A photothermal controlled water collection / release material based on nano-intercalation

By introducing nano-intercalation technology and rare earth composites, a light-temperature regulated water collection/release material was constructed, which solved the bottlenecks of existing materials in terms of mechanical stability and photothermal efficiency. It achieved a synergistic improvement in the mechanical properties and hygroscopic properties of the material and light-temperature regulation function, and was applied to agricultural films to alleviate drought stress.

CN123107637APending Publication Date: 2026-11-17NANJING NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611155803.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-31
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing water collection/release materials have bottlenecks in terms of mechanical stability and photothermal efficiency, which limits their practical application as functional components of agricultural films and makes it impossible to achieve active water collection, intelligent water release and coordinated light and temperature control.

Method used

By employing nano-intercalation technology, layered silicates and natural polymers are formed into an intercalated composite network framework through hydrogen bonding, and rare earth complexes are introduced to achieve spectral conversion, thereby enhancing the light absorption capacity of carbon-based photothermal materials and constructing a light-temperature regulated water collection/release material.

Benefits of technology

It achieves a synergistic improvement in the mechanical and hygroscopic properties of materials, enhances photothermal efficiency, can actively capture water vapor at night and release moisture during the day, regulates the temperature and light environment inside the membrane, alleviates drought stress, reduces irrigation water use, and increases crop yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123107637A_ABST
    Figure CN123107637A_ABST
Patent Text Reader

Abstract

This invention discloses a photothermal-controlled water collection / release material based on nano-intercalation, belonging to the field of chemical materials technology. This invention utilizes natural polymer chains to expand layered silicate sheets, forming a nano-intercalated composite structure. This structure not only provides numerous hygroscopic sites for ethanolamine-based hygroscopic compounds, enabling rapid water adsorption, but also effectively improves the material's mechanical properties. Simultaneously, by introducing rare-earth complexes through the cation exchange characteristics of layered silicates, the material is endowed with spectral conversion capabilities, thereby enhancing the light absorption efficiency of carbon-based photothermal materials, thus achieving photothermal control and giving the material excellent water collection / release performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of chemical materials technology, specifically relating to a photothermal-controlled water collection / release material based on nano-intercalation. Background Technology

[0002] The mechanical properties of water-collecting / releasing materials are closely related to their framework structure. Currently, the framework matrix is ​​mainly divided into two categories: synthetic polymers and natural polymers. Synthetic polymers have high mechanical strength but poor biodegradability; natural polymers are widely available and degradable, but their mechanical properties decrease significantly after moisture absorption. Existing technologies mostly use interpenetrating polymer networks to improve their stability, but it is still difficult to achieve synergistic optimization of moisture absorption capacity and structural strength. Layered silicates have a nanosheet structure and can form intercalated or exfoliated organic-inorganic hybrid networks with natural polymers through hydrogen bonds, which can enhance mechanical strength and inhibit the leakage of moisture-absorbing components. However, research on polymer / layered silicate composites in atmospheric water collection is limited. Their interfacial interaction mechanisms, structural regulation rules, and moisture absorption performance optimization have not been systematically studied, resulting in a significant technological gap.

[0003] In terms of photothermal performance, carbon-based photothermal materials are a class of photothermal materials with great application potential due to their wide light absorption range. However, the solar spectrum energy is mainly concentrated in the visible and near-infrared regions, with ultraviolet light accounting for less than 5%. The direct absorption of ultraviolet light by carbon-based photothermal materials has limited impact on improving the overall photothermal efficiency. Although rare earth composites do not directly produce a photothermal effect, they can convert the low-proportion, high-energy ultraviolet light into visible light that carbon black can efficiently absorb through spectral conversion, achieving cascade utilization of the solar spectrum. This, in turn, creates a synergistic effect with carbon-based photothermal materials, further enhancing light absorption. Currently, rare earth composites have been successfully applied in agriculture, lighting, and other fields. However, research on introducing them as functional components into atmospheric water collection systems for photothermal regulation has not yet been reported, indicating significant research value and application potential.

[0004] The limitations of the aforementioned water-collecting / releasing materials in terms of mechanical stability and photothermal efficiency restrict their practical application as functional components of agricultural films. Agricultural production in arid and semi-arid regions faces challenges such as rapid soil moisture evaporation and large diurnal temperature variations. Traditional agricultural films only provide basic heat preservation and shading functions, failing to achieve active water collection, intelligent water release, and coordinated light and temperature regulation. Photothermal-regulated water-collecting / releasing materials based on nano-intercalation can be used as functional components in agricultural films in the future. They can actively capture water vapor from the air at night and release water to crop roots during the day through photothermal effects, while simultaneously regulating the temperature and light environment inside the film. This effectively alleviates drought stress, reduces irrigation water usage, and increases crop yield, demonstrating broad application prospects. Summary of the Invention

[0005] The purpose of this invention is to provide a photothermal-controlled water collection / release material based on nano-intercalation, which is prepared using the following steps: Step 1: Dissolve the basic hygroscopic compound in ethanol, add ethanolamine and stir until homogeneous, dry to obtain ethanolamine basic hygroscopic compound, then dissolve it in deionized water to prepare an ethanolamine basic hygroscopic compound solution. The basic hygroscopic compound is lithium chloride (LiCl), magnesium chloride (MgCl2), or cobalt chloride (CoCl2). Step 2: Mix the dispersant with deionized water evenly, add the carbon-based photothermal material, and grind to obtain a carbon-based photothermal material dispersion; The dispersant is argyne diol (AG), alkylphenol polyoxyethylene ether (APEO), or fatty alcohol polyoxyethylene ether (AEO). The carbon-based photothermal material is carbon nanotube (CNT), carbon black (CB), or activated carbon (AC). Step 3: Mix europium ions, organic ligands, organosilicon surfactants, and solvents and heat to react. Wash, dry, and pulverize the resulting product to obtain a rare earth complex. The europium ions are provided by trivalent europium nitrate or hydrochloride; the organic ligand is triphenylphosphine oxide (TPPO), benzoyltrifluoroacetone (BTA), or dibenzoylmethane (DBM); the organosilicon surfactant is 3-triethoxysilylpropyldimethyldodecylammonium chloride, 3-triethoxysilylpropyldimethylhexadecylammonium chloride, or 3-trimethoxysilylpropyldimethyloctadecylammonium chloride; the solvent is methanol, ethanol, or toluene. Step 4: Mix the natural polymer solution, layered silicate solution, carbon-based photothermal material dispersion, rare earth complex solution, and ethanolamine salt-based hygroscopic compound solution, heat and stir, let stand, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. The natural polymer is guar gum (GG), carboxymethyl cellulose (CMC), hydroxypropyl methyl cellulose (HPMC), carboxymethyl chitosan (CS), or sodium alginate (SA). The layered silicate is montmorillonite (MMT), talc (T), or mica (M).

[0006] Further, in step one, the ratio of the basic hygroscopic compound, ethanol, and ethanolamine is 1-7 g: 10-25 mL: 0.1-0.5 mL; the stirring time is 0.3-1.5 h; and the drying temperature is 70-85 ℃.

[0007] Furthermore, in step two, the ratio of the dispersant, deionized water, and carbon-based photothermal material is 3-20 g: 30-110 g: 3-22 g; the grinding time is 5-13 h.

[0008] Furthermore, in step three, the molar ratio of europium ions, organic ligands, organosilicon surfactants, and solvents is 1-4 mol: 2-5 mol: 3-6 mol: 2-10 mol; the heating temperature is 50-250 ℃, and the stirring time is 3-8 h.

[0009] Furthermore, in step four, the ratio of the amounts of the natural polymer solution, layered silicate solution, carbon-based photothermal material dispersion, rare earth complex solution, and ethanolamine salt-based hygroscopic compound solution is 5-15 mL: 2-7 mL: 0.01-0.15 g: 1-3 mL: 1-8 mL.

[0010] Further, in step four, the concentration of the natural polymer solution is 1.0-4.0 wt%, the concentration of the layered silicate solution is 1.0-3.0 wt%, the concentration of the carbon-based photothermal material dispersion is 5.0-10.0 wt%, the concentration of the rare earth composite solution is 2.0-6.0 wt%, and the concentration of the ethanolamine salt-based hygroscopic compound solution is 3.0-6.0 wt%; the solvent for all the above solutions is deionized water.

[0011] Furthermore, in step four, the temperature is 50-80 ℃, the stirring time is 2-6 h, and the standing time is 1-2 h.

[0012] In this invention, layered silicates can form hydrogen bonds with hydroxyl groups on natural polymer chains, effectively expanding their stacked layered structure to form a nano-intercalated composite network framework. This framework not only restricts the free movement of polymer chains and provides rigid support, improving the material's mechanical properties, but also retains abundant network pores, providing stable loading sites for salts and ensuring their uniform distribution within the network structure, thus laying the foundation for the material's excellent hygroscopic properties. To fully utilize the solar spectrum, rare earth composites are further introduced to endow the material with spectral conversion capabilities, enhancing the light absorption capacity of the carbon-based photothermal material, achieving photothermal regulation, and ultimately achieving the goal of efficient water collection / release.

[0013] Beneficial effects: Compared with the prior art, the present invention has the following advantages: (1) This invention is the first to use natural polymers to intercalate and modify layered silicates to construct a nano-intercalated composite network framework. Among them, the layered silicate sheets serve as a rigid framework to provide mechanical support for the material, while the natural polymer chains intercalated between the sheets maintain the integrity of the network structure and provide stable loading sites for salts, thereby achieving a synergistic improvement in the mechanical strength and moisture absorption properties of the material.

[0014] (2) This invention introduces rare earth composites for the first time, realizing the efficient utilization of the solar spectrum. The rare earth composites can convert ultraviolet light in sunlight into visible light, which is then efficiently absorbed by carbon-based photothermal materials and converted into heat energy, significantly improving the overall light absorption capacity of the materials.

[0015] (3) The method for synthesizing water collection / release materials prepared by the present invention is simple to operate and easy to scale up for production. Attached Figure Description

[0016] Figure 1 Scanning electron microscope (SEM) image of GG-MMT / E-LiCl / CB / GX.

[0017] Figure 2 The following are the Fourier Transform Infrared (FTIR) spectra of MMT, GG, GX, E-LiCl, and CB.

[0018] Figure 3 The infrared spectra (FTIR) of GG-MMT / E-LiCl / CB and GG-MMT / E-LiCl / CB / GX are shown.

[0019] Figure 4 The X-ray diffraction pattern (XRD) of MMT.

[0020] Figure 5 X-ray diffraction (XRD) patterns of GG-MMT, GG-MMT / E-LiCl / CB, and GG-MMT / E-LiCl / CB / GX.

[0021] Figure 6 Tensile stress-strain curves for GG-MMT / E-LiCl / CB / GX.

[0022] Figure 7 The moisture absorption rate of GG-MMT / E-LiCl / CB / GX under the conditions of 25 °C, 30% RH, 50% RH, 70% RH and 90% RH.

[0023] Figure 8 This is the emission spectrum of GX.

[0024] Figure 9 The emission spectrum of GG-MMT / E-LiCl / CB / GX is shown.

[0025] Figure 10 The surface temperatures of GG-MMT / E-LiCl and GG-MMT / E-LiCl / CB at 1.0 sun, and the surface temperatures of GG-MMT / E-LiCl / CB / GX at 0.5 sun, 1.0 sun, and 1.5 sun.

[0026] Figure 11 The percentage of residual water in GG-MMT / E-LiCl and GG-MMT / E-LiCl / CB at 1.0 sun, and the percentage of residual water in GG-MMT / E-LiCl / CB / GX at 0.5 sun, 1.0 sun, and 1.5 sun. Detailed Implementation

[0027] The preferred embodiments of the present invention will now be described in detail with reference to specific examples. It should be understood that the following examples are given for illustrative purposes only and are not intended to limit the scope of the invention. Those skilled in the art can make various modifications and substitutions to the present invention without departing from its spirit and essence.

[0028] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.

[0029] Unless otherwise specified, all materials and reagents used in the following examples are commercially available. Example 1

[0030] Step 1: Dissolve 3.0 g of LiCl in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-LiCl; then dissolve 0.35 g of E-LiCl in 5 mL of deionized water to prepare a 7.0 wt% E-LiCl solution.

[0031] Step 2: Mix 10 g of AG with 80 g of deionized water thoroughly, add 10 g of CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0032] Step 3: 1 mol europium chloride, 2.1 mol BTA, 6 mol 3-triethoxysilylpropyldimethyldodecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain rare earth complex GX. Step 4: Mix 10 mL GG solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (10.0 wt%), 2 mL GX solution (3.0 wt%), and 5 mL E-LiCl solution (7.0 wt%), stir at 60 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a photothermal-controlled water collection / release material (GG-MMT / E-LiCl / CB / GX) with a nano-intercalation structure.

[0033] like Figure 1As shown, GG-MMT / E-LiCl / CB / GX exhibits a rich and interconnected porous network structure. This is because, under the influence of GG molecules, the originally stacked MMT sheets are successfully expanded, and the guar gum molecular chains connect the MMT sheets to each other through hydrogen bonds formed with the hydroxyl groups on the surface of the MMT sheets, thereby constructing a network structure with excellent pore connectivity.

[0034] like Figure 2 As shown, in the FTIR spectra of MMT and GX, the region is located at 1036-1096 cm⁻¹. -1 The absorption peak at [cm] is attributed to the stretching vibration of Si-O-Si, a typical characteristic peak of MMT as a layered silicate mineral. In the FTIR spectra of GG and CB, it is located at 3486-3487 cm⁻¹. -1 The absorption peak at [value missing] is attributed to the stretching vibration of OH, indicating the presence of hydroxyl groups in GG and CB. In the FTIR spectrum of E-LiCl, [value missing] is located at 1060 cm⁻¹. -1 The absorption peak at 995 cm⁻¹ is attributed to the stretching vibration of CO; -1 The absorption peak at that location is attributed to the stretching vibration of CN. For example... Figure 3 As shown, in the FTIR spectra of GG-MMT / E-LiCl / CB and GG-MMT / E-LiCl / CB / GX, the wavelength range is 10¹³–10⁹⁸ cm⁻¹. -1 The appearance of Si-O-Si stretching vibration absorption peaks at 993-995 cm⁻¹ confirms the successful introduction of MMT and GX; -1 The presence of characteristic peaks for CN stretching vibrations at this location confirms the introduction of E-LiCl. Furthermore, peaks located at 3434-3444 cm⁻¹... -1 The characteristic peak of the OH stretching vibration at the point of origin redshifted, indicating that the guar gum molecular chains formed hydrogen bonds with the hydroxyl groups on the surface of the MMT sheets.

[0035] like Figure 4 , 5 As shown, the d of MMT, GG-MMT, GG-MMT / E-LiCl / CB and GG-MMT / E-LiCl / CB / GX 001 The interlayer spacings were 1.283, 1.481, 1.426, and 1.431 nm, respectively. The interlayer spacing of GG-MMT increased by 0.198 nm compared to MMT, indicating that GG molecular chains inserted into the MMT sheets via hydrogen bonds and expanded the layered structure. The interlayer spacing of GG-MMT / E-LiCl / CB decreased by 0.055 nm compared to GG-MMT, which may be due to the Li... + Enhanced interlayer electrostatic attraction or CB filling of interlayer voids; no significant change in interlayer spacing after GX introduction.

[0036] like Figure 6 As shown, the tensile strength of GG-MMT / E-LiCl / CB / GX increased to 0.25 MPa, and the elongation at break was 75.58%.

[0037] like Figure 7 As shown, the moisture absorption rates of GG-MMT / E-LiCl / CB / GX at 25 ℃ and relative humidity of 30%, 50%, 70% and 90% are 0.54 g / g, 1.12 g / g, 1.75 g / g and 2.48 g / g, respectively, demonstrating excellent moisture absorption capacity.

[0038] like Figure 8 , 9 As shown, GG-MMT / E-LiCl / CB / GX exhibits fluorescence emission characteristics dominated by red light and supplemented by blue light at four excitation wavelengths of 260, 300, 320 and 360 nm. The fluorescence behavior is highly consistent with the characteristic spectrum of GX, indicating that the introduction of GX enables the composite material to have the ability to efficiently convert ultraviolet light into blue and red light, with red light emission being dominant.

[0039] like Figure 10 As shown, under a solar irradiance of 1.0, the surface temperatures of GG-MMT / E-LiCl, GG-MMT / E-LiCl / CB, and GG-MMT / E-LiCl / CB / GX exhibit significant differences. GG-MMT / E-LiCl shows a relatively slow heating rate, reaching an equilibrium temperature of 54.6 °C after 100 minutes. The GG-MMT / E-LiCl / CB with introduced CB shows a significantly faster heating rate, reaching a surface temperature of 58.3 °C in just 5 minutes, and eventually stabilizing at 80.1 °C. In contrast, GG-MMT / E-LiCl / CB / GX rapidly rises to 65 °C within 5 minutes, finally reaching an equilibrium temperature of 86 °C after 100 minutes. Furthermore, the surface temperature of GG-MMT / E-LiCl / CB / GX increases gradually with increasing solar irradiance. When the light intensity was 0.5 sun, 1.0 sun, and 1.5 sun, the surface temperature of GG-MMT / E-LiCl / CB / GX stabilized at 62.8 ℃, 86 ℃, and 108 ℃ after 100 minutes, respectively.

[0040] like Figure 11As shown, under a light intensity of 1.0 sun, the residual water percentages of GG-MMT / E-LiCl, GG-MMT / E-LiCl / CB, and GG-MMT / E-LiCl / CB / GX after 100 minutes of irradiation were 31.50%, 12.00%, and 8.56%, respectively. This indicates a synergistic effect between CB and GX, enhancing the water release performance of GG-MMT / E-LiCl / CB / GX. Furthermore, when the light intensities were 0.5 sun, 1.0 sun, and 1.5 sun, the residual water content of GG-MMT / E-LiCl / CB / GX decreased to 21.60%, 8.56%, and 5.65% after 100 minutes, respectively. This suggests that the water release of GG-MMT / E-LiCl / CB / GX gradually increases with increasing light intensity. Example 2

[0041] Step 1: Dissolve 3.0 g of MgCl2 in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain MgCl2; then dissolve 0.35 g of E-MgCl2 in 5 mL of deionized water to prepare a 7.0 wt% E-MgCl2 solution.

[0042] Step 2: Mix 12 g of AG with 90 g of deionized water thoroughly, add 10 g of CB, and grind for 10 h to obtain an 8.9 wt% CB dispersion.

[0043] Step 3: 1 mol europium chloride, 2.1 mol TPPO, 6 mol 3-triethoxysilylpropyldimethylhexadecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain the rare earth complex MX.

[0044] Step 4: Mix 10 mL CS solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (8.9 wt%), 2 mL MX solution (3.0 wt%) and 5 mL E-MgCl2 solution (7.0 wt%), stir at 70 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. Example 3

[0045] Step 1: Dissolve 4.0 g of CoCl2 in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-CoCl2; then dissolve 0.35 g of E-CoCl2 in 5 mL of deionized water to prepare a 7.0 wt% E-CoCl2 solution.

[0046] Step 2: Mix 10 g APEO with 90 g deionized water thoroughly, add 10 g CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0047] Step 3: 1 mol europium chloride, 2.1 mol DBM, 6 mol 3-trimethoxysilylpropyldimethyloctadecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain the rare earth complex KX.

[0048] Step 4: Mix 10 mL CS solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (10.0 wt%), 2 mL KX solution (3.0 wt%) and 5 mL E-CoCl2 solution (7.0 wt%), stir at 70 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. Example 4

[0049] Step 1: Dissolve 4.0 g of CoCl2 in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-CoCl2; then dissolve 0.35 g of E-CoCl2 in 5 mL of deionized water to prepare a 7.0 wt% E-CoCl2 solution.

[0050] Step 2: Mix 10 g of AG with 90 g of deionized water thoroughly, add 10 g of CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0051] Step 3: 1 mol europium chloride, 2.1 mol BTA, 6 mol 3-trimethoxysilylpropyldimethyloctadecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain the rare earth complex GX.

[0052] Step 4: Mix 10 mL SA solution (2.0 wt%), 6 mL mica solution (3.0 wt%), 0.04 g CB dispersion (10.0 wt%), 3 mL GX solution (3.0 wt%) and 5 mL E-CoCl2 solution (7.0 wt%), stir at 70 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. Example 5

[0053] Step 1: Dissolve 3.0 g of LiCl in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-LiCl; then dissolve 0.35 g of E-LiCl in 5 mL of deionized water to prepare a 7.0 wt% E-LiCl solution.

[0054] Step 2: Mix 10 g of AG with 80 g of deionized water thoroughly, add 10 g of CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0055] Step 3: 1 mol europium chloride, 2.1 mol BTA, 6 mol 3-triethoxysilylpropyldimethyldodecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain rare earth complex GX. Step 4: Mix 10 mL CMC solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (10.0 wt%), 2 mL GX solution (3.0 wt%) and 5 mL E-LiCl solution (7.0 wt%), stir at 60 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. Example 6

[0056] Step 1: Dissolve 4.0 g of CoCl2 in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-CoCl2; then dissolve 0.35 g of E-CoCl2 in 5 mL of deionized water to prepare a 7.0 wt% E-CoCl2 solution.

[0057] Step 2: Mix 10 g APEO with 90 g deionized water thoroughly, add 10 g CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0058] Step 3: 1 mol europium chloride, 2.1 mol DBM, 6 mol 3-trimethoxysilylpropyldimethyloctadecylammonium chloride, and 7 mol ethanol were reacted at 180 °C for 6 hours. The resulting product was washed, dried, and pulverized to obtain the rare earth complex KX.

[0059] Step 4: Mix 10 mL HPMC solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (10.0 wt%), 2 mL KX solution (3.0 wt%) and 5 mL E-CoCl2 solution (7.0 wt%), stir at 70 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. Comparative Example 1

[0060] The difference between this embodiment and Embodiment 1 is that GX was not added.

[0061] Step 1: Dissolve 3.0 g of LiCl in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-LiCl; then dissolve 0.35 g of E-LiCl in 5 mL of deionized water to prepare a 7.0 wt% E-LiCl solution.

[0062] Step 2: Mix 10 g of AG with 80 g of deionized water thoroughly, add 10 g of CB, and grind for 10 h to obtain a 10.0 wt% CB dispersion.

[0063] Step 3: Mix 10 mL GG solution (2.0 wt%), 5 mL MMT solution (2.0 wt%), 0.025 g CB dispersion (10.0 wt%) and 5 mL E-LiCl solution (7.0 wt%), stir at 60 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain a water-collecting / water-releasing material (GG-MMT / E-LiCl / CB) with a nano-intercalated structure. Comparative Example 2

[0064] The difference between this embodiment and Embodiment 1 is that GX and CB are not added.

[0065] Step 1: Dissolve 3.0 g of LiCl in 20 mL of ethanol, add 0.2 mL of ethanolamine and stir for 30 min; dry at 80 °C to obtain E-LiCl; then dissolve 0.35 g of E-LiCl in 5 mL of deionized water to prepare a 7.0 wt% E-LiCl solution.

[0066] Step 2: Mix 10 mL of GG solution (2.0 wt%), 5 mL of MMT solution (2.0 wt%), and 5 mL of E-LiCl solution (7.0 wt%), stir at 60 ℃ for 4 h, let stand for 1 h, and freeze dry to obtain the water collecting material (GG-MMT / E-LiCl). Comparative Example 3

[0067] The difference between this embodiment and Embodiment 1 is that E-LiCl, GX, and CB were not added.

[0068] 10 mL of GG solution (2.0 wt%) and 5 mL of MMT solution (2.0 wt%) were mixed, stirred at 60 °C for 4 h, allowed to stand for 1 h, and then freeze-dried to obtain the water-collecting material (GG-MMT).

[0069] The above comparative experiments show that: (1) such as Figure 10 As shown, under a sun illumination intensity of 1.0, there are significant differences in the surface temperatures of GG-MMT / E-LiCl, GG-MMT / E-LiCl / CB, and GG-MMT / E-LiCl / CB / GX. GG-MMT / E-LiCl exhibits a relatively slow heating rate, reaching an equilibrium temperature of 54.6 ℃ after 100 minutes. GG-MMT / E-LiCl / CB, with the addition of CB, shows a significantly faster heating rate, reaching a surface temperature of 58.3 ℃ in just 5 minutes, and eventually stabilizing at 80.1 ℃. In contrast, GG-CNF / E-LiCl / CB / GX rapidly rises to 65 ℃ within 5 minutes and finally reaches an equilibrium temperature of 86 ℃ after 100 minutes. Its heating rate and equilibrium temperature are both higher than those of GG-MMT / E-LiCl and GG-MMT / E-LiCl / CB. This is mainly attributed to the fact that after GX converts ultraviolet light into blue and red light, these specific wavelengths of light can complement and superimpose with the visible light wavelengths absorbed by CB, allowing the material to capture more light energy that would otherwise be underutilized. This captured light is ultimately converted into heat energy, thereby driving a significant increase in the surface temperature of the material.

[0070] (2) For example Figure 11 As shown, under a sun intensity of 1.0, the residual water percentages of GG-MMT / E-LiCl, GG-MMT / E-LiCl / CB, and GG-MMT / E-LiCl / CB / GX after 100 minutes of irradiation were 31.50%, 12.00%, and 8.56%, respectively. This indicates that the synergistic effect between CB and GX enhances the water release performance of GG-MMT / E-LiCl / CB / GX.

[0071] The above are merely specific embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, various modifications and substitutions can be made to the present invention without departing from its spirit and intent, and all such modifications and substitutions fall within the scope of protection of the present invention.

Claims

1. A photothermal-controlled water collection / release material based on nano-intercalation, characterized in that, It is prepared by the following steps: Step 1: Dissolve the basic hygroscopic compound in ethanol, add ethanolamine and stir until homogeneous, dry to obtain ethanolamine basic hygroscopic compound, then dissolve it in deionized water to prepare an ethanolamine basic hygroscopic compound solution. The basic hygroscopic compound is lithium chloride, magnesium chloride, or cobalt chloride; Step 2: Mix the dispersant with deionized water evenly, add the carbon-based photothermal material, and grind to obtain a carbon-based photothermal material dispersion; The dispersant is acetylenic diol, alkylphenol polyoxyethylene ether, or fatty alcohol polyoxyethylene ether; The carbon-based photothermal material is carbon nanotubes, carbon black, or activated carbon. Step 3: Mix europium ions, organic ligands, organosilicon surfactants, and solvents and heat to react. Wash, dry, and pulverize the resulting product to obtain a rare earth complex. The europium ions are provided by trivalent europium nitrate or hydrochloride; the organic ligand is triphenylphosphine oxide, benzoyltrifluoroacetone, or dibenzoylmethane; the organosilicon surfactant is 3-triethoxysilylpropyldimethyldodecylammonium chloride, 3-triethoxysilylpropyldimethylhexadecylammonium chloride, or 3-trimethoxysilylpropyldimethyloctadecylammonium chloride; the solvent is methanol, ethanol, or toluene. Step 4: Mix the natural polymer solution, layered silicate solution, carbon-based photothermal material dispersion, rare earth complex solution, and ethanolamine salt-based hygroscopic compound solution, heat and stir, let stand, and freeze dry to obtain a light-temperature regulated water collection / release material with a nano-intercalation structure. The natural polymer is guar gum, carboxymethyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl chitosan, or sodium alginate; The layered silicate is montmorillonite, talc, or mica.

2. The photothermal controlled water collection / release material based on nano-intercalation according to claim 1, characterized in that, In step one, the ratio of the basic hygroscopic compound, ethanol, and ethanolamine is 1-7 g: 10-25 mL: 0.1-0.5 mL; the stirring time is 0.3-1.5 h; and the drying temperature is 70-85 ℃.

3. The photothermal controlled water collection / release material based on nano-intercalation according to claim 1, characterized in that, In step two, the ratio of the dispersant, deionized water and carbon-based photothermal material is 3-20 g: 30-110 g: 3-22 g; the grinding time is 5-13 h.

4. The photothermal controlled water collection / release material based on nano-intercalation according to claim 1, characterized in that, In step three, the molar ratio of europium ions, organic ligands, organosilicon surfactants, and solvents is 1-4 mol: 2-5 mol: 3-6 mol: 2-10 mol; the heating temperature is 50-250 ℃, and the stirring time is 3-8 h.

5. The photothermal controlled water collection / release material based on nano-intercalation according to claim 1, characterized in that, In step four, the ratio of the amounts of the natural polymer solution, layered silicate solution, carbon-based photothermal material dispersion, rare earth complex solution, and ethanolamine salt-based hygroscopic compound solution is 5-15 mL: 2-7 mL: 0.01-0.15 g: 1-3 mL: 1-8 mL.

6. The photothermal controlled water collection / release material based on nano-intercalation according to claim 5, characterized in that, In step four, the concentrations of the natural polymer solution are 1.0-4.0 wt%, the layered silicate solution is 1.0-3.0 wt%, the carbon-based photothermal material dispersion is 5.0-10.0 wt%, the rare earth composite solution is 2.0-6.0 wt%, and the ethanolamine salt-based hygroscopic compound solution is 3.0-6.0 wt%; all of the above solutions are in deionized water as the solvent.

7. The photothermal controlled water collection / release material based on nano-intercalation according to claim 1, characterized in that, In step four, the temperature is 50-80 ℃, the stirring time is 2-6 h, and the standing time is 1-2 h.