociate into Si-O- in the solution, making the surface of the silicon micropowder negatively charged. Hexadecyltrimethylammonium bromide (CTAB), as a cationic modifier, dissociates into C in the solution. 16 H 33 N+(CH3)3 and Br-, through electrostatic adsorption, branch C16 long alkyl groups onto the surface of silicon micropowder to form a hydrophobic monolayer. The surface of the silicon micropowder changes from negatively hydrophilic to positively hydrophobic, and the Zeta potential changes from negative to positive, which can generate electrostatic adsorption with anionic modified fillers.

[0050] In one embodiment of the present invention, the preparation steps of the modified alumina include: Disperse aluminum stearate in anhydrous ethanol; Alumina filler was added, the temperature was raised to 100℃, and anhydrous ethanol solution of aluminum stearate was added. After stirring evenly, the mixture was dried at 100~110℃ for 2-4 hours to obtain modified alumina with anionic surface.

[0051] Specifically, an anhydrous ethanol solution (5-20 wt%) of anionic modifier aluminum stearate is prepared, and alumina filler is added in a high-speed mixer (1000-1500 rpm). The mixture is heated to 100°C, and the prepared anhydrous ethanol solution of anionic modifier (0.5-3 wt% of the thermally conductive filler) is added. The mixture is stirred for 0.5-1 h. The mixture is then dried at 100-110°C for 3-5 h to obtain anionic modified alumina thermally conductive filler.

[0052] In this step, the aluminum hydroxyl groups (Al-OH) on the surface of alumina react with aluminum stearate (Al(C)). 17 H 35 The reaction of COO3) is a surface chemical adsorption reaction, the core of which is the dehydration and bonding of aluminum hydroxyl groups with aluminum stearate, and the stearate C 17 H 35 COO grafting onto the alumina surface transforms the alumina surface from hydrophilic and oleophobic (hydroxyl groups) to oleophilic and hydrophobic (stearic acid chains), while also carrying a negative charge, allowing it to electrostatically adsorb with cationic modified fillers.

[0053] Example 1 S1: Surface treatment of alumina filler: Weigh 1g of anionic modifier aluminum stearate and disperse it in 4g of anhydrous ethanol. Add 500g of alumina filler to a high-speed mixer (1000 rpm), heat to 100℃, add 5g of the prepared aluminum stearate anhydrous ethanol solution, and stir for 0.5 h; dry at 100℃ for 3 h to obtain anionic modified alumina thermally conductive filler.

[0054] S2: Surface treatment of silica powder filler: Weigh 1g of cationic modifier hexadecyltrimethylammonium bromide and disperse it in 4g of anhydrous ethanol. Add 500g of silica powder filler to a high-speed mixer (1000rpm), heat to 100℃, add 5g of the above-prepared hexadecyltrimethylammonium bromide anhydrous ethanol solution, and stir for 0.5h; dry at 100℃ for 3h to obtain modified silica powder thermally conductive filler with cationic surface.

[0055] S3: Thermally conductive filler compound: 40um modified silicon micro powder: 5um modified alumina: 2um modified alumina are compounded in a mass ratio of 45%: 35%: 20%.

[0056] S4: Preparation of potting compound component A: 75g of vinyl silicone oil (α,ω-divinyl polydimethylsiloxane), 0.1~0.3 parts of color paste (carbon black paste with vinyl silicone oil as carrier, carbon black 30%), 0.2g of platinum catalyst (a complex of chloroplatinic acid and 1,3-divinyl-1,1,3,3-tetramethyldisiloxane), and 500g of modified thermally conductive filler were mixed using a double planetary vacuum mixer. The vacuum degree was -0.1MPa, the mixing time was 10min, the stirring speed was 1500rpm, and the stirring temperature was 25℃ to obtain potting compound component A. S5: Preparation of potting compound component B: 75g of vinyl silicone oil (α,ω-divinyl polydimethylsiloxane), 5g of hydrogen-containing silicone oil (side-chain hydrogen-containing polydimethylsiloxane), 0.2g of inhibitor (1-ethynylcyclohexanol), and 500g of modified thermally conductive filler were mixed using a dual planetary vacuum mixer. The vacuum degree was -0.1MPa, the mixing time was 10min, the mixing speed was 1500 rpm, and the mixing temperature was 25℃ to obtain potting compound component B. S6: Mixing of Component A and Component B: Mix and stir the above Component A and Component B at a mass ratio of 1:1, with a vacuum degree of -0.1MPa, a mixing time of 10 min, a stirring speed of 1500 rpm, and a stirring temperature of 25℃.

[0057] S7: Curing: Inject the potting compound into the mold and cure it at 80°C for 1 hour to obtain the silicone potting compound material.

[0058] Example 2 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 45%: 40%: 15%.

[0059] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0060] Example 3 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 45%: 30%: 25%.

[0061] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0062] Example 4 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 40%: 35%: 25%.

[0063] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0064] Example 5 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 50%: 35%: 15%.

[0065] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0066] Example 6 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 50%: 30%: 20%.

[0067] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0068] Example 7 The difference from Example 1 is as follows: The filler mass ratio in step S3 is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 40%: 40%: 20%.

[0069] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0070] Comparative Example 1 The difference from Example 1 is as follows: The filler used in step S3 is only 40µm modified silica powder.

[0071] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0072] Comparative Example 2 The difference from Example 1 is as follows: The filler used in step S3 is only 5µm modified alumina.

[0073] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0074] Comparative Example 3 The difference from Example 1 is as follows: The filler used in step S3 is only 2µm modified alumina.

[0075] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0076] Comparative Example 4 The difference from Example 1 is as follows: The filler in step S3 is an unmodified thermally conductive powder, with a mass ratio of 40µm unmodified silicon micropowder: 5µm unmodified alumina: 2µm unmodified alumina = 45%: 35%: 20%.

[0077] The remaining conditions and parameters are the same as in Example 1, and the silicone thermally conductive potting compound is obtained.

[0078] Comparative Example 5 The difference from Example 1 is as follows: In step S3, the 40µm modified silica powder used as filler is replaced with 30µm modified silica powder. The 30µm modified silica powder, 5µm modified alumina, and 2µm modified alumina are compounded in a mass ratio of 45%:35%:20%.

[0079] The remaining conditions and parameters are the same as in Example 1, and the silicone potting compound is obtained.

[0080] Comparative Example 6 The difference from Example 1 is as follows: In step S3, the 40µm modified silica powder used as filler is replaced with 50µm modified silica powder. The 50µm modified silica powder, 5µm modified alumina, and 2µm modified alumina are compounded in a mass ratio of 45%:35%:20%.

[0081] The remaining conditions and parameters are the same as in Example 1, and the silicone potting compound is obtained.

[0082] Comparative Example 7 The difference from Example 1 is as follows: The cationic modifier used in step S2 is octadecyltrimethylammonium chloride (OTAC).

[0083] The remaining conditions and parameters are the same as in Example 1, and the silicone potting compound is obtained.

[0084] Comparative Example 8 The difference from Example 1 is as follows: The anionic modifier used in step S1 is sodium oleate.

[0085] The remaining conditions and parameters are the same as in Example 1, and the silicone potting compound is obtained.

[0086] Comparative Example 9 The difference from Example 1 is as follows: In step S1, aluminum hydroxide is used as the thermally conductive filler modified with the anionic modifier aluminum stearate; in step S2, aluminum nitride is used as the thermally conductive filler modified with the cationic modifier hexadecyltrimethylammonium bromide. In step S3, 40µm modified aluminum nitride, 5µm modified aluminum hydroxide, and 2µm modified aluminum hydroxide are compounded in a mass ratio of 45%:35%:20%.

[0087] The remaining conditions and parameters are the same as in Example 1, and the silicone potting compound is obtained.

[0088] Performance testing The silicone potting compounds prepared in Examples 1-9 were subjected to performance tests. The test items and test standards are shown in Table 1. Table 1

[0089] The silicone potting compounds prepared in Examples 1-7 and Comparative Examples 1-9 were subjected to performance tests, and the test results are shown in Table 2: Table 2

[0090] The above experimental results show that: The comparison of Examples 1-7 shows that when the mass ratio of modified filler compound is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 45%: 35%: 20%, the organosilicon thermally conductive potting compound has the highest thermal conductivity (2.47 W / m·K), the lowest viscosity (4100 mPa·s), and the best leveling properties (128.9 mm / min); no bottom hardening occurred after standing for 112 days. When the filler particle size ratio in Examples 2-7 deviated from the above ratio, the thermal conductivity decreased to 2.28-2.42 W / m·K, the viscosity increased to 4300-5100 mPa·s, the leveling properties decreased to 113.7-123.5 mm / min, and the anti-settling performance decreased to 82-109 days. It can be concluded that as the proportion of large-particle-size fillers increases, the contact interface between fillers decreases, and the thermal conductivity improves. Additionally, the smaller specific surface area and lower surface energy of the powder reduce the adsorption of Si polymer chains, thereby lowering internal friction and resulting in less free-flowing silicone oil in the system, leading to a decrease in viscosity and an increase in leveling properties. However, as the proportion of small-particle-size fillers continues to increase, the increased contact interface between powder particles affects the thermal conductivity and easily forms hard aggregates between large particles, thus reducing the system's fluidity. When the mass ratio of modified filler compound is 40µm modified silica powder: 5µm modified alumina: 2µm modified alumina = 45%: 35%: 20%, relatively optimal leveling performance and stability are achieved.

[0091] A comparison of Examples 1-7 and Comparative Examples 1-3 shows that, compared to a single thermally conductive powder, the leveling and anti-settling properties of thermally conductive powders with different particle sizes are significantly improved. The thermal conductivity of Comparative Examples 1-3 is only 1.63-1.85 W / m·K, significantly lower than that of Examples 1-7. This is because the bulk density of thermally conductive powders with a single particle size is low. By using powders of different particle sizes, smaller particle sizes can be filled into the gaps between larger particle sizes, forming a continuous and efficient thermally conductive network. Furthermore, Comparative Example 1, which simply uses larger particle sizes to improve thermal conductivity, further affects the anti-settling performance; Comparative Examples 2 and 3, which only use smaller particle sizes to improve sedimentation, result in a surge in viscosity and a decrease in leveling.

[0092] The comparison between Example 1 and Comparative Example 4 shows that, compared to unmodified thermally conductive fillers, the thermally conductive potting compound prepared with thermally conductive fillers treated with cationic and anionic surface modifiers exhibits an increase in thermal conductivity from 2.09 W / m·K to 2.47 W / m·K, a decrease in viscosity of approximately 47.4%, significantly improved leveling performance, and an increase in anti-settling performance from 58 days to 112 days. This is because after the thermally conductive fillers are treated with cationic and anionic surface modifiers, the positively charged silica powder and the negatively charged alumina powder particles attract each other through electrostatic interactions, forming dense aggregates. This reduces the number of individually dispersed particles in the system, providing more free flow space for the external silicone oil, effectively reducing frictional resistance during silicone oil flow, and ultimately significantly reducing the viscosity of the silicone potting compound. In contrast, when unmodified powder is filled into silicone oil, the degree of particle aggregation within the system is lower, resulting in a reduced free flow space for the silicone oil, leading to a significantly higher system viscosity and decreased leveling performance. In addition, the modified stearic acid chains and long alkyl links are branched onto the surface of the thermally conductive filler, changing the surface from hydrophilic and oleophobic to hydrophobic and oleophilic, which improves the compatibility with silicone oil and enhances the stability and anti-settling properties of the silicone potting compound.

[0093] The comparison between Example 1 and Comparative Examples 5-6 shows that the particle size selection of large-diameter silica powder also affects the overall performance of the potting compound. In Comparative Example 5, replacing 40µm modified silica powder with 30µm modified silica powder resulted in a decrease in thermal conductivity to 2.31 W / m·K, an increase in viscosity to 5300 mPa·s, and a decrease in leveling to 110.2 mm / min. This indicates that when the particle size of the large-diameter filler is too small, the specific surface area increases, leading to increased silicone oil adsorption and interparticle friction, which is detrimental to low viscosity and high leveling. In Comparative Example 6, replacing 40µm modified silica powder with 50µm modified silica powder resulted in a thermal conductivity of 2.41 W / m·K, a viscosity of 4300 mPa·s, and a leveling of 124.6 mm / min. However, the anti-settling performance decreased to 42 days. This indicates that while a larger particle size is beneficial for reducing flow resistance, it also increases particle weight and accelerates settling, making it difficult to maintain storage stability.

[0094] A comparison of Example 1 with Comparative Examples 7-8 shows that the type of cationic and anionic modifiers has a significant impact on the interfacial compatibility and electrostatic synergistic effect of the filler. Comparative Example 7 used octadecyltrimethylammonium chloride instead of hexadecyltrimethylammonium bromide as a cationic modifier, and Comparative Example 8 used sodium oleate instead of aluminum stearate as an anionic modifier; both resulted in a decrease in the thermal conductivity and leveling properties of the thermally conductive potting compound. The results indicate that the use of aluminum stearate anionic modifier and hexadecyltrimethylammonium bromide cationic modifier in this invention can more effectively adjust the surface charge of alumina and silica powder, enabling the filler to form a moderately aggregated and stably distributed thermally conductive network in the silicone oil.

[0095] A comparison of Example 1 and Comparative Example 9 shows that the aluminum stearate anionic modifier and hexadecyltrimethylammonium bromide cationic modifier used in this patent are suitable not only for alumina / silica powder filler systems but also for aluminum nitride / aluminum hydroxide thermally conductive fillers. However, even with the same anionic and cationic surface modification and the same compounding ratio, the thermal conductivity of the resulting potting compound is only 2.15 W / m·K, the viscosity increases to 6900 mPa·s, the leveling property decreases to 102.5 mm / min, and the anti-settling property decreases to 61 days. This indicates that the present invention selects 40µm silica powder, 5µm alumina, and 2µm alumina for compounding, which not only has lower raw material costs but also has better compatibility with the aforementioned anionic and cationic modified system and organosilicon matrix, enabling the simultaneous achievement of high thermal conductivity, low viscosity, high leveling, and good anti-settling properties at higher filling amounts.

[0096] In summary, Example 1 outperforms the comparative examples in all four aspects: thermal conductivity, viscosity, leveling, and anti-settling properties. This demonstrates that the present invention, through the synergistic effect of specific particle size thermally conductive filler compound and anionic and cationic surface modification, can effectively solve the problems of high viscosity, poor leveling, discontinuous thermal conductive network, and insufficient storage stability of traditional silicone thermally conductive potting compounds under high filling conditions.

[0097] Although preferred embodiments of the present application have been described, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments as well as all changes and modifications falling within the scope of the embodiments of the present application.

[0098] Finally, it should be noted that in this document, relational terms such as "first" and "second" are used only to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or terminal device that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or terminal device. Without further limitations, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or terminal device that includes said element.

[0099] The above provides a detailed description of the high-level silicone thermally conductive potting compound based on filler compounding and anion-cation modification, and its preparation method. Specific examples have been used to illustrate the principles and implementation methods of this application. The above description of the embodiments is only for the purpose of helping to understand the method and core ideas of this application. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of this application. Therefore, the content of this specification should not be construed as a limitation of this application.

Claims

1. A high-flow leveling silicone thermal conductive pouring sealant based on filler compounding and anion-cation modification, characterized in that, It includes a first potting compound and a second potting compound with a mass ratio of 1:1; By weight, the first potting compound comprises 70-80 parts vinyl silicone oil, 0.1-0.3 parts colorant, 0.1-0.3 parts platinum catalyst, and 400-600 parts modified thermally conductive filler; The second potting compound comprises 70-80 parts vinyl silicone oil, 3-8 parts hydrogen-containing silicone oil, 0.1-0.3 parts inhibitor, and 400-600 parts modified thermally conductive filler; The modified conductive filler includes modified silicon micropowder with a first particle size, modified alumina with a second particle size, and modified alumina with a third particle size.

2. The high-level silicone thermally conductive potting compound according to claim 1, characterized in that, The mass ratio of the modified silica powder of the first particle size, the modified alumina of the second particle size, and the modified alumina of the third particle size is (40-50)%: (30-40)%: (15-25)%.

3. The high-level silicone thermally conductive potting compound according to claim 1, characterized in that, The modified silicon micropowder is obtained by modifying silicon micropowder with a cationic modifier to obtain the modified silicon micropowder with cationic surface. 4.The high-flowing organic silicon heat-conducting pouring sealant according to claim 3, characterized in that, The cationic modifier is hexadecyltrimethylammonium bromide.

5. The high-level silicone thermally conductive potting compound according to claim 1, characterized in that, The modified alumina is obtained by modifying alumina with anionic modifier to obtain the modified alumina with anionic surface. 6.The high-flowing organic silicon heat-conducting pouring sealant according to claim 5, characterized in that, The anionic modifier is aluminum stearate.

7. The high-flowing silicone thermal conductive potting adhesive according to claim 1, wherein, The first particle size is 30-50 μm, the second particle size is 4-6 μm, and the third particle size is 1-3 μm.

8. A method for preparing the high-flowing leveling silicone heat-conducting pouring sealant based on filler compound and anion-cation modification according to any one of claims 1-7, characterized in that, Including the following steps: Vinyl silicone oil, color paste, platinum catalyst and modified conductive and thermally conductive filler in a first specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000rpm, and the mixing temperature is 20-30℃ to obtain the first potting compound. The vinyl silicone oil, hydrogen-containing silicone oil, inhibitor, and the modified conductive and thermally conductive filler in the second specified mass ratio are added to a double planetary vacuum mixer for mixing. The vacuum degree is -0.1MPa, the mixing time is 5-15min, the mixing speed is 1000-2000 rpm, and the mixing temperature is 20-30℃ to obtain the second potting compound. The first potting compound and the second potting compound are mixed and stirred at a mass ratio of 1:1, with a vacuum degree of -0.1MPa, a mixing time of 5-15 min, a stirring speed of 1000-2000 rpm, and a stirring temperature of 20-30℃. The potting compound is injected into the mold and cured at 70-90℃ for 0.5-2 h to obtain the target silicone potting compound material.

9. The preparation method according to claim 8, characterized in that, The preparation steps of the modified silicon micropowder include: Disperse hexadecyltrimethylammonium bromide in anhydrous ethanol; Add silica powder, heat to 100℃, add hexadecyltrimethylammonium bromide anhydrous ethanol solution, stir evenly, and dry at 100~110℃ for 2-4 hours to obtain modified silica powder with cations on the surface.

10. The preparation method according to claim 8, characterized in that, The preparation steps of the modified alumina include: Disperse aluminum stearate in anhydrous ethanol; Alumina filler was added, the temperature was raised to 100℃, and anhydrous ethanol solution of aluminum stearate was added. After stirring evenly, the mixture was dried at 100~110℃ for 2-4 hours to obtain modified alumina with anionic surface.