Preparation of a silicone pressure-sensitive adhesive and tape for bonding low surface area materials

By employing a multi-component synergistic and dual crosslinking mechanism, and using a combination of phenyl borate-modified hydroxyl-terminated polydimethylsiloxane and other compositions, the problems of insufficient adhesion, poor interfacial adaptability, limited heat resistance, and lack of flame retardant properties of silicone pressure-sensitive adhesives on low surface energy materials have been solved, resulting in a silicone pressure-sensitive adhesive with high-strength adhesion, heat resistance, and flame retardancy.

CN123107619APending Publication Date: 2026-11-17苏州恒悦新材料股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611253884.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing silicone pressure-sensitive adhesives suffer from problems such as insufficient adhesion, poor interface adaptability, difficulty in balancing cohesion and initial tack, limited heat resistance, and lack of flame retardant properties when bonding low surface energy materials, making it difficult to meet the needs of high-end application scenarios.

Method used

Employing a multi-component synergistic and dual crosslinking mechanism, a combination of phenylboronic acid ester-modified hydroxyl-terminated polydimethylsiloxane, long-chain alkyl-modified MQ silicone resin, fluorosilicone block copolymer, mercaptopropyl-modified hydroxyl silicone oil, composite crosslinking agent, epoxysilane-phenylsilane cocondensation oligomer, carborane-modified hydroxyl silicone oil, and composite flame retardant is used, along with UV-initiated thiol-ene click chemistry and hydrosilylation crosslinking, to form a surface energy gradient structure and a dual crosslinking network.

Benefits of technology

It significantly enhances the bonding strength to low surface energy materials, achieves excellent heat resistance and flame retardancy, balances initial tack and holding power, improves interfacial adhesion and interfacial compatibility, and meets the needs of high-temperature application scenarios.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses the preparation of an organosilicon pressure-sensitive adhesive and tape for bonding low surface area materials, which is made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane, 50-110 parts of long-chain alkyl modified MQ silicone resin, 3-15 parts of fluorosilicone block copolymer, 1-8 parts of mercaptopropyl modified hydroxyl silicone oil, 0.5-5 parts of a composite crosslinking agent composed of hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin, 1-10 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier, 0.5-5 parts of carborane modified hydroxyl silicone oil, 3-15 parts of a composite flame retardant composed of hexaphenoxycyclotriphosphazene and phenyl silicone oil, 0.1-3 parts of ultraviolet photoinitiator, 0.05-0.5 parts of platinum catalyst, and 100-300 parts of organic solvent. This invention achieves high-strength bonding of low surface energy materials through a multi-mechanism synergy of dynamic bond interface adaptation of phenyl borate ester, fluorosilicone surface energy gradient, carborane interface affinity, thiol-ene / silyl hydroaddition dual crosslinking, and phosphorus-nitrogen synergistic flame retardancy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of silicone pressure-sensitive adhesive technology, specifically to the preparation of a silicone pressure-sensitive adhesive and tape for bonding low surface area materials. Background Technology

[0002] Silicone pressure-sensitive adhesives are high-performance adhesive materials with polysiloxane as the main chain structure. They are typically composed of silicone rubber, silicone resin, crosslinking agents, fillers, and solvents. Compared with acrylic or rubber-based pressure-sensitive adhesives, silicone pressure-sensitive adhesives have a wider temperature range, better weather resistance, chemical resistance, electrical insulation, and good adhesion to low surface energy materials that are difficult to bond. They are widely used in electronics, aerospace, and automotive manufacturing.

[0003] However, existing silicone pressure-sensitive adhesives still have many shortcomings when bonding low surface energy materials, failing to meet the comprehensive requirements of high-end applications for adhesion, heat resistance, and flame retardancy. The core deficiencies of existing technologies are mainly reflected in the following five aspects: First, the adhesion is insufficient. Existing silicone pressure-sensitive adhesives generally have low peel strength to low surface energy materials, making it difficult to achieve reliable adhesion and limiting their application in fields such as electronic packaging and flexible circuits. Secondly, the interface adaptability is poor. The molecular chain structure of existing silicone pressure-sensitive adhesives is fixed, and they cannot adaptively spread to the surface of low surface energy substrates when pressure is applied, resulting in limited contact area and weak interfacial adhesion. Third, it is difficult to balance cohesion and initial tack. Most of the existing silicone pressure-sensitive adhesives have a single curing mechanism. Either the cohesion is insufficient, resulting in poor tack, or the excessive crosslinking leads to loss of initial tack, making it difficult to achieve a balance between the two. Fourth, the heat resistance is limited. Existing silicone pressure-sensitive adhesives are prone to thermal degradation and residue when used for a long time at temperatures above 200°C, which cannot meet the needs of high-temperature application scenarios. Fifth, the lack of flame retardant properties means that very few existing silicone pressure-sensitive adhesives possess flame retardant functions, posing safety hazards when used in fields such as electronics and electrical appliances.

[0004] Therefore, in order to overcome the shortcomings of the prior art, the present invention proposes a method for preparing an organosilicon pressure-sensitive adhesive and tape for bonding low surface energy materials, thereby achieving high-strength bonding of low surface energy materials and simultaneously imparting heat resistance and flame retardancy to the pressure-sensitive adhesive. Summary of the Invention

[0005] The purpose of this invention is to overcome the shortcomings of existing silicone pressure-sensitive adhesives, such as insufficient adhesion to low surface energy materials, poor interface adaptability, difficulty in balancing cohesion and initial tack, limited heat resistance, and lack of flame retardancy. This invention provides a method for preparing silicone pressure-sensitive adhesives and tapes for bonding low surface energy materials. Through multi-component synergy and a dual crosslinking mechanism, this method achieves high-strength bonding of low surface energy materials and imparts excellent heat resistance and flame retardancy.

[0006] To achieve the above objectives, the present invention provides the following technical solution: The technical solution provided by this invention is: An organosilicon pressure-sensitive adhesive for bonding low surface area materials is made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane, 50-110 parts of long-chain alkyl-modified MQ silicone resin, 3-15 parts of fluorosilicone block copolymer, 1-8 parts of mercaptopropyl-modified hydroxyl silicone oil, 0.5-5 parts of a composite crosslinking agent composed of hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin in a weight ratio of 1:0.3-1.5, 1-10 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier, 0.5-5 parts of carborane-modified hydroxyl silicone oil, 3-15 parts of a composite flame retardant composed of hexaphenoxycyclotriphosphazene and phenyl silicone oil in a weight ratio of 1:0.5-2, 0.1-3 parts of ultraviolet photoinitiator, 0.05-0.5 parts of platinum catalyst, and 100-300 parts of organic solvent.

[0007] The phenylboronic acid ester-modified hydroxyl-terminated polydimethylsiloxane has a number average molecular weight of 10,000-80,000. Its molecular chain contains phenylboronic acid ester side groups, which are connected to the silicon atoms of the siloxane backbone via propylene groups. The phenylboronic acid ester side groups account for 1%-8% of the total molar number of siloxane segments, with the remaining siloxane segments being dimethylsiloxane segments. The preparation method of the phenylboronic acid ester-modified hydroxyl-terminated polydimethylsiloxane is as follows: [The text abruptly ends here, so the translation stops.] Hydroxyl-terminated polydimethylsiloxane with methylhydrosiloxane segments is mixed with pinacol ester of allyl phenyl borate at a molar ratio of 1:1.05-1.2 (silicon-hydrogen bond to allyl group). A platinum catalyst containing 10-50 ppm of polydimethylsiloxane with methylhydrosiloxane segments is added. The mixture is stirred at 150-250 r / min for 2-4 h at 80-90 °C. Unreacted substances are removed by vacuum distillation at 110-120 °C for 1-2 h.

[0008] In the long-chain alkyl-modified MQ silicone resin, the organic groups of the M unit are composed of methyl, vinyl and long-chain alkyl with 8-18 carbon atoms, wherein the long-chain alkyl accounts for 5%-25% of the total molar number of the organic groups of the M unit, the vinyl accounts for 1%-10% of the total molar number of the organic groups of the M unit, and the remainder is methyl; the M / Q molar ratio of the MQ silicone resin is 0.6-1.2; the preparation method of the long-chain alkyl-modified MQ silicone resin is as follows: hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane and long-chain alkyl dimethylchlorosilane with 8-18 carbon atoms are mixed according to the designed ratio, tetraethyl orthosilicate is added as the source of Q unit, toluene is used as solvent, deionized water is added dropwise at 0-5℃, the temperature is raised to 70-80℃ and refluxed for 4-6 hours, the aqueous layer is removed by separation, the organic layer is washed with deionized water until neutral, and the solvent is removed by vacuum distillation to obtain the product.

[0009] The fluorosilicone block copolymer is a hydroxyl-terminated polymethyltrifluoropropylsiloxane-polydimethylsiloxane-polymethyltrifluoropropylsiloxane triblock copolymer with a number average molecular weight of 5000-30000, wherein the degree of polymerization of the polymethyltrifluoropropylsiloxane block is 3-15 and the degree of polymerization of the polydimethylsiloxane block is 20-80. The preparation method of the fluorosilicone block copolymer is as follows: using a hydroxyl-terminated polydimethylsiloxane with a number average molecular weight of 5000-15000 as a macromolecular initiator, adding a methyltrifluoropropylcyclotrisiloxane monomer and an alkali metal hydroxide catalyst, stirring at 120-140℃ and 200-300 r / min for 6-10 h, heating to 150-160℃ for 1-2 h for inactivation, and removing low molecular weight substances by vacuum distillation to obtain the copolymer.

[0010] The mercaptopropyl modified hydroxyl silicone oil has a mercapto content of 0.5%-3.0% and a number-average molecular weight of 1000-10000 for the hydroxyl silicone oil portion. The preparation method of the mercaptopropyl modified hydroxyl silicone oil is as follows: hydroxyl silicone oil containing methylhydrosiloxane linkages is mixed with an allyl mercapto compound at a molar ratio of 1:1.0-1.2 between silane bonds and allyl groups. A platinum catalyst with a mass of 10-30 ppm of the hydroxyl silicone oil containing methylhydrosiloxane linkages is added. The mixture is stirred at 70-85℃ and 150-250 r / min for 2-4 h. Unreacted substances are removed by vacuum distillation at 100-110℃ for 1-2 h.

[0011] In the composite crosslinking agent, the hydrogen content of the hydrogen-containing silicone oil is 0.1%-1.6%, the hydrogen content of the methyl hydrogen-containing MQ silicone resin is 0.5%-1.6%, and the M / Q molar ratio is 0.6-1.0. The preparation method of the composite crosslinking agent is as follows: add the hydrogen-containing silicone oil and the methyl hydrogen-containing MQ silicone resin into a mixer at a weight ratio of 1:0.3-1.5, stir at 200-400 r / min for 30-60 minutes at room temperature, and mix evenly to obtain the final product.

[0012] The epoxy-silane-phenylsilane co-condensation oligomer tackifier is formed by partial co-hydrolysis condensation of epoxy-silane and phenylsilane coupling agent, with a weight ratio of epoxy-silane to phenylsilane coupling agent of 1:0.3-1 and a degree of polymerization of 3-6; the epoxy-silane is selected from one or more of γ-glycidyl etheroxypropyltrimethoxysilane and γ-glycidyl etheroxypropyltriethoxysilane; the phenylsilane coupling agent is selected from phenyltrimethoxysilane and diphenyldimethoxysilane. The epoxy silane-phenyl silane co-condensation oligomer thickener is prepared by mixing epoxy silane and phenyl silane coupling agent at a weight ratio of 1:0.3-1, adding methanol or ethanol as solvent, adding strong acid cation exchange resin as catalyst, stirring and reacting at 20-80℃ for 2-6 hours to carry out partial co-hydrolysis condensation, filtering to remove strong acid cation exchange resin, and removing solvent and low volatile matter by vacuum distillation to obtain the product.

[0013] In the carborane-modified hydroxyl silicone oil, the carborane alkyl group is linked to the silicon atom of the siloxane backbone via propylene groups. The carborane alkyl group accounts for 1%-10% of the total molar number of siloxane segments, and the number average molecular weight of the hydroxyl silicone oil portion is 2000-15000. The preparation method of the carborane-modified hydroxyl silicone oil is as follows: first, allyl carborane is prepared by reacting o-carborane with allyl bromide under nitrogen protection and alkaline conditions. Then, allyl carborane is mixed with hydroxyl silicone oil containing methylhydrosiloxane segments at a molar ratio of 1:1.0-1.1 between silane-hydrogen bonds and allyl groups. A platinum catalyst with a mass of 15-40 ppm of hydroxyl silicone oil containing methylhydrosiloxane segments is added. The mixture is stirred at 80-95℃ and 150-250 r / min for 3-6 h. The mixture is then heated to 110-120℃ and distilled under reduced pressure for 1-2 h to remove unreacted substances, thus obtaining the final product.

[0014] In the composite flame retardant, hexaphenoxycyclotriphosphazene is an additive-type halogen-free phosphorus-nitrogen flame retardant, and the phenyl silicone oil is methylphenyl silicone oil with a number average molecular weight of 500-5000. The preparation method of the composite flame retardant is as follows: hexaphenoxycyclotriphosphazene and phenyl silicone oil are added to a mixer at a weight ratio of 1:0.5-2, and stirred at 300-500 r / min for 1-2 hours at 80-100℃ to completely dissolve the hexaphenoxycyclotriphosphazene in the phenyl silicone oil, and then cooled to room temperature to obtain the final product.

[0015] The ultraviolet photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl diphenylphosphine oxide; the platinum catalyst is selected from chloroplatinic acid-isopropanol complex or platinum-divinyltetramethyldisiloxane complex; and the organic solvent is selected from toluene, xylene, n-heptane, or mixtures thereof.

[0016] This invention also provides a silicone pressure-sensitive adhesive tape for bonding low surface area materials, comprising a substrate layer and a silicone pressure-sensitive adhesive layer coated on at least one surface of the substrate layer. The silicone pressure-sensitive adhesive layer is formed by coating, UV-initiated thiol-olefin crosslinking, and hydrosilylation crosslinking of the aforementioned silicone pressure-sensitive adhesive. The dry adhesive thickness of the silicone pressure-sensitive adhesive layer is 20-100 μm. The substrate layer is selected from one of polyimide film, polyester film, polytetrafluoroethylene film, or glass cloth. After curing, the silicone pressure-sensitive adhesive layer has a surface energy gradient structure, i.e., the surface energy of the adhesive layer near the substrate layer is higher than that near the bonding surface. The tape has a 180° peel strength ≥3.0 N / cm at 25°C for low surface area materials with a surface energy ≤30 mN / m. The tape is flame-retardant with a limiting oxygen index ≥28%.

[0017] This invention also provides a method for preparing the above-mentioned low-surface-area adhesive silicone pressure-sensitive adhesive, comprising the following steps: S1: Mix phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with an organic solvent and stir until completely dissolved to obtain the base solution; S2: Add long-chain alkyl-modified MQ silicone resin to the base liquid obtained in step S1, stir at 200-500 r / min at 60-90℃ for 2-4 hours, and cool to room temperature; S3: Add the fluorosilicone block copolymer to the mixture obtained in step S2, stir at 40-60°C for 1-2 hours, and then let it stand at room temperature for 0.5-1 hours to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add mercaptopropyl modified hydroxyl silicone oil, epoxy silane-phenyl silane cocondensation oligomer tackifier, carborane modified hydroxyl silicone oil and composite flame retardant to the mixture obtained in step S3, and stir at 50-60℃ for 30-60 minutes. S5a: Add a UV photoinitiator to the mixture obtained in step S4, stir at 40-50℃ for 10-20 minutes to obtain component A; take the base liquid obtained in step S1, add a composite crosslinking agent and a platinum catalyst, stir at 40-50℃ for 10-20 minutes to obtain component B; S5b: Mix component A and component B rapidly at a weight ratio of (8-12):1, stir for 2-5 minutes, and degas to obtain the silicone pressure-sensitive adhesive liquid.

[0018] Components A and B are stored separately and mixed only before coating to modify the hydroxyl groups with mercaptopropyl groups.

[0019] This invention also provides a method for preparing the above-mentioned low-surface-area adhesive silicone pressure-sensitive tape. The prepared silicone pressure-sensitive adhesive liquid is coated onto the surface of a substrate layer. After irradiation with ultraviolet light, free radicals generated by an ultraviolet photoinitiator initiate thiol-olefin click chemical crosslinking between the mercaptopropyl-modified hydroxyl silicone oil and the vinyl groups in the long-chain alkyl-modified MQ silicone resin. The ultraviolet light wavelength is 254-365 nm, and the irradiation dose is 500-2000 mJ / cm². 2 The mercaptan-olefin click crosslinking reduces the free thiol content to below 0.01%, eliminating the risk of thiol poisoning of the platinum catalyst. Then, heating at 60-90℃ for 1-3 hours allows the Si-H bonds in the composite crosslinking agent to undergo hydrosilylation crosslinking with the vinyl groups in the long-chain alkyl-modified MQ silicone resin under the action of a platinum catalyst, resulting in the organosilicon pressure-sensitive tape.

[0020] The beneficial effects of this technical solution are: (1) This technical solution uses phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane as the base polymer. The phenylboronic acid ester side groups in its molecular chain have dynamic reversible characteristics. When pressure is applied, the phenylboronic acid ester bonds can undergo reversible rearrangement at the interface, so that the molecular chain can adaptively spread to the surface of the low surface energy substrate, significantly increasing the contact area and interfacial adhesion. At the same time, the phenyl groups in the phenylboronic acid ester generate enhanced interactions with the surface of nonpolar low surface energy materials through van der Waals forces, which is different from the disadvantage of the fixed network structure in the prior art that cannot adaptively spread.

[0021] (2) The triblock structure design of the fluorosilicone block copolymer is one of the core advantages of this technology. During the coating and drying process, the polymethyltrifluoropropylsiloxane blocks migrate directionally to the air interface, which reduces the surface energy of the adhesive layer bonding side and forms a surface energy gradient from the substrate side to the bonding side, thereby enhancing the wettability of the low surface energy substrate. The hydroxyl end capping ensures that the copolymer is anchored in the network through chemical crosslinking and does not migrate or lose, which is different from the problem of easy migration and short-lasting effect of simple blending of fluorosilicone modifiers in the prior art.

[0022] (3) This invention uses a two-component packaging and step-by-step curing process to solve the compatibility problem of thiol-platinum catalysts. The mercaptopropyl-modified hydroxyl silicone oil and the vinyl groups in the long-chain alkyl-modified MQ silicone resin undergo click chemical crosslinking of thiol-olefin under ultraviolet light initiation, forming the first crosslinking network. After the thiol-olefin reaction is completed, the free mercapto groups are almost completely consumed (residual amount <0.01%), and no longer poison the platinum catalyst. The Si-H bonds in the composite crosslinking agent and the vinyl groups in the MQ resin undergo hydrosilylation crosslinking under platinum catalysis, forming the second crosslinking network. Component A contains mercaptopropyl-modified hydroxyl silicone oil and an ultraviolet initiator, and component B contains a platinum catalyst and a composite crosslinking agent. They are rapidly mixed before coating, and the coexistence time of mercapto groups and the platinum catalyst is controlled within 5 minutes. The thiol-olefin reaction is completed within a few seconds to tens of seconds after ultraviolet irradiation, effectively avoiding the poisoning of the platinum catalyst by mercapto groups. The dual crosslinking mechanism works synergistically: the thiol-olefin reaction is highly efficient, produces no byproducts, and allows for rapid initial curing under UV light, facilitating winding; the hydrosilylation crosslinking can controllably supplement cohesive strength under heating. This dual crosslinking design is more effective than a single curing system in balancing both initial tack and holding power.

[0023] (4) The carborane cage structure in the carborane-modified hydroxyl silicone oil has a unique electronic vacancy feature. Its boron atoms have an affinity with the surface of fluorine-containing materials such as polytetrafluoroethylene, which can enhance the interfacial adhesion. The high thermal stability (>600℃) of the carborane skeleton significantly improves the temperature resistance of the pressure-sensitive adhesive. The boron atoms in the carborane-modified hydroxyl silicone oil have an affinity with the P=O groups of phosphazene in the composite flame retardant, which can enhance the interfacial compatibility of the flame retardant. This is different from the problem of insufficient interfacial enhancement and heat resistance of organosilicon pressure-sensitive adhesives in the prior art.

[0024] (5) The composite flame retardant is composed of hexaphenoxycyclotriphosphazene and phenyl silicone oil pre-dissolved composite. The phenyl in the phenyl silicone oil and the six phenoxy groups on the phosphazene molecule enhance compatibility through π-π conjugation, so that the phosphazene is stably dispersed in the organosilicon system without precipitation. The phosphorus-nitrogen synergistic flame retardant mechanism of hexaphenoxycyclotriphosphazene (condensed phase char formation + gas phase free radical capture + dilution flame retardant triple mechanism) endows the pressure-sensitive adhesive with excellent flame retardant properties, which is different from the problem that organosilicon pressure-sensitive adhesives in the prior art rarely have flame retardant functions.

[0025] (6) In the epoxy silane-phenyl silane cocondensation oligomer tackifier, the phenyl and the phenyl borate ester modified PDMS side group enhance compatibility through π-π conjugation. The epoxy group reacts with the residual hydroxyl group of MQ resin and the trace polar groups on the surface of low surface energy materials to form a chemical anchor. The oligomer form avoids the migration and volatilization of small molecule silanes, which is different from the problem of easy migration and unsustainable tackifying effect of silane coupling agents when added directly in the prior art.

[0026] (7) The composite crosslinking agent is composed of hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin in a specific ratio. The hydrogen-containing silicone oil provides flexible crosslinking points, and the methyl hydrogen-containing MQ silicone resin provides rigid crosslinking points. The dual-scale crosslinking with both rigidity and flexibility can effectively control the crosslinking density and mechanical properties, which is different from the problem that single hydrogen-containing silicone oil crosslinking in the existing technology cannot take into account both flexibility and cohesion. Detailed Implementation

[0027] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] The specific implementation process is as follows: In the various embodiments and comparative examples, the preparation method of hydroxyl-terminated polydimethylsiloxane modified with phenylboronic acid ester is as follows: hydroxyl-terminated polydimethylsiloxane containing methylhydrosiloxane linkages is mixed with allyl phenylboronic acid pinacol ester at a molar ratio of 1:1.1 between silane-hydrogen bonds and allyl groups. A platinum catalyst (platinum-divinyltetramethyldisiloxane complex) with a mass of 30 ppm of polydimethylsiloxane containing methylhydrosiloxane linkages is added. The mixture is stirred at 200 r / min at 85 °C for 3 h, and then heated to 115 °C and distilled under reduced pressure for 1.5 h to remove unreacted substances, thus obtaining the product.

[0029] In the various embodiments and comparative examples, the preparation method of long-chain alkyl modified MQ silicone resin is as follows: hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane and octadecyldimethylchlorosilane are mixed according to the designed ratio, tetraethyl orthosilicate is added as the source of Q units, toluene is used as solvent, deionized water is added dropwise at 3°C, the temperature is raised to 75°C and refluxed for 5 hours, the aqueous layer is removed by separation, the organic layer is washed with deionized water until neutral, and the solvent is removed by vacuum distillation to obtain the product.

[0030] In the various embodiments and comparative examples, the preparation method of the fluorosilicone block copolymer is as follows: using a dihydroxyl-terminated polydimethylsiloxane with a number average molecular weight of 10,000 as a macromolecular initiator, adding methyltrifluoropropylcyclotrisiloxane monomer and potassium hydroxide catalyst, stirring at 250 r / min for 8 h at 130 °C, heating to 155 °C for 1.5 h for inactivation, and removing low molecular weight substances by vacuum distillation to obtain the copolymer.

[0031] In the various embodiments and comparative examples, the preparation method of mercaptopropyl modified hydroxyl silicone oil is as follows: hydroxyl silicone oil containing methylhydrosiloxane linkages is mixed with allyl mercapto compound at a molar ratio of 1:1.1 between silane-hydrogen bonds and allyl groups. A platinum catalyst with a mass of 20 ppm of hydroxyl silicone oil containing methylhydrosiloxane linkages is added. The mixture is stirred at 200 r / min at 78°C for 3 h. The mixture is then heated to 105°C and distilled under reduced pressure for 1.5 h to remove unreacted substances, thus obtaining the product.

[0032] In each embodiment and comparative example, the composite crosslinking agent was prepared by adding hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin into a mixer in a weight ratio, stirring at 300 r / min for 45 minutes at room temperature until uniformly mixed.

[0033] In the various embodiments and comparative examples, the preparation method of the epoxy silane-phenyl silane cocondensation oligomer tackifier is as follows: γ-glycidyl etheroxypropyltrimethoxysilane, phenyltrimethoxysilane, diphenyldimethoxysilane, and methylphenyldimethoxysilane are mixed in a weight ratio, ethanol is added as a solvent, a strong acid cation exchange resin is added as a catalyst, and the mixture is stirred at 50°C for 4 hours to carry out partial co-hydrolysis condensation. The strong acid cation exchange resin is removed by filtration, and the solvent and low volatile matter are removed by vacuum distillation to obtain the final product.

[0034] In the various embodiments and comparative examples, the preparation method of carborane-modified hydroxyl silicone oil is as follows: first, o-carborane is reacted with allyl bromide under nitrogen protection and sodium hydroxide conditions to obtain allyl carborane; then, allyl carborane is mixed with hydroxyl silicone oil containing methylhydrosiloxane links at a molar ratio of 1:1.05 between silane-hydrogen bonds and allyl groups; 25 ppm of platinum catalyst containing methylhydrosiloxane links is added; the mixture is stirred at 200 r / min at 88°C for 4 h; and then heated to 115°C and distilled under reduced pressure for 1.5 h to remove unreacted substances, thus obtaining the product.

[0035] In each embodiment and comparative example, the composite flame retardant was prepared by adding hexaphenoxycyclotriphosphazene and phenyl silicone oil into a mixer in a weight ratio, stirring at 400 r / min for 1.5 hours at 90°C to completely dissolve the hexaphenoxycyclotriphosphazene in the phenyl silicone oil, and then cooling to room temperature.

[0036] The specific implementation process is as follows: Example 1:

[0037] This invention provides a technical solution: an organosilicon pressure-sensitive adhesive for bonding low surface area materials, made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane (number average molecular weight 10000, phenylboronic acid ester side groups accounting for 1% of the total molar number of siloxane chain segments), 50 parts of long-chain alkyl-modified MQ silicone resin (long-chain alkyl is octadecyl, accounting for 5% of the total molar number of M unit organic groups, vinyl accounts for 1% of the total molar number of M unit organic groups, M / Q molar ratio is 0.6), 3 parts of fluorosilicone block copolymer (polymethyltrifluoropropylsiloxane block polymerization degree of 3, polydimethylsiloxane block polymerization degree of 20), 1 part of mercaptopropyl-modified hydroxyl silicone oil (mercaptoyl content 0.5%, hydroxyl silicone oil part number average molecular weight 1000), and 0.5 parts of composite crosslinking agent (hydrogen content of hydrogen-containing silicone oil 0). 0.1%, methyl hydrogen-containing MQ silicone resin with hydrogen content of 0.5% and M / Q molar ratio of 0.6 (weight ratio of 1:0.3), 1 part epoxy silane-phenyl silane cocondensation oligomer tackifier (γ-glycidyl ether oxypropyltrimethoxysilane and phenyl silane coupling agent weight ratio of 1:0.3, degree of polymerization of 3), 0.5 parts carborane modified hydroxyl silicone oil (carborane alkyl groups account for 1% of the total molar number of siloxane segments, number average molecular weight of hydroxyl silicone oil is 2000), 3 parts composite flame retardant (hexaphenoxycyclotriphosphazene and methyl phenyl silicone oil with a number average molecular weight of 500 weight ratio of 1:0.5), 0.1 parts ultraviolet photoinitiator (2-hydroxy-2-methyl-1-phenyl-1-propanone), 0.05 parts platinum catalyst (platinum-divinyltetramethyldisiloxane complex), and 100 parts organic solvent (toluene).

[0038] Its preparation method includes the following steps: S1: Mix 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with 100 parts of toluene and stir until completely dissolved to obtain the base solution; S2: Add 50 parts of long-chain alkyl modified MQ silicone resin to the base liquid obtained in step S1, stir at 200 r / min at 60℃ for 4 hours, and cool to room temperature; S3: Add 3 parts of fluorosilicone block copolymer to the mixture obtained in step S2, stir at 40°C for 2 hours, and then let stand at room temperature for 1 hour to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add 1 part mercaptopropyl modified hydroxyl silicone oil, 1 part epoxy silane-phenyl silane cocondensation oligomer tackifier, 0.5 part carborane modified hydroxyl silicone oil and 3 parts composite flame retardant to the mixture obtained in step S3, and stir at 50°C for 60 minutes. S5a: Add 0.1 parts of ultraviolet photoinitiator to the mixture obtained in step S4, stir at 40°C for 15 minutes to obtain component A; take another base liquid obtained in step S1, add 0.5 parts of composite crosslinking agent and 0.05 parts of platinum catalyst, stir at 40°C for 15 minutes to obtain component B; S5b: Mix component A and component B rapidly at a weight ratio of 10:1, stir for 3 minutes, and then perform vacuum degassing treatment (vacuum degree -0.09MPa, degassing time 30 minutes) to obtain the silicone pressure-sensitive adhesive liquid; The silicone pressure-sensitive adhesive was coated onto the surface of a polyimide film, with a dry adhesive thickness of 20 μm. The film was then irradiated with ultraviolet light (wavelength 365 nm, irradiation dose 500 mJ / cm²). 2 The free radicals generated by the ultraviolet photoinitiator initiate the mercapto-alkene click chemical crosslinking of mercaptopropyl modified hydroxy silicone oil with vinyl groups in long-chain alkyl modified MQ silicone resin. The free mercapto groups are consumed under ultraviolet light. Then, heating at 60°C for 3 hours allows the Si-H bonds in the composite crosslinking agent to complete the hydrosilylation crosslinking of vinyl groups in long-chain alkyl modified MQ silicone resin under the action of a platinum catalyst, thus obtaining the organosilicon pressure-sensitive tape.

[0039]

[0040] The experimental data above show that the silicone pressure-sensitive tape prepared in Example 1 meets all the design requirements. The 180° peel strength against PTFE reaches 3.2 N / cm, far exceeding the typical peel strength (<1.5 N / cm) of existing silicone pressure-sensitive adhesives against low surface energy materials. This indicates that the triple mechanism of interfacial self-adaptation of the phenylboronic acid ester dynamic bonds, carborane interfacial affinity, and fluorosilicone surface energy gradient effectively enhances the adhesion to fluorinated materials. The peel strengths against PE and PP are 3.5 N / cm and 3.8 N / cm, respectively, further verifying its wide applicability to different low surface energy materials. The initial tack is 8 N, and the holding power reaches 48 h, indicating that the dual crosslinking of thiol-olefin and hydrosilylation achieves a good balance between initial tack and holding power. The limiting oxygen index is 28.2%, meeting the flame retardant requirements. The peel strength retention rate after 200℃ / 72h is 85.3%, indicating that the carborane cage structure effectively improves the heat resistance. In summary, Example 1, using the lower limit ratio and process parameters, meets the basic requirements for various performance aspects, thus verifying the feasibility of the technical solution of the present invention.

[0041] Example 2:

[0042] This invention provides a technical solution: an organosilicon pressure-sensitive adhesive for bonding low surface area materials, made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane (number average molecular weight 45,000, phenylboronic acid ester side groups accounting for 4.5% of the total molar number of siloxane units), 80 parts of long-chain alkyl-modified MQ silicone resin (long-chain alkyl is octadecyl, accounting for 15% of the total molar number of M unit organic groups, vinyl accounts for 5% of the total molar number of M unit organic groups, M / Q molar ratio is 0.9), 9 parts of fluorosilicone block copolymer (polymethyltrifluoropropylsiloxane block polymerization degree of 9, polydimethylsiloxane block polymerization degree of 50), 4.5 parts of mercaptopropyl-modified hydroxyl silicone oil (mercaptopropyl content 1.8%, hydroxyl silicone oil part number average molecular weight 5,500), and 2.75 parts of composite crosslinking agent (hydrogen content of hydrogen in hydrogen-containing silicone oil 0.85%, methyl hydrogen content of hydrogen-containing silicone oil). The composition includes: MQ silicone resin with 1.05% hydrogen content and an M / Q molar ratio of 0.8 (weight ratio of 1:0.9); 5.5 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier (γ-glycidyl etheroxypropyltrimethoxysilane and phenyl silane coupling agent in a weight ratio of 1:0.65, degree of polymerization 4.5); 2.75 parts of carborane-modified hydroxyl silicone oil (carborane alkyl groups account for 5.5% of the total molar number of siloxane segments, hydroxyl silicone oil fraction with a number average molecular weight of 8500); 9 parts of composite flame retardant (hexaphenoxycyclotriphosphazene and methylphenyl silicone oil with a number average molecular weight of 2750 in a weight ratio of 1:1.25); 1.55 parts of ultraviolet photoinitiator (1-hydroxycyclohexylphenyl ketone); 0.275 parts of platinum catalyst (platinum-divinyltetramethyldisiloxane complex); and 200 parts of organic solvent (toluene and n-heptane mixed solvent in a weight ratio of 3:1).

[0043] Its preparation method includes the following steps: S1: Mix 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with 200 parts of mixed solvent and stir until completely dissolved to obtain the base solution; S2: Add 80 parts of long-chain alkyl modified MQ silicone resin to the base liquid obtained in step S1, stir at 350 r / min at 75°C for 3 hours, and cool to room temperature; S3: Add 9 parts of fluorosilicone block copolymer to the mixture obtained in step S2, stir at 50°C for 1.5 hours, and then let stand at room temperature for 0.75 hours to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add 4.5 parts of mercaptopropyl modified hydroxyl silicone oil, 5.5 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier, 2.75 parts of carborane modified hydroxyl silicone oil and 9 parts of composite flame retardant to the mixture obtained in step S3, and stir at 55°C for 45 minutes. S5a: Add 1.55 parts of ultraviolet photoinitiator to the mixture obtained in step S4, stir at 45°C for 15 minutes to obtain component A; take the base liquid obtained in step S1, add 2.75 parts of composite crosslinking agent and 0.275 parts of platinum catalyst, stir at 45°C for 15 minutes to obtain component B; S5b: Mix component A and component B rapidly at a weight ratio of 10:1, stir for 3 minutes, and then perform vacuum degassing treatment (vacuum degree -0.09MPa, degassing time 20 minutes) to obtain the silicone pressure-sensitive adhesive liquid; The silicone pressure-sensitive adhesive was coated onto the surface of a polyimide film, with a dry adhesive thickness of 60 μm. The film was then irradiated with ultraviolet light (wavelength 365 nm, irradiation dose 1250 mJ / cm²). 2 The free radicals generated by the ultraviolet photoinitiator initiate the mercapto-alkene click chemical crosslinking of mercaptopropyl modified hydroxy silicone oil with vinyl groups in long-chain alkyl modified MQ silicone resin. The free mercapto groups are consumed under ultraviolet light. Then, heating at 75°C for 2 hours allows the Si-H bonds in the composite crosslinking agent to complete the hydrosilylation crosslinking of vinyl groups in long-chain alkyl modified MQ silicone resin under the action of a platinum catalyst, thus obtaining the organosilicon pressure-sensitive tape.

[0044]

[0045] The silicone pressure-sensitive tape prepared in Example 2 showed significantly better performance than that of Example 1, with outstanding performance in core indicators. Specifically, the 180° peel strength against PTFE reached 5.8 N / cm, an 81% improvement compared to Example 1. This indicates that the optimal effect is achieved through a synergistic four-mechanism approach: the interfacial self-adaptation of the dynamic bonds of phenylboronic ester, the interfacial affinity of carborane, the surface energy gradient of fluorosilicone, and the chemical anchoring of the epoxy silane-phenyl silane co-condensation oligomer tackifier. The peel strengths against PE and PP were 6.2 N / cm and 6.5 N / cm, respectively, also showing a significant improvement. The initial tack was 12 N, and the holding power was 96 h, with the optimal balance between initial tack and holding power achieved through dual crosslinking of thiol-olefin and hydrosilylation. The limiting oxygen index was 32.5%, demonstrating a significant phosphorus-nitrogen synergistic flame retardant effect, meeting the UL94V-0 requirement. The peel strength retention rate after 200℃ / 72 h was 92.1%, highlighting the excellent dual protection of heat resistance and flame retardancy provided by the carborane cage structure and phosphazene. In summary, Example 2, by using intermediate ratios and process parameters, achieved optimal performance in all aspects, fully demonstrating the synergistic effect of the technical solution of this invention.

[0046] Example 3:

[0047] This invention provides a technical solution: an organosilicon pressure-sensitive adhesive for bonding low surface area materials, made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane (number average molecular weight 80,000, phenylboronic acid ester side groups accounting for 8% of the total molar number of siloxane units), 110 parts of long-chain alkyl-modified MQ silicone resin (long-chain alkyl is octadecyl, accounting for 25% of the total molar number of M unit organic groups, vinyl accounts for 10% of the total molar number of M unit organic groups, M / Q molar ratio is 1.2), 15 parts of fluorosilicone block copolymer (polymethyltrifluoropropylsiloxane block polymerization degree of 15, polydimethylsiloxane block polymerization degree of 80), 8 parts of mercaptopropyl-modified hydroxyl silicone oil (mercaptoyl content 3.0%, hydroxyl silicone oil part number average molecular weight 10,000), and 5 parts of composite crosslinking agent (hydrogen content of hydrogen in hydrogen-containing silicone oil 1.6%). %, methyl hydrogen-containing MQ silicone resin with hydrogen content of 1.6% and M / Q molar ratio of 1.0, with a weight ratio of 1:1.5), 10 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier (γ-glycidyl ether oxypropyltrimethoxysilane and phenyl silane coupling agent in a weight ratio of 1:1, degree of polymerization of 6), 5 parts of carborane modified hydroxyl silicone oil (carborane alkyl groups account for 10% of the total molar number of siloxane segments, and the number average molecular weight of the hydroxyl silicone oil portion is 15000), 15 parts of composite flame retardant (hexaphenoxycyclotriphosphazene and methyl phenyl silicone oil with a number average molecular weight of 5000 in a weight ratio of 1:2), 3 parts of ultraviolet photoinitiator (2,4,6-trimethylbenzoyl diphenylphosphine oxide), 0.5 parts of platinum catalyst (chloroplatinic acid-isopropanol complex), and 300 parts of organic solvent (toluene and xylene mixed solvent in a weight ratio of 1:1).

[0048] Its preparation method includes the following steps: S1: Mix 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with 300 parts of mixed solvent and stir until completely dissolved to obtain the base solution; S2: Add 110 parts of long-chain alkyl modified MQ silicone resin to the base liquid obtained in step S1, stir at 500 r / min at 90°C for 2 hours, and cool to room temperature; S3: Add 15 parts of fluorosilicone block copolymer to the mixture obtained in step S2, stir at 60°C for 1 hour, and then let stand at room temperature for 0.5 hours to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add 8 parts of mercaptopropyl modified hydroxyl silicone oil, 10 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier, 5 parts of carborane modified hydroxyl silicone oil and 15 parts of composite flame retardant to the mixture obtained in step S3, and stir at 60°C for 30 minutes. S5a: Add 3 parts of ultraviolet photoinitiator to the mixture obtained in step S4, stir at 50°C for 10 minutes to obtain component A; take another base liquid obtained in step S1, add 5 parts of composite crosslinking agent and 0.5 parts of platinum catalyst, stir at 50°C for 10 minutes to obtain component B; S5b: Mix component A and component B rapidly at a weight ratio of 10:1, stir for 2 minutes, and then perform vacuum degassing treatment (vacuum degree -0.1MPa, degassing time 10 minutes) to obtain the silicone pressure-sensitive adhesive liquid; The silicone pressure-sensitive adhesive was coated onto the surface of a polyester film, with a dry adhesive thickness of 100 μm. The film was then irradiated with ultraviolet light (wavelength 254 nm, irradiation dose 2000 mJ / cm²). 2 The free radicals generated by the ultraviolet photoinitiator initiate the mercapto-alkene click chemical crosslinking of mercaptopropyl modified hydroxy silicone oil with vinyl groups in long-chain alkyl modified MQ silicone resin. The free mercapto groups are consumed under ultraviolet light. Then, heating at 90°C for 1 hour allows the Si-H bonds in the composite crosslinking agent to complete the hydrosilylation crosslinking of vinyl groups in long-chain alkyl modified MQ silicone resin under the action of a platinum catalyst, thus obtaining the organosilicon pressure-sensitive tape.

[0049]

[0050] The silicone pressure-sensitive tape prepared in Example 3 met all design requirements, and its overall performance was better than that of Example 1, while some indicators were slightly lower than those of Example 2, which is consistent with the variation law of the ratio and process parameters. Specifically, the 180° peel strength against PTFE was 5.2 N / cm, higher than that of Example 1 but lower than that of Example 2. This is mainly because the crosslinking density was higher at the upper limit ratio, resulting in enhanced cohesion but a slight decrease in interfacial adaptability. The peel strength against PE and PP was 5.6 N / cm and 5.9 N / cm, respectively, also better than that of Example 1. The initial tack was 10 N, and the holding power was 72 h. The holding power was better than that of Example 1 but lower than that of Example 2, indicating that the initial tack was somewhat lost when the crosslinking density was too high. The limiting oxygen index was 34.8%, indicating the best flame retardant effect. The increased amount of phosphazene added further improved the flame retardant performance. The peel strength retention rate after 200℃ / 72h was 94.5%, indicating the best heat resistance, and the addition of carborane and phosphazene was sufficient. In summary, Example 3, using the upper limit ratio and process parameters, was still able to stably prepare silicone pressure-sensitive tape with excellent overall performance, further verifying the wide applicability and stability of the technical solution of the present invention.

[0051] Example 4:

[0052] This invention provides a technical solution: an organosilicon pressure-sensitive adhesive for bonding low surface area materials, made from the following raw materials in parts by weight: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane (number average molecular weight 30,000, phenylboronic acid ester side groups accounting for 3% of the total molar number of siloxane units), 65 parts of long-chain alkyl-modified MQ silicone resin (long-chain alkyl is dodecyl, accounting for 10% of the total molar number of M unit organic groups, vinyl accounts for 3% of the total molar number of M unit organic groups, M / Q molar ratio is 0.8), 6 parts of fluorosilicone block copolymer (polymethyltrifluoropropylsiloxane block polymerization degree of 6, polydimethylsiloxane block polymerization degree of 35), 3 parts of mercaptopropyl-modified hydroxyl silicone oil (mercaptopropyl content 1.2%, hydroxyl silicone oil part number average molecular weight 4,000), and 1.5 parts of composite crosslinking agent (hydrogen content of hydrogen in hydrogen-containing silicone oil 0.6%, hydrogen content of methyl hydrogen-containing MQ silicone resin 0.8%). The following components are included: M / Q molar ratio 0.7 (weight ratio of M / Q to phenylsilane 1:0.6); 3 parts epoxy silane-phenyl silane cocondensation oligomer tackifier (γ-glycidyl etheroxypropyltriethoxysilane and phenyl silane coupling agent weight ratio 1:0.5, degree of polymerization 4); 1.5 parts carborane modified hydroxyl silicone oil (carborane alkyl groups account for 3% of the total molar number of siloxane segments, hydroxyl silicone oil fraction number average molecular weight 6000); 6 parts composite flame retardant (hexaphenoxycyclotriphosphazene and methylphenyl silicone oil with a number average molecular weight of 1500 weight ratio 1:1); 0.8 parts ultraviolet photoinitiator (mixture of 1-hydroxycyclohexylphenyl ketone and 2,4,6-trimethylbenzoyl diphenylphosphine oxide in a weight ratio of 2:1); 0.15 parts platinum catalyst (platinum-divinyltetramethyldisiloxane complex); and 150 parts organic solvent (mixture of toluene and n-heptane in a weight ratio of 2:1).

[0053] Its preparation method includes the following steps: S1: Mix 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with 150 parts of mixed solvent and stir until completely dissolved to obtain the base solution; S2: Add 65 parts of long-chain alkyl-modified MQ silicone resin to the base liquid obtained in step S1, stir at 300 r / min at 70°C for 3.5 hours, and cool to room temperature; S3: Add 6 parts of fluorosilicone block copolymer to the mixture obtained in step S2, stir at 45°C for 1.5 hours, and then let stand at room temperature for 0.75 hours to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add 3 parts of mercaptopropyl modified hydroxyl silicone oil, 3 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier, 1.5 parts of carborane modified hydroxyl silicone oil and 6 parts of composite flame retardant to the mixture obtained in step S3, and stir at 52°C for 50 minutes. S5a: Add 0.8 parts of ultraviolet photoinitiator to the mixture obtained in step S4, stir at 42°C for 15 minutes to obtain component A; take another base liquid obtained in step S1, add 1.5 parts of composite crosslinking agent and 0.15 parts of platinum catalyst, stir at 42°C for 15 minutes to obtain component B; S5b: Mix component A and component B rapidly at a weight ratio of 10:1, stir for 3 minutes, and then perform vacuum degassing treatment (vacuum degree -0.09MPa, degassing time 25 minutes) to obtain the silicone pressure-sensitive adhesive liquid; The silicone pressure-sensitive adhesive was coated onto the surface of a polytetrafluoroethylene film, with a dry adhesive thickness of 50 μm. The film was then irradiated with ultraviolet light (wavelength 365 nm, irradiation dose 800 mJ / cm²). 2 The free radicals generated by the ultraviolet photoinitiator initiate the mercapto-alkene click chemical crosslinking of mercaptopropyl modified hydroxy silicone oil with vinyl groups in long-chain alkyl modified MQ silicone resin. The free mercapto groups are consumed under ultraviolet light. Then, heating at 70°C for 2.5 hours allows the Si-H bonds in the composite crosslinking agent to complete the hydrosilylation crosslinking of vinyl groups in long-chain alkyl modified MQ silicone resin under the action of a platinum catalyst, thus obtaining the organosilicon pressure-sensitive tape.

[0054]

[0055] Example 4 uses raw materials with different parameters within a defined range (such as dodecyl instead of octadecyl, different types of epoxy silanes, and combinations of UV photoinitiators), and adjusts the ratio and process parameters. The prepared silicone pressure-sensitive tape still meets all the design requirements, and its overall performance is better than that of Example 1, with some indicators approaching those of Example 2. Specifically, the 180° peel strength against PTFE is 4.8 N / cm, which is better than that of Example 1, indicating that the dodecyl-modified MQ silicone resin can also effectively improve the wettability of low surface energy materials; the peel strength against PE and PP is 5.1 N / cm and 5.4 N / cm, respectively; the initial tack is 11 N, and the holding power is 80 h, indicating that the double crosslinking system maintains a good balance between initial tack and holding power even with adjusted ratios; the limiting oxygen index is 30.5%, indicating good flame retardant properties; and the peel strength retention rate after 200℃ / 72h is 89.7%, showing better heat resistance than that of Example 1. In summary, Example 4 further verifies the flexibility of the technical solution of the present invention. As long as the raw material parameters, proportions and process parameters are within the scope defined by the claims, regardless of the specific values, a silicone pressure-sensitive tape with excellent comprehensive performance can be stably prepared.

[0056] Comparative Example 1: The present invention provides a comparative scheme, which differs from Example 2 in that: it does not contain phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane, but replaces it with an equal amount of ordinary hydroxyl-terminated polydimethylsiloxane (without phenylboronic acid ester side groups); it does not contain fluorosilicone block copolymers; it does not contain carborane-modified hydroxyl silicone oil; it does not contain epoxy silane-phenyl silane cocondensation oligomer tackifiers; it does not contain mercaptopropyl-modified hydroxyl silicone oil; the composite crosslinking agent uses only hydrogen-containing silicone oil (without methyl hydrogen MQ silicone resin), and the amount is the same as the total amount of composite crosslinking agent in Example 2; it does not contain composite flame retardants; the ultraviolet curing is only conventional light curing (without thiol-olefin crosslinking mechanism), and the crosslinking is only completed through hydrosilylation; the remaining raw material ratios and preparation process parameters are completely consistent with Example 2.

[0057]

[0058] Comparative Example 1, due to the use of ordinary hydroxyl-terminated polydimethylsiloxane instead of phenylborane-modified PDMS, lacks fluorosilicone block copolymers, carborane-modified hydroxyl silicone oil, epoxy silane-phenyl silane co-condensation oligomer tackifiers, and composite flame retardants, and employs single hydrosilylation crosslinking, exhibits significantly different performance characteristics compared to Example 2. Its 180° peel strength against PTFE is only 1.2 N / cm, far lower than the 5.8 N / cm of Example 2, indicating the lack of interfacial self-adaptation of phenylborane dynamic bonds, carborane interfacial affinity, and fluorosilicone surface energy gradient. Ordinary silicone pressure-sensitive adhesives are almost ineffective at bonding low surface energy materials. Initial tack is 6 N, and holding power is 36 h; single hydrosilylation crosslinking cannot achieve a balance between initial tack and holding power. The limiting oxygen index is only 22.0%, lacking flame retardancy. After 200℃ / 72h, the peel strength retention rate is 72.5%, indicating a significant decrease in heat resistance due to the lack of carborane heat-enhancing properties. The difference between Comparative Example 1 and Example 2 is very obvious. Without phenyl borate modified PDMS, fluorosilicone block copolymer, carborane modified hydroxyl silicone oil, tackifier, composite flame retardant and dual crosslinking of two-component packaging and step-by-step curing, the pressure-sensitive adhesive can hardly bond effectively on low surface energy materials and does not have flame retardancy.

[0059] Comparative Example 2: The present invention provides a comparative scheme: the difference from Example 2 is that it does not contain fluorine-silicone block copolymer; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0060]

[0061] Comparative Example 2, lacking the fluorosilicone block copolymer, showed a significant decrease in peel strength for low surface energy materials. The 180° peel strength for PTFE decreased from 5.8 N / cm in Example 2 to 4.2 N / cm, a reduction of 27.6%. This indicates that the absence of the surface energy gradient constructed by the fluorosilicone block copolymer prevented effective reduction of surface energy on the adhesive bonding surface, resulting in insufficient wettability, reduced contact area, and decreased interfacial adhesion. Peel strength for PE and PP also decreased significantly. Initial tack and holding tack were largely unaffected, while flame retardancy and heat resistance showed little change, indicating that the fluorosilicone block copolymer primarily affects interfacial wettability rather than the crosslinking network and flame retardant and heat resistance properties. This comparative example demonstrates that the fluorosilicone block copolymer is a key component in constructing a surface energy gradient and enhancing the wettability and adhesion of low surface energy materials.

[0062] Comparative Example 3: The present invention provides a comparative scheme, which differs from Example 2 in that it does not contain carborane-modified hydroxyl silicone oil; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0063]

[0064] Comparative Example 3, lacking carborane-modified hydroxyl silicone oil, showed a 22.4% decrease in the 180° peel strength of PTFE from 5.8 N / cm in Example 2 to 4.5 N / cm, indicating a significant reduction in interfacial adhesion to fluorinated materials due to the absence of carborane interfacial affinity. The decrease in peel strength for PE and PP was smaller because carborane interfacial affinity is primarily effective for fluorinated materials and has less impact on non-fluorinated materials with low surface energy. Regarding heat resistance, the peel strength retention rate after 200℃ / 72h decreased from 92.1% in Example 2 to 82.3%, indicating a decrease in the thermal stability of the crosslinked network at high temperatures due to the lack of heat-enhancing carborane cage structure. This comparative example demonstrates that carborane-modified hydroxyl silicone oil is a key component for enhancing the adhesion and heat resistance of fluorinated materials.

[0065] Comparative Example 4: The present invention provides a comparative scheme, which differs from Example 2 in that it does not contain mercaptopropyl modified hydroxyl silicone oil, and the ultraviolet curing is only conventional light curing (without thiol-olefin crosslinking mechanism), and the crosslinking is only completed through hydrosilylation; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0066]

[0067] Comparative Example 4 lacks mercaptopropyl-modified hydroxyl silicone oil and thus lacks thiol-olefin click chemical crosslinking, relying solely on a hydrosilylation crosslinking mechanism. Furthermore, since the thiol-olefin reaction is unnecessary, this comparative example employs a single-component system. While avoiding the coexistence problem of thiols and platinum catalysts, it sacrifices the advantage of rapid initial curing under UV light. Initial tack decreased from 12N in Example 2 to 8N, and holding power decreased from 96h to 60h, indicating that single hydrosilylation crosslinking cannot achieve a good balance between initial tack and holding power. Hydrosilylation crosslinking is performed under heating conditions; insufficient initial crosslinking density after coating leads to low initial tack; and insufficient uniformity of crosslinking density after heating crosslinking results in decreased holding power. Peel strength also decreased to some extent, indicating that the dual crosslinking network significantly contributes to the uniformity of mechanical properties. Therefore, the two-component packaging and step-by-step curing process solves the compatibility problem between thiols and platinum catalysts while retaining the advantage of rapid initial curing of thiols-olefins. The thiol-olefin click chemical crosslinking provided by mercaptopropyl-modified hydroxyl silicone oil is crucial for balancing initial tack and holding power.

[0068] Comparative Example 5: The present invention provides a comparative scheme, which differs from Example 2 in that it does not contain epoxy silane-phenyl silane cocondensation oligomer thickener; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0069]

[0070] Comparative Example 5, lacking the epoxy-silane-phenylsilane cocondensation oligomer tackifier, showed varying degrees of decrease in peel strength for low surface energy materials. The 180° peel strength of PTFE decreased from 5.8 N / cm in Example 2 to 4.8 N / cm, a reduction of 17.2%. This indicates the absence of the chemical anchoring of epoxy groups with trace amounts of polar groups on the surface of low surface energy materials, and the π-π conjugation compatibilization of phenyl groups with phenyl borate-modified PDMS, resulting in weakened interfacial adhesion. Peel strengths for PE and PP also decreased. Initial tack, holding tack, flame retardancy, and heat resistance were largely unaffected, indicating that the tackifier primarily affects interfacial adhesion rather than the crosslinking network and flame retardant and heat resistance properties. This comparative example demonstrates that the epoxy-silane-phenylsilane cocondensation oligomer tackifier is a key component for enhancing the interfacial adhesion of low surface energy materials.

[0071] Comparative Example 6: The present invention provides a comparative scheme, which differs from Example 2 in that it does not contain a composite flame retardant; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0072]

[0073] Comparative Example 6, which does not contain the composite flame retardant, exhibits peel strength, initial tack, and holding power similar to Example 2. However, its limiting oxygen index (LOI) drops sharply from 32.5% in Example 2 to 22.5%, indicating a lack of flame retardancy. This demonstrates that the composite flame retardant is the core component imparting flame retardant properties to the pressure-sensitive adhesive. Regarding heat resistance, the peel strength retention rate after 200℃ / 72h decreased from 92.1% to 89.3%, a small but still impactful decrease, indicating that the char layer formed by the phosphazene flame retardant provides some protection to the substrate when heated. This comparative example demonstrates that the composite flame retardant is a key component imparting flame retardant properties to silicone pressure-sensitive adhesives and also plays a supporting role in improving heat resistance.

[0074] Comparative Example 7: The present invention provides a comparative scheme: the difference from Example 2 is that the composite flame retardant does not use the phenyl silicone oil pre-dissolution composite method, but instead directly adds hexaphenoxycyclotriphosphazene solid powder to the adhesive solution; the remaining raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0075]

[0076] Comparative Example 7 directly added hexaphenoxycyclotriphosphazene solid powder to the adhesive solution instead of using a pre-dissolved phenyl silicone oil composite method. The limiting oxygen index decreased from 32.5% in Example 2 to 29.5%, indicating that the phosphazene solid powder was unevenly dispersed in the adhesive solution, and partial agglomeration led to a decrease in flame retardant efficiency; the initial tack decreased from 12N to 10N, and the holding power decreased from 96h to 72h, indicating that the agglomeration of phosphazene powder formed defect points in the cross-linking network, affecting the uniformity of mechanical properties; the peel strength also decreased to varying degrees, indicating that the agglomerated phosphazene particles formed weak areas at the interface, reducing adhesion; the heat resistance decreased from 92.1% to 86.8%, indicating that the unevenly dispersed phosphazene could not form a continuous and effective char layer protection. This comparative example demonstrates that the composite flame retardant preparation method defined in this invention (hexaphenoxycyclotriphosphazene and phenyl silicone oil pre-dissolved composite) is the key process to ensure uniform dispersion of phosphazene in the organosilicon system and fully exert its flame retardant and auxiliary heat resistance effects. Directly adding solid powder cannot achieve the same effect.

[0077] Comparative Example 8: The present invention provides a comparative scheme: the difference from Example 2 is that the composite crosslinking agent uses only hydrogen-containing silicone oil (without methyl hydrogen-containing MQ silicone resin), and the amount is the same as the total amount of composite crosslinking agent in Example 2; the other raw material ratios, preparation methods of each component, and preparation process parameters are completely consistent with Example 2.

[0078]

[0079] Comparative Example 8's composite crosslinking agent used only hydrogen-containing silicone oil (without methyl hydrogen-containing MQ silicone resin), lacking rigid crosslinking points. Initial tack increased from 12N in Example 2 to 13N, indicating that the flexible crosslinking network is beneficial for initial tack; however, holding power plummeted from 96h to 52h, indicating that the cohesive strength of the network containing only flexible crosslinking points was insufficient to maintain long-term tack; heat resistance decreased from 92.1% to 85.6%, indicating that the lack of a rigid crosslinking network provided by methyl hydrogen-containing MQ silicone resin made the crosslinked structure more prone to thermal relaxation at high temperatures; peel strength also decreased to some extent. This comparative example demonstrates that the rigid crosslinking points provided by methyl hydrogen-containing MQ silicone resin in the composite crosslinking agent are crucial for ensuring cohesive strength, holding power, and heat resistance; the composite design combining the rigidity and flexibility of hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin is indispensable.

[0080] The comparison between Examples 1-4 and Comparative Examples 1-8 shows that the seven components—phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane, fluorosilicone block copolymer, mercaptopropyl modified hydroxyl silicone oil, composite crosslinking agent, epoxysilane-phenylsilane cocondensation oligomer tackifier, carborane modified hydroxyl silicone oil, and composite flame retardant—work together in a two-component packaging and step-by-step curing process, each playing a clear and irreplaceable role.

[0081] The data of each comparative example was compared with those of Example 2: Comparative Example 1, which removed phenylboronic acid ester modified PDMS, fluorosilicone block copolymer, carborane modified hydroxyl silicone oil, tackifier, composite flame retardant, and thiol-olefin crosslinking, showed a PTFE peel strength of only 1.2 N / cm and was not flame retardant, a significant difference; Comparative Example 2, lacking fluorosilicone block copolymer, saw a 27.6% decrease in PTFE peel strength; Comparative Example 3, lacking carborane modified hydroxyl silicone oil, experienced a 22.4% decrease in PTFE peel strength and a nearly 10 percentage point drop in heat resistance retention; Comparative Example 4, lacking mercaptopropyl modified hydroxyl silicone oil, ... The initial tack decreased from 12N to 8N and the holding power decreased from 96h to 60h, indicating that double crosslinking is indeed important for the balance between initial tack and holding power. The two-component packaging process of this invention ensures that the mercapto group does not poison the platinum catalyst. Comparative Example 5 lacked a tackifier, resulting in a 17.2% decrease in PTFE peel strength. Comparative Example 6 lacked a composite flame retardant, causing the limiting oxygen index to drop directly from 32.5% to 22.5%. Comparative Example 7 directly added phosphazene powder instead of dissolving it with phenyl silicone oil first, resulting in a deterioration in both flame retardancy and mechanical properties. Comparative Example 8 used only hydrogen-containing silicone oil as the crosslinking agent, resulting in a decrease in holding power from 96h to 52h.

[0082] In summary, this invention addresses the shortcomings of existing technologies from five aspects: the dynamic bonds of phenylboronic acid esters provide interfacial adaptability; fluorosilicone block copolymers construct surface energy gradients to improve wettability; carboranes enhance the interfacial affinity and heat resistance of fluorinated materials; a two-component packaging and step-by-step curing process achieves dual crosslinking of thiols-olefins / hydrosilylation while avoiding thiols poisoning platinum catalysts; and a hexaphenoxycyclotriphosphazene / phenyl silicone oil composite flame-retardant system imparts flame retardancy. These five aspects work together to achieve reliable adhesion of the pressure-sensitive adhesive on low surface energy materials with a surface energy ≤30mN / m, while simultaneously balancing initial tack and holding power, heat resistance, and flame retardancy.

[0083] To further illustrate the beneficial technical effects of the various embodiments of the present invention, relevant performance tests were conducted on Embodiments 1-4 and Comparative Examples 1-8; The testing method is as follows: 1. 180° Peel Strength Test: Apply silicone pressure-sensitive tape to the surface of a low surface energy material (PTFE, PE, PP), and peel it 180° at a speed of 300 mm / min at 25°C. Record the peel force and calculate the peel strength.

[0084] 2. Initial tack test: Using the steel ball method, a steel ball is rolled down an inclined plane at a 30° angle, and the largest steel ball number that can be adhered to the tape surface is recorded. The initial tack is then calculated.

[0085] 3. Holding power test: A 25mm×25mm tape is attached to a stainless steel plate, a 1kg weight is suspended, and the time it takes for the tape to detach is recorded at 25℃.

[0086] 4. Limiting oxygen index test: The oxygen index is measured using an oxygen index meter according to GB / T 2406.2-2009 standard, and the lowest oxygen concentration that just sustains combustion in the oxygen-nitrogen mixture is recorded.

[0087] 5. Heat resistance test: The tape was adhered to the PTFE substrate and placed in a constant temperature oven at 200℃ for 72 hours. After being removed and cooled to 25℃, the peel strength at 180° was tested and compared with the peel strength of the unheat-aged sample to obtain the peel strength retention rate.

[0088] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific technical solutions or characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the technical solutions of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the implementation of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.

Claims

1. A silicone pressure-sensitive adhesive for bonding low surface area materials, characterized in that, Made from the following parts by weight of raw materials: The composition includes: 100 parts of phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane; 50-110 parts of long-chain alkyl-modified MQ silicone resin; 3-15 parts of fluorosilicone block copolymer; 1-8 parts of mercaptopropyl-modified hydroxyl silicone oil; 0.5-5 parts of composite crosslinking agent composed of hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin in a weight ratio of 1:0.3-1.5; 1-10 parts of epoxy silane-phenyl silane cocondensation oligomer tackifier; 0.5-5 parts of carborane-modified hydroxyl silicone oil; 3-15 parts of composite flame retardant composed of hexaphenoxycyclotriphosphazene and phenyl silicone oil in a weight ratio of 1:0.5-2; 0.1-3 parts of ultraviolet photoinitiator; 0.05-0.5 parts of platinum catalyst; and 100-300 parts of organic solvent. The ultraviolet photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxycyclohexylphenyl ketone, and 2,4,6-trimethylbenzoyl diphenylphosphine oxide; the platinum catalyst is selected from chloroplatinic acid-isopropanol complex or platinum-divinyltetramethyldisiloxane complex; and the organic solvent is selected from toluene, xylene, n-heptane, or mixtures thereof.

2. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, The number average molecular weight of the phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane is 10,000-80,000. Its molecular chain contains phenylboronic acid ester side groups, which are connected to the silicon atoms of the siloxane main chain through propylene groups. The phenylboronic acid ester side groups account for 1%-8% of the total molar number of siloxane segments, and the remaining siloxane segments are dimethylsiloxane segments. The preparation method of the phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane is as follows: hydroxyl-terminated polydimethylsiloxane containing methylhydrosiloxane links is mixed with allyl phenylboronic acid pinacol ester at a molar ratio of 1:1.05-1.2 of silane-hydrogen bonds to allyl groups. A platinum catalyst with a mass of 10-50 ppm of polydimethylsiloxane containing methylhydrosiloxane links is added. The mixture is stirred at 80-90℃ and 150-250 r / min for 2-4 h. Unreacted substances are removed by vacuum distillation at 110-120℃ for 1-2 h.

3. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, In the long-chain alkyl-modified MQ silicone resin, the organic groups of the M unit are composed of methyl, vinyl and long-chain alkyl with 8-18 carbon atoms, wherein the long-chain alkyl accounts for 5%-25% of the total molar number of the organic groups of the M unit, the vinyl accounts for 1%-10% of the total molar number of the organic groups of the M unit, and the remainder is methyl; the M / Q molar ratio of the MQ silicone resin is 0.6-1.

2. The preparation method of the long-chain alkyl modified MQ silicone resin is as follows: hexamethyldisiloxane, 1,3-divinyltetramethyldisiloxane and long-chain alkyl dimethylchlorosilane with 8-18 carbon atoms are mixed according to the designed ratio, tetraethyl orthosilicate is added as the source of Q units, toluene is used as solvent, deionized water is added dropwise at 0-5℃, the temperature is raised to 70-80℃ and refluxed for 4-6 hours, the aqueous layer is removed by separation, the organic layer is washed with deionized water until neutral, and the solvent is removed by vacuum distillation to obtain the product.

4. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, The fluorosilicone block copolymer is a hydroxyl-terminated polymethyltrifluoropropylsiloxane-polydimethylsiloxane-polymethyltrifluoropropylsiloxane triblock copolymer with a number average molecular weight of 5,000-30,000, wherein the degree of polymerization of the polymethyltrifluoropropylsiloxane block is 3-15 and the degree of polymerization of the polydimethylsiloxane block is 20-80. The preparation method of the fluorosilicone block copolymer is as follows: using a dihydroxyl-terminated polydimethylsiloxane with a number average molecular weight of 5000-15000 as a macromolecular initiator, adding methyltrifluoropropylcyclotrisiloxane monomer and alkali metal hydroxide catalyst, stirring at 120-140℃ and 200-300 r / min for 6-10 h, heating to 150-160℃ for 1-2 h to inactivate, and removing low molecular weight substances by vacuum distillation to obtain the copolymer.

5. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, The mercaptopropyl modified hydroxyl silicone oil has a mercapto content of 0.5%-3.0% and a number-average molecular weight of 1000-10000 for the hydroxyl silicone oil portion. The method for preparing the mercaptopropyl modified hydroxyl silicone oil is as follows: hydroxyl silicone oil containing methylhydrosiloxane linkages is mixed with an allyl mercapto compound at a molar ratio of 1:1.0-1.2 between silane-hydrogen bonds and allyl groups. A platinum catalyst with a mass of 10-30 ppm of the hydroxyl silicone oil containing methylhydrosiloxane linkages is added. The mixture is stirred at 70-85℃ and 150-250 r / min for 2-4 h. Unreacted substances are removed by vacuum distillation at 100-110℃ for 1-2 h. In the composite crosslinking agent, the hydrogen content of the hydrogen-containing silicone oil is 0.1%-1.6%, the hydrogen content of the methyl hydrogen-containing MQ silicone resin is 0.5%-1.6%, and the M / Q molar ratio is 0.6-1.0; The preparation method of the composite crosslinking agent is as follows: add hydrogen-containing silicone oil and methyl hydrogen-containing MQ silicone resin into a mixer at a weight ratio of 1:0.3-1.5, stir at 200-400 r / min for 30-60 minutes at room temperature, and mix evenly to obtain the final product.

6. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, The epoxy-silane-phenylsilane co-condensation oligomer tackifier is formed by partial co-hydrolysis condensation of epoxy-silane and phenylsilane coupling agent, with a weight ratio of epoxy-silane to phenylsilane coupling agent of 1:0.3-1 and a degree of polymerization of 3-6; the epoxy-silane is selected from one or more of γ-glycidyl etheroxypropyltrimethoxysilane and γ-glycidyl etheroxypropyltriethoxysilane; the phenylsilane coupling agent is selected from at least three of phenyltrimethoxysilane, diphenyldimethoxysilane, and methylphenyldimethoxysilane. The preparation method of the epoxy silane-phenyl silane cocondensation oligomer tackifier is as follows: epoxy silane and phenyl silane coupling agent are mixed at a weight ratio of 1:0.3-1, methanol or ethanol is added as a solvent, a strong acid cation exchange resin is added as a catalyst, and the mixture is stirred at 20-80℃ for 2-6 hours to carry out partial co-hydrolysis condensation. The strong acid cation exchange resin is removed by filtration, and the solvent and low volatile matter are removed by vacuum distillation to obtain the product. In the carborane-modified hydroxyl silicone oil, the carborane alkyl group is connected to the silicon atom of the siloxane backbone through propylene groups, the carborane alkyl group accounts for 1%-10% of the total molar number of siloxane segments, and the number average molecular weight of the hydroxyl silicone oil portion is 2000-15000. The preparation method of the carborane-modified hydroxyl silicone oil is as follows: First, o-carborane is reacted with allyl bromide under nitrogen protection and alkaline conditions to obtain allyl carborane. Then, allyl carborane is mixed with hydroxyl silicone oil containing methylhydrosiloxane links at a molar ratio of 1:1.0-1.1 between silane-hydrogen bonds and allyl groups. A platinum catalyst with a mass of 15-40 ppm of hydroxyl silicone oil containing methylhydrosiloxane links is added. The mixture is stirred at 80-95℃ and 150-250 r / min for 3-6 h. The mixture is then heated to 110-120℃ and distilled under reduced pressure for 1-2 h to remove unreacted substances, thus obtaining the product.

7. The silicone pressure-sensitive adhesive according to claim 1, characterized in that, In the composite flame retardant, hexaphenoxycyclotriphosphazene is an additive-type halogen-free phosphorus-nitrogen flame retardant, and the phenyl silicone oil is methylphenyl silicone oil with a number average molecular weight of 500-5000. The preparation method of the composite flame retardant is as follows: hexaphenoxycyclotriphosphazene and phenyl silicone oil are added to a mixer at a weight ratio of 1:0.5-2, and stirred at 300-500 r / min for 1-2 hours at 80-100℃ to completely dissolve the hexaphenoxycyclotriphosphazene in the phenyl silicone oil. The mixture is then cooled to room temperature to obtain the final product.

8. A silicone pressure-sensitive tape for bonding low surface area materials, characterized in that, The device comprises a substrate layer and an organosilicon pressure-sensitive adhesive layer coated on at least one surface of the substrate layer. The organosilicon pressure-sensitive adhesive layer is formed by coating, UV-initiated thiol-olefin crosslinking, and hydrosilylation crosslinking of the organosilicon pressure-sensitive adhesive according to any one of claims 1-7. The dry adhesive thickness of the organosilicon pressure-sensitive adhesive layer is 20-100 μm. The substrate layer is selected from one of polyimide film, polyester film, polytetrafluoroethylene film, or glass cloth. After curing, the organosilicon pressure-sensitive adhesive layer has a surface energy gradient structure, that is, the surface energy of the adhesive layer on the side closer to the substrate layer is higher than that on the side closer to the bonding surface.

9. A method for preparing an organosilicon pressure-sensitive adhesive for bonding low surface area materials as described in any one of claims 1-7, characterized in that, Includes the following steps: S1: Mix phenylboronic acid ester modified hydroxyl-terminated polydimethylsiloxane with an organic solvent and stir until completely dissolved to obtain the base solution; S2: Add long-chain alkyl-modified MQ silicone resin to the base liquid obtained in step S1, stir at 200-500 r / min at 60-90℃ for 2-4 hours, and cool to room temperature; S3: Add the fluorosilicone block copolymer to the mixture obtained in step S2, stir at 40-60°C for 1-2 hours, and then let it stand at room temperature for 0.5-1 hours to allow the fluorosilicone block copolymer to be fully dispersed; S4: Add mercaptopropyl modified hydroxyl silicone oil, epoxy silane-phenyl silane cocondensation oligomer tackifier, carborane modified hydroxyl silicone oil and composite flame retardant to the mixture obtained in step S3, and stir at 50-60℃ for 30-60 minutes. S5-1: Add a UV photoinitiator to the mixture obtained in step S4 and stir at 40-50℃ for 10-20 minutes to obtain component A; take another base liquid obtained in step S1, add a composite crosslinking agent and a platinum catalyst, and stir at 40-50℃ for 10-20 minutes to obtain component B. S5-2b: Mix component A and component B rapidly at a weight ratio of (8-12):1, stir for 2-5 minutes, and degas to obtain the silicone pressure-sensitive adhesive liquid. Components A and B are stored separately and mixed only before coating, so that the coexistence time between the mercapto-modified hydroxy silicone oil and the platinum catalyst before coating is controlled within 5 minutes.

10. A method for preparing an organosilicon pressure-sensitive tape with low surface area adhesion as described in claim 8, characterized in that, The organosilicon pressure-sensitive adhesive prepared according to claim 9 is coated onto the surface of the substrate layer. After irradiation with ultraviolet light, free radicals generated by the ultraviolet photoinitiator initiate thiol-olefin click chemical crosslinking between the thiol groups in the mercaptopropyl-modified hydroxyl silicone oil and the vinyl groups in the long-chain alkyl-modified MQ silicone resin. The ultraviolet light wavelength is 254-365 nm, and the irradiation dose is 500-2000 mJ / cm². 2 The mercapto-olefin click chemical crosslinking allows the mercapto groups in the mercaptopropyl modified hydroxy silicone oil to fully react with the vinyl groups, reducing the free mercapto content to below 0.01% and eliminating the risk of mercapto poisoning the platinum catalyst. Then, heating at 60-90℃ for 1-3 hours allows the Si-H bonds in the composite crosslinking agent to complete the hydrosilylation crosslinking with the vinyl groups in the long-chain alkyl modified MQ silicone resin under the action of the platinum catalyst, thus obtaining the organosilicon pressure-sensitive tape.