A heat treatment process to improve the microstructure and properties of high-strength non-oriented silicon steel

By precisely controlling the annealing temperature and atmosphere of high-strength non-oriented silicon steel, combined with pretreatment processes, a synergistic optimization of high strength and low iron loss was achieved, solving the problems of insufficient recrystallization and uncontrollable texture in traditional processes, and meeting the performance requirements of high-end equipment such as drive motors for new energy vehicles.

CN123108249APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611410599.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The annealing temperature control of traditional high-strength non-oriented silicon steel is vague, resulting in insufficient recrystallization or excessive grain growth, uncontrollable texture, poor coordination between pretreatment and annealing processes, and imbalance between magnetic and mechanical properties, making it difficult to meet the needs of high-end equipment such as drive motors for new energy vehicles.

Method used

The temperature is raised to 700-775℃ at a heating rate of 7.5-8.5℃/min, held for 1.5-2.5h, using a N2+H2 mixed atmosphere and real-time monitoring of the furnace temperature. After cooling to 300℃ in the furnace, it is allowed to cool naturally. Combined with vacuum induction furnace melting, multi-pass hot rolling and cold rolling processes, this ensures sufficient recrystallization, uniform grain size and favorable texture formation.

Benefits of technology

It achieves a recrystallization ratio of ≥98%, uniform grain size control at 12-18μm, a favorable texture {100}+{110} ratio of ≥22%, magnetic induction intensity B5000 ≥1.60T, low-frequency iron loss P1.5/50 ≤6.8W/kg, and yield strength of 480-550MPa, making it suitable for the high strength and low energy consumption requirements of high-end motors.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel, belonging to the field of heat treatment technology for electrical steel. The heat treatment process includes: a heating stage: heating to the target annealing temperature of 700-775℃ at a rate of 7.5-8.5℃ / min, maintaining a N2+H2 mixed atmosphere flow rate of 5.5-6.5L / min during the heating process; a holding stage: holding at the target temperature for 1.5-2.5 hours; and a cooling stage: after the holding stage, cooling in the furnace to 300℃ at a rate of 4.8-5.2℃ / min, then switching to an N2 atmosphere and naturally cooling to room temperature to avoid stress concentration due to excessively rapid cooling. The purpose of this invention is to achieve a microstructure characterized by "sufficient recrystallization, moderate grain size, and favorable texture enrichment," thereby achieving synergistic optimization of strong magnetic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of heat treatment technology for electrical steel, and particularly relates to a heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel. It is applicable to components with stringent requirements for magnetic and mechanical properties, such as drive motors for new energy vehicles, rotors for high-speed motors, and cores for high-efficiency transformers, achieving a precise match between high strength, low iron loss, and high magnetic induction intensity. Background Technology

[0002] High-strength non-oriented silicon steel is the core material for drive motors in new energy vehicles, and it must simultaneously meet three major requirements: high magnetic induction intensity (to ensure efficient energy conversion), low iron loss (to reduce energy consumption), and high strength (to resist high-speed centrifugal force). However, traditional processes have significant drawbacks: ambiguous control of annealing temperature leads to insufficient recrystallization (650-700℃) or excessive grain growth (>800℃); a single annealing atmosphere results in uncontrollable texture evolution, with a low proportion of favorable texture {100}+{110} and an excessively high proportion of unfavorable texture {111}; poor synergy between pretreatment (hot rolling, normalizing, cold rolling) and annealing processes leads to insufficient microstructure uniformity, ultimately causing an imbalance between magnetic and mechanical properties (e.g., high strength is accompanied by high iron loss, while low iron loss results in insufficient strength).

[0003] Current technologies lack an integrated optimization scheme for "pretreatment-annealing-atmosphere," making it difficult to precisely control the degree of recrystallization, grain size, and texture type, thus hindering the application of high-strength non-oriented silicon steel in high-end motors. Therefore, there is an urgent need to develop a heat treatment process with clearly defined process parameters and excellent synergistic strong magnetic properties. Summary of the Invention

[0004] The purpose of this invention is to provide a heat treatment process that improves the microstructure and properties of high-strength non-oriented silicon steel, thereby achieving excellent synergistic properties of strong magnetic properties.

[0005] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:

[0006] This invention discloses a heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel, comprising:

[0007] Heating stage: Increase the temperature at a rate of 7.5-8.5℃ / min to the target annealing temperature of 700-775℃, and maintain the N2+H2 mixed atmosphere flow rate of 5.5-6.5L / min during the heating process;

[0008] Heat preservation stage: Heat preservation at the target temperature for 1.5-2.5 hours to ensure complete recrystallization and promote the formation of favorable texture. During the heat preservation process, the furnace temperature is monitored in real time, and the fluctuation is ≤±1℃.

[0009] Cooling stage: After the heat preservation is completed, the furnace is cooled to 300°C at a rate of 4.8-5.2°C / min, and then switched to N2 atmosphere and allowed to cool naturally to room temperature to avoid stress concentration caused by excessive cooling.

[0010] Furthermore, specifically including:

[0011] Heating stage: Increase the temperature at a rate of 8℃ / min to the target annealing temperature of 700-775℃, and maintain the N2+H2 mixed atmosphere flow rate of 6L / min during the heating process;

[0012] Heat preservation stage: Heat preservation at the target temperature for 2 hours to ensure complete recrystallization and promote the formation of favorable texture. During the heat preservation process, the furnace temperature is monitored in real time, and the fluctuation is ≤±1℃.

[0013] Cooling stage: After the heat preservation is completed, the furnace is cooled to 300°C at a rate of 5°C / min, and then switched to N2 atmosphere and allowed to cool naturally to room temperature to avoid stress concentration caused by excessive cooling.

[0014] Furthermore, the composition of the high-strength non-oriented silicon steel by mass fraction is designed as follows: Si 2.8-3.2%, Mn 0.4-0.6%, Al 0.2-0.4%, P≤0.02%, S≤0.01%, C≤0.005%, with the remainder being Fe and unavoidable impurities.

[0015] Furthermore, it also includes smelting and billet preparation: smelting is carried out using a vacuum induction furnace with a vacuum degree ≤5×10⁻⁶. -3 Pa, cast into a 200mm×120mm×800mm billet, with a billet cooling rate of 10℃ / min to avoid component segregation.

[0016] Furthermore, it also includes: pretreatment processes:

[0017] (1) Hot rolling process

[0018] Heating and holding: The billet is placed in a walking beam furnace and heated to 1150℃ at a rate of 15℃ / min, and held for 3 hours to ensure that elements such as Si and Al are fully dissolved and the grains are homogenized.

[0019] Multi-pass hot rolling: The 200mm thick billet is rolled into a 30mm thick hot-rolled plate through 7 passes at an initial temperature of 1150℃. The reduction rates of each pass are 15%, 18%, 20%, 22%, 25%, 30%, and 35% respectively. The final rolling temperature is 900℃. High-pressure water descaling (water pressure 18MPa) is used during the hot rolling process to prevent oxide scale from being pressed in.

[0020] Cooling after hot rolling: air cool to 600℃, then stack cool to room temperature, controlling the cooling rate at 15℃ / min to avoid coarse microstructure;

[0021] (2) Normalization treatment

[0022] Normalizing process: Place a 30mm thick hot-rolled plate into a continuous annealing furnace, under N2 atmosphere protection, with a flow rate of 8L / min, heat to 950℃ at a rate of 12℃ / min, hold for 1h, refine the hot-rolled structure and reduce residual stress.

[0023] Cooling method: The furnace is cooled to 500℃ at a rate of 8℃ / min, and then air-cooled to room temperature. After normalization, the microstructure is ferrite + a small amount of pearlite, and the grain size is ≤20μm.

[0024] (3) Cold rolling process

[0025] Pickling pretreatment: The normalized plate is pickled with 15% hydrochloric acid solution at 60℃ for 30 minutes to remove the surface oxide layer, rinsed with water and dried.

[0026] Cold rolling implementation: A six-roll cold rolling mill is used to cold roll a 30mm thick normalized plate to a 9mm thick cold-rolled plate with a reduction rate of 70%. The rolling speed is 2.0m / s, and the reduction rate per pass is ≤25% to avoid excessive deformation that could lead to structural distortion. The residual stress after cold rolling is ≤200MPa.

[0027] Furthermore, this also includes preparations before annealing:

[0028] Surface cleaning: Wipe the surface oil stains of the cold-rolled sheet with alcohol, let it dry, and then put it into the annealing furnace. The spacing between the sheets should be ≥50mm to ensure uniform atmosphere flow.

[0029] Atmosphere replacement: A mixed atmosphere of 50% N2 + 50% H2 is introduced into the annealing furnace to replace the air in the furnace, so that the final oxygen content in the furnace is ≤50ppm.

[0030] Furthermore, the air inside the replacement furnace is replaced a total of 3 times, with each venting lasting 30 minutes.

[0031] This paper addresses the core pain points of traditional processes, such as insufficient recrystallization, inadequate texture optimization, and imbalance of strong magnetic properties, and proposes an integrated process of "co-optimized pretreatment + precise temperature-controlled annealing + atmosphere control".

[0032] This invention mainly provides a uniform deformation structure for annealing through standardized pretreatment (hot rolling-normalizing-cold rolling), precisely controls the annealing temperature (700-775℃) to regulate recrystallization and grain growth, and uses a 50%N2+50%H2 mixed atmosphere to suppress oxidation and optimize texture evolution, ultimately achieving a microstructure state of "sufficient recrystallization, moderate grain size, and favorable texture enrichment", thus achieving synergistic optimization of strong magnetic properties.

[0033] Compared with the prior art, the beneficial technical effects of the present invention are as follows:

[0034] 1. Thoroughly optimized structure: recrystallization ratio ≥98%, no residual deformed structure, grain size uniformly controlled within 12-18μm (the optimal range for matching magnetic properties and strength), and the structure uniformity is improved by 35% compared with traditional processes.

[0035] 2. Precise texture control: the proportion of favorable texture {100}+{110} is ≥22%, the texture factor is ≥1.0, and the proportion of unfavorable texture {111} is ≤10%, laying the foundation for high magnetic induction intensity.

[0036] 3. Excellent synergistic effect of strong magnetic properties: magnetic induction intensity B 5000 ≥1.60T, low-frequency iron loss P 1.5 / 50 ≤6.8W / kg, medium and high frequency iron loss P 1.0 / 400 ≤42W / kg; yield strength 480-550MPa, tensile strength 580-630MPa, meeting the dual requirements of "high strength + low energy consumption" for high-end motors.

[0037] 4. Standardized process: Pretreatment and annealing parameters are clearly quantified, and the performance deviation of different batches of products is ≤±3%, which is suitable for industrial mass production.

[0038] 5. Wide adaptability: Compatible with high-strength non-oriented silicon steel with Si 2.8-3.2wt%, the annealing temperature can be flexibly adjusted according to the application scenario (motor rotor / core, transformer) to achieve targeted performance control. Detailed Implementation

[0039] A heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel includes the following specific steps:

[0040] 1. Raw material pretreatment and composition design:

[0041] Composition design (wt%): Si 2.8-3.2%, Mn 0.4-0.6%, Al 0.2-0.4%, P≤0.02%, S≤0.01%, C≤0.005%, Fe balance. Specifically: Si (2.8-3.2%) ensures magnetic permeability and resistivity, reducing iron loss; Mn (0.4-0.6%) improves hardenability and cold rolling workability; Al (0.2-0.4%) refines grains and inhibits the formation of undesirable textures.

[0042] Melting and billet preparation: Melting was carried out in a vacuum induction furnace (vacuum degree ≤ 5 × 10⁻⁶). -3 The casting is carried out in 200mm×120mm×800mm billets, with a cooling rate of 10℃ / min to avoid component segregation.

[0043] 2. Pretreatment process:

[0044] (1) Hot rolling process

[0045] Heating and holding: The billet is placed in a walking beam furnace and heated to 1150℃ at a rate of 15℃ / min. It is then held for 3 hours to ensure that elements such as Si and Al are fully dissolved and the grains are homogenized (initial grain size ≤50μm).

[0046] Multi-pass hot rolling: The 200mm thick billet is rolled into a 30mm thick hot-rolled plate through 7 passes at an initial temperature of 1150℃. The reduction rates of each pass are 15%, 18%, 20%, 22%, 25%, 30%, and 35% respectively. The final rolling temperature is 900℃. High-pressure water descaling (18MPa) is used during the hot rolling process to prevent oxide scale from being pressed in.

[0047] Cooling after hot rolling: air-cool to 600℃, then stack-cool to room temperature, controlling the cooling rate at 15℃ / min to avoid coarse microstructure.

[0048] (2) Normalization treatment

[0049] Normalizing process: Place a 30mm thick hot-rolled plate into a continuous annealing furnace, protect it with N2 atmosphere (flow rate 8L / min), heat it to 950℃ at a rate of 12℃ / min, hold it for 1 hour to refine the hot-rolled structure and reduce residual stress.

[0050] Cooling method: The furnace is cooled to 500℃ at a rate of 8℃ / min, followed by air cooling to room temperature. After normalization, the microstructure is ferrite with a small amount of pearlite and the grain size is ≤20μm.

[0051] (3) Cold rolling process

[0052] Pickling pretreatment: The normalized plate is pickled with 15% hydrochloric acid solution (temperature 60℃, time 30min) to remove the surface oxide layer, rinsed with water and dried.

[0053] Cold rolling implementation: A six-roll cold rolling mill is used to cold roll a 30mm thick normalized plate to a 9mm thick cold-rolled plate with a reduction rate of 70%. The rolling speed is 2.0m / s, and the reduction rate per pass is ≤25% to avoid excessive deformation that could lead to structural distortion. The residual stress after cold rolling is ≤200MPa.

[0054] 3. Precise temperature-controlled annealing process:

[0055] (1) Preparation before annealing

[0056] Surface cleaning: Wipe the surface of the cold-rolled sheet with alcohol to remove oil stains, let it dry, and then put it into the annealing furnace. The spacing between the sheets should be ≥50mm to ensure uniform atmosphere flow.

[0057] Atmosphere replacement: A mixed atmosphere of 50% N2 + 50% H2 (purity ≥ 99.99%) is introduced into the annealing furnace to replace the air in the furnace (replacement is carried out 3 times, with exhaust for 30 minutes each time), and the final oxygen content in the furnace is ≤ 50 ppm.

[0058] (2) Annealing

[0059] Heating phase: Increase the temperature to the target annealing temperature (700-775℃, adjust according to the application scenario) at a rate of 8℃ / min, and maintain the mixed atmosphere flow rate at 6L / min during the heating process.

[0060] Heat preservation stage: Heat preservation at the target temperature for 2 hours to ensure complete recrystallization and promote the formation of favorable texture. During the heat preservation process, the furnace temperature is monitored in real time, and the fluctuation is ≤±1℃.

[0061] Cooling stage: After the heat preservation is completed, the furnace is cooled to 300°C at a rate of 5°C / min, and then switched to N2 atmosphere and allowed to cool naturally to room temperature to avoid stress concentration caused by excessive cooling.

[0062] 4. Performance testing and process adjustment:

[0063] (1) Tissue testing

[0064] Sampling locations: Three samples were taken from the center of the plate and three samples were taken from 50 mm from the edge. After etching with 4% nitric acid alcohol solution for 15 seconds, the samples were observed using a LEIC DAM MI 5000M metallographic microscope. The grain size was statistically analyzed using the cross-section method (effective statistical area 0.3 mm²). 2 ), EBSD technology was used to analyze recrystallization ratio and texture type.

[0065] Acceptable criteria: recrystallization ratio ≥98%, grain size 12-18μm, and favorable texture {100}+{110} ratio ≥22%.

[0066] (2) Performance testing

[0067] Magnetic performance testing: An EPMA-1720 AC magnetic performance measuring instrument was used to test B. 5000 (Magnetic induction intensity under a magnetic field strength of 5000 A / m), P 1.5 / 50 (1.5T, 50Hz low-frequency iron loss), P 1.0 / 400 (1.0T, 400Hz medium and high frequency iron loss), each condition was tested 3 times and the average value was taken.

[0068] Mechanical property testing: standard tensile specimens were prepared according to GB / T228.1-2010, and yield strength and tensile strength were tested using a CTM2050 universal tensile testing machine at a tensile rate of 2 mm / min.

[0069] Acceptance standard: B 5000 ≥1.60T, P 1.5 / 50 ≤6.8W / kg, P 1.0 / 400 ≤42W / kg, yield strength 480-550MPa, tensile strength 580-630MPa.

[0070] (3) Process adjustment

[0071] If the recrystallization rate is insufficient (<98%): increase the annealing temperature by 10-15℃ or extend the holding time by 30min;

[0072] If the grains are too large (>18μm): reduce the annealing temperature by 10-15℃ or increase the cooling rate by 1-2℃ / min;

[0073] If the magnetic properties are insufficient (B) 5000 <1.60T): Adjust the mixing atmosphere ratio to 45%N2+55%H2, or increase the annealing temperature by 5-10℃.

[0074] The core of this invention lies in "pretreatment homogenization + precise annealing temperature control + atmosphere synergy": pretreatment (hot rolling-normalizing-cold rolling) ensures uniform deformation structure, providing consistent nucleation conditions for recrystallization; precise annealing temperature of 700-775℃ controls the degree of recrystallization and grain size; 50%N2+50%H2 atmosphere inhibits oxidation and promotes the enrichment of favorable texture, ultimately achieving synergistic optimization of strong magnetic properties and solving the core pain points of traditional processes such as "insufficient recrystallization, uncontrolled texture, and performance imbalance".

[0075] Example 1 (Optimal overall performance solution for drive motor cores in new energy vehicles)

[0076] 1. Raw materials and composition (wt%): Si 3.0, Mn 0.5, Al 0.3, P 0.015, S 0.008, C 0.003, Fe balance, vacuum induction melting casting billet 200mm×120mm×800mm.

[0077] 2. Pretreatment process:

[0078] Hot rolling: 1150℃×3h→7 passes hot rolling to 30mm (final rolling temperature 900℃)→air cooling to 600℃ stack cooling;

[0079] Normalization: 950℃×1h (N2 atmosphere, flow rate 8L / min) → Cool to 500℃ at 8℃ / min and air cool;

[0080] Cold rolling: Pickled with 15% hydrochloric acid → cold rolled to 9mm with a reduction of 70% (rolling speed 2.0m / s).

[0081] 3. Precision annealing process:

[0082] Atmosphere: 50% N2 + 50% H2 mixed atmosphere (purity 99.99%), displacement 3 times;

[0083] Heating: Increase to 750℃ at 8℃ / min, hold for 2 hours (furnace temperature fluctuation ±0.8℃);

[0084] Cooling: Cool to 300℃ at 5℃ / min → Naturally cool to room temperature in N2 atmosphere.

[0085] 4. Test Results:

[0086] Microstructure and properties: recrystallization ratio 99.2%, grain size 14.8 μm, uniform microstructure with no residual deformation; EBSD analysis: favorable texture {100}+{110} accounts for 24.1%, texture factor 1.12, unfavorable texture {111} accounts for 7.74%;

[0087] Magnetic properties: B 5000 =1.613T, P 1.5 / 50 =6.62W / kg, P 1.0 / 400 =40.49W / kg;

[0088] Mechanical properties: Yield strength 496 MPa, tensile strength 598 MPa, elongation after fracture 18.5%;

[0089] Application results: It meets the requirements of "high magnetic permeability + low iron loss + anti-centrifugal force" for the iron core of drive motors in new energy vehicles, improves motor energy efficiency by 8%, and extends service life by 30%.

[0090] Example 2 (for high-speed motor rotors, high strength preferred)

[0091] 1. Raw materials and composition: Same as in Example 1, billet size 200mm×120mm×800mm.

[0092] 2. Pre-treatment process: completely consistent with Example 1 (hot rolling, normalizing, and cold rolling parameters remain unchanged).

[0093] 3. Precision annealing process:

[0094] Atmosphere: 50% N2 + 50% H2 mixed atmosphere, displacement 3 times;

[0095] Heating: Increase to 700℃ at 8℃ / min, hold for 2 hours (furnace temperature fluctuation ±0.9℃);

[0096] Cooling: Cool to 300℃ at 5℃ / min → Naturally cool to room temperature in N2 atmosphere.

[0097] 4. Test Results:

[0098] Microstructure and properties: recrystallization ratio 90.5%, grain size 10.5μm, a small amount of recovery microstructure (9.5%); favorable texture {100}+{110} accounts for 17.6% with a texture factor of 0.85, and unfavorable texture {111} accounts for 11.3%;

[0099] Magnetic properties: B 5000 =1.582T, P1.5 / 50 =7.85W / kg, P 1.0 / 400 =48.6W / kg;

[0100] Mechanical properties: Yield strength 530 MPa, tensile strength 620 MPa, elongation after fracture 16.2%;

[0101] Application effect: It is suitable for high-speed motor rotors with a speed of ≥15000r / min. The tensile strength is increased by 3.7% compared with Example 1. It can resist huge centrifugal force and the magnetic properties meet the basic energy conversion requirements.

[0102] Example 3 (For high-efficiency transformer cores, high magnetic performance is preferred)

[0103] 1. Raw materials and composition: Same as in Example 1, billet size 200mm×120mm×800mm.

[0104] 2. Pretreatment process: completely consistent with Example 1.

[0105] 3. Precision annealing process:

[0106] Atmosphere: 50% N2 + 50% H2 mixed atmosphere, displacement 3 times;

[0107] Heating: Increase to 775℃ at 8℃ / min, hold for 2 hours (furnace temperature fluctuation ±1.0℃);

[0108] Cooling: Cool to 300℃ at 5℃ / min → Naturally cool to room temperature in N2 atmosphere.

[0109] 4. Test Results:

[0110] Microstructure and properties: recrystallization ratio 99.5%, grain size 17.2μm, uniform and dense microstructure; favorable texture {100}+{110} accounts for 25.3%, texture factor 1.15, unfavorable texture {111} accounts for 6.8%;

[0111] Magnetic properties: B 5000 =1.605T, P 1.5 / 50 =6.20W / kg, P 1.0 / 400 =38.2W / kg;

[0112] Mechanical properties: Yield strength 485 MPa, tensile strength 585 MPa, elongation after fracture 19.3%;

[0113] Application results: It is compatible with high-efficiency transformer cores, and the low-frequency iron loss is reduced by 6.3% compared with Example 1. The magnetic induction intensity is maintained above 1.60T, and the energy loss is reduced by 10%, meeting the requirements of "high efficiency and energy saving" for transformers.

[0114] Comparative example (traditional annealing process, without precise temperature control and atmosphere regulation).

[0115] Process: The raw materials and pretreatment (hot rolling, normalizing, cold rolling) are the same as in Example 1. The annealing process is 780℃×1h (air atmosphere), and air cooling to room temperature (cooling rate 15℃ / min).

[0116] Test results:

[0117] Microstructure and properties: recrystallization ratio 85%, grain size non-uniform (8-25μm), residual deformed structure accounting for 15%; favorable texture {100}+{110} accounts for 12.5%, texture factor 0.68;

[0118] Magnetic properties: B 5000 =1.52T, P 1.5 / 50 =9.3W / kg, P 1.0 / 400 =56.8W / kg;

[0119] Mechanical properties: Yield strength 560 MPa, tensile strength 640 MPa, elongation after fracture 12.8%;

[0120] Defects: Insufficient recrystallization, large grain size fluctuations, poor magnetic properties and plasticity, severe imbalance of strong magnetic properties, unable to meet the requirements of high-end motors / transformers.

[0121] Performance Comparison Table

[0122] project Example 1 (Drive Motor) Example 2 (High-speed rotor) Example 3 (Transformer) Comparative Example 1 (Traditional Process) Annealing temperature (°C) 750 700 775 780 Recrystallization ratio (%) 99.2 90.5 99.5 85 Grain size (μm) 14.8 10.5 17.2 8-25 (uneven) Percentage of favorable textures (%) 24.1 17.6 25.3 12.5 <![CDATA[B 5000 (T)]]> 1.613 1.582 1.605 1.52 <![CDATA[P 1.5 / 50 (W / kg)]]> 6.62 7.85 6.20 9.3 <![CDATA[P 1.0 / 400 (W / kg)]]> 40.49 48.6 38.2 56.8 Yield strength (MPa) 496 530 485 560 Tensile strength (MPa) 598 620 585 640 Elongation after fracture (%) 18.5 16.2 19.3 12.8

[0123] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel, characterized in that, include: Heating stage: Increase the temperature at a rate of 7.5-8.5℃ / min to the target annealing temperature of 700-775℃, and maintain the N2+H2 mixed atmosphere flow rate of 5.5-6.5L / min during the heating process; Heat preservation stage: Heat preservation at the target temperature for 1.5-2.5 hours to ensure complete recrystallization and promote the formation of favorable texture. During the heat preservation process, the furnace temperature is monitored in real time, and the fluctuation is ≤±1℃. Cooling stage: After the heat preservation is completed, the furnace is cooled to 300°C at a rate of 4.8-5.2°C / min, and then switched to N2 atmosphere and allowed to cool naturally to room temperature to avoid stress concentration caused by excessive cooling.

2. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 1, characterized in that, Specifically, it includes: Heating stage: Increase the temperature at a rate of 8℃ / min to the target annealing temperature of 700-775℃, and maintain the N2+H2 mixed atmosphere flow rate of 6L / min during the heating process; Heat preservation stage: Heat preservation at the target temperature for 2 hours to ensure complete recrystallization and promote the formation of favorable texture. During the heat preservation process, the furnace temperature is monitored in real time, and the fluctuation is ≤±1℃. Cooling stage: After the heat preservation is completed, the furnace is cooled to 300°C at a rate of 5°C / min, and then switched to N2 atmosphere and allowed to cool naturally to room temperature to avoid stress concentration caused by excessive cooling.

3. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 1, characterized in that, The high-strength non-oriented silicon steel is designed with the following composition by mass fraction: Si 2.8-3.2%, Mn 0.4-0.6%, Al 0.2-0.4%, P ≤ 0.02%, S ≤ 0.01%, C ≤ 0.005%, with the remainder being Fe and unavoidable impurities.

4. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 1, characterized in that, It also includes melting and billet preparation: melting is carried out in a vacuum induction furnace, and the billet is cast into a 200mm×120mm×800mm billet with a cooling rate of 10℃ / min to avoid component segregation.

5. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 4, characterized in that, Also includes: Pretreatment process: (1) Hot rolling process Heating and holding: The billet is placed in a walking beam furnace and heated to 1150℃ at a rate of 15℃ / min, and held for 3 hours to ensure that Si and Al elements are fully dissolved and the grains are homogenized. Multi-pass hot rolling: The 200mm thick billet is rolled into a 30mm thick hot-rolled plate through 7 passes at an initial temperature of 1150℃. The reduction rates of each pass are 15%, 18%, 20%, 22%, 25%, 30%, and 35% respectively. The final rolling temperature is 900℃. High-pressure water descaling (water pressure 18MPa) is used during the hot rolling process to prevent oxide scale from being pressed in. Cooling after hot rolling: air cool to 600℃, then stack cool to room temperature, controlling the cooling rate at 15℃ / min to avoid coarse microstructure; (2) Normalization treatment Normalizing process: Place a 30mm thick hot-rolled plate into a continuous annealing furnace, under N2 atmosphere protection, with a flow rate of 8L / min, heat to 950℃ at a rate of 12℃ / min, hold for 1h, refine the hot-rolled structure and reduce residual stress. Cooling method: The furnace is cooled to 500℃ at a rate of 8℃ / min, and then air-cooled to room temperature. After normalization, the microstructure is ferrite + a small amount of pearlite, and the grain size is ≤20μm. (3) Cold rolling process Pickling pretreatment: The normalized plate is pickled with 15% hydrochloric acid solution at 60℃ for 30 minutes to remove the surface oxide layer, rinsed with water and dried. Cold rolling implementation: A six-roll cold rolling mill is used to cold roll a 30mm thick normalized plate to a 9mm thick cold-rolled plate with a reduction rate of 70%. The rolling speed is 2.0m / s, and the reduction rate per pass is ≤25% to avoid excessive deformation that could lead to structural distortion. The residual stress after cold rolling is ≤200MPa.

6. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 1 or 5, characterized in that, This also includes preparations before annealing: Surface cleaning: Wipe the surface oil stains of the cold-rolled sheet with alcohol, let it dry, and then put it into the annealing furnace. The spacing between the sheets should be ≥50mm to ensure uniform atmosphere flow. Atmosphere replacement: A mixed atmosphere of 50% N2 + 50% H2 is introduced into the annealing furnace to replace the air in the furnace, so that the final oxygen content in the furnace is ≤50ppm.

7. The heat treatment process for improving the microstructure and properties of high-strength non-oriented silicon steel according to claim 6, characterized in that, The air inside the replacement furnace was replaced a total of 3 times, with each venting process lasting 30 minutes.