A method for preparing St37-2G cold-rolled carbon structural steel
By optimizing the chemical composition and process parameters of St37-2G cold-rolled carbon structural steel, the problems of mechanical property fluctuation and grain inhomogeneity were solved, achieving product consistency and stability of forming performance, and improving production efficiency and product quality.
Patent Information
- Application Number
- CN202611260115.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-19
- Publication Date
- 2026-11-17
AI Technical Summary
The current production of St37-2G cold-rolled carbon structural steel suffers from inaccurate control of chemical composition, resulting in large fluctuations in mechanical properties, uneven grain size, unstable formability, and poor product consistency.
By optimizing chemical composition control and process parameters, including converter control, LF furnace refining, slab continuous casting, cold rolling process, bell-type annealing and leveling process, and adopting full hydrogen bell-type annealing and dynamic hydrogen flow control, combined with the precise setting of elongation rate for thickness grading, a closed-loop collaborative control of the entire process is formed.
It improves the consistency of mechanical properties between different furnace cycles, reduces the center segregation and surface crack rate of slabs, improves grain size uniformity and slab straightness, and enhances product yield and surface quality.
Abstract
Description
Technical Field
[0001] This invention relates to the field of iron and steel metallurgy technology, specifically to a method for preparing St37-2G cold-rolled carbon structural steel. Background Technology
[0002] St37-2G is a cold-rolled carbon structural steel grade defined according to the German standard DIN1623(2). Its tensile strength is 360-510 MPa, yield strength is not less than 215 MPa, and elongation after fracture is not less than 20%. It has good formability and weldability and is widely used in the manufacture of mechanical parts with relatively low load-bearing capacity, such as automotive parts, rail transit equipment structural components, chemical plant auxiliary components, and hardware products. With the increasing demands for material quality consistency and dimensional accuracy from downstream manufacturing industries, how to achieve precise control of the entire process from smelting to finished product for St37-2G cold-rolled carbon structural steel plates has become a pressing technical problem for steel companies.
[0003] Currently, the production of St37-2G cold-rolled carbon structural steel plates in China mainly refers to the Q / BQB410-2023 standard "Cold-rolled carbon structural steel plates and strips". The typical process route is: hot metal desulfurization treatment → converter smelting → LF refining → slab continuous casting → heating → hot continuous rolling → laminar flow cooling → cold rolling pickling mill → bell annealing → cold rolling leveling → recoiling → packaging.
[0004] However, existing technologies still have the following shortcomings in the production process: the chemical composition control window is relatively wide, especially the carbon content range (0.13%-0.17%) and manganese content range (0.70%-0.90%), which have a large span, resulting in significant fluctuations in mechanical properties between different furnace cycles and making it difficult to guarantee product consistency; at the same time, the matching between the bell-type annealing process parameters and the steel grade characteristics is insufficient, and the uniformity of grain size after annealing is poor, resulting in unstable product elongation and stamping performance. Summary of the Invention
[0005] The purpose of this invention is to provide a method for preparing St37-2G cold-rolled carbon structural steel, in order to solve the problems of large fluctuations in mechanical properties and poor consistency of finished products caused by the wide range of carbon and manganese composition control in existing St372G cold-rolled carbon structural steel, and the incompatibility of bell-type annealing process leading to uneven grains, unstable elongation and stamping performance.
[0006] To achieve the above objectives, the basic solution provided by this invention is as follows: a method for preparing St37-2G cold-rolled carbon structural steel, wherein the chemical composition of the St37-2G cold-rolled carbon structural steel, by weight percentage, includes C: 0.14%-0.16%, Si: ≤0.04%, Mn: 0.78%-0.84%, P: ≤0.015%, S: ≤0.008%, Al: 0.025%-0.035%, N: ≤0.005%, residual elements Cr ≤0.05%, Ni ≤0.05%, Cu ≤0.05%, Mo ≤0.05%, As ≤0.04%, V ≤0.010%, with the balance being Fe and unavoidable impurities; the method further includes the following steps: S1. Converter control: The endpoint [C] is 0.08%-0.12%, the endpoint [P] is ≤0.015%, the endpoint [S] is ≤0.025%, the tapping temperature is 1620-1660℃, the tapping time is 3.5-6min, and a dual slag-blocking measure of sliding plate slag blocking and slag detection is adopted. The phosphorus return of molten steel in the ladle is ≤0.003%. Deoxidation and alloying are added in the order of composite deoxidizer, aluminum ferroalloy, and low-carbon ferromanganese. Low-carbon ferromanganese and aluminum ferroalloy are added when the steel is 1 / 3 to 1 / 2 tapped. S2, LF furnace refining control: LF furnace refining adopts white slag operation, the white slag holding time is not less than 12 minutes, the soft blowing time is not less than 8 minutes, the killing time is not less than 6 minutes, the sulfur content of molten steel before leaving the LF furnace is controlled at ≤0.008%, the temperature at the furnace outlet is controlled according to the continuous casting requirements, and aluminum iron must not be added. S3. Slab continuous casting control: Continuous casting adopts argon protection throughout the process, using carbon-free protective slag and carbon-free ladle covering agent. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The target slab casting speed is 1.4±0.1m / min. Constant casting speed is used, with casting speed fluctuation ≤0.05m / min. The liquid level fluctuation in the crystallizer is controlled within ±3mm. The arc of the continuous casting machine head is ≤0.05mm, the streamline arc of the continuous casting machine is ≤1±0.3mm, the slab straightening temperature is not lower than 950℃, and the number of tundish continuous castings is not more than 25. Slag is removed once every 4-5 heats. S4. Slab heating and hot continuous rolling control: The slab heating temperature, roughing rolling temperature and coiling temperature are all controlled according to the finished product thickness. The slab heating time in the furnace is ≥160min, the temperature difference between the head and tail of the slab is ≤20℃, the final rolling temperature is 860±20℃, the descaling pressure is ≥18.5MPa, the laminar flow cooling adopts the front-end low-pressure sparse cooling mode, and the failure valve ratio is ≤10%. S5. Cold rolling process control: HCl concentration in acid tank #1 is ≥45g / L, iron ion concentration is ≤120g / L, temperature of acid tanks #1-#4 is 65-80℃, acid specific gravity in acid tank #4 is controlled at 1.09-1.15, cold rolling mill stands F1-F5 are allocated according to differentiated reduction rate, total reduction rate is controlled at 60%-75%, deformation of rolling mill #5 is controlled at 8%-10%, and plate surface roughness is controlled at 0.8-1.5μm; S6. Bell-type annealing process control: All-hydrogen bell-type annealing is adopted, the annealing curve adopts process curve No. 103, and the furnace exit temperature is ≤95℃. S7. Leveling process control: The elongation rate mode is adopted to control the leveling elongation rate according to the thickness of the finished product. S8. Oiling and Straightening: Oil application amount 0.6-1.1 g / m 2 The elongation of the tension leveler is controlled at 0.6%-1.1%.
[0007] The beneficial effects of the present invention are as follows: (1) By narrowing the chemical composition C: 0.14%-0.16% and Mn: 0.78%-0.84%, the consistency of mechanical properties between different heats is improved while ensuring the good formability of St37-2G steel, and the yield strength fluctuation range is controlled within ±15MPa; (2) The continuous casting process adopts a strategy of low superheat, high precision liquid level control and constant casting speed, which effectively reduces the occurrence rate of slab center segregation and surface cracks. The center segregation of the slab at low magnification is ≤0.5 grade, and the surface defect-free rate reaches more than 98.5%. (3) The bell-type annealing process adopts a staged dynamic hydrogen flow control strategy, combined with optimized heating rate and heat preservation regime, which significantly improves the uniformity of grain size after annealing and controls the grain size at level 9.0-9.5. (4) The flattening process has established a precise setting system for elongation rate based on thickness grading, realizing the coordinated control of plate flatness and surface roughness. The flatness of the finished plate is ≤3IU and the surface reflectivity is ≥70%. (5) The parameters of each process in the whole process form a closed-loop collaborative control system, and the overall yield of the product is 3-5 percentage points higher than that of traditional processes, which is suitable for large-scale stable industrial production.
[0008] Option 2, which is the preferred option of the basic option, in S3, the superheat of molten steel in the tundish is controlled as follows: first heat ≤ 42℃, consecutive heats ≤ 32℃.
[0009] Option 3, which is the preferred option of the basic option, in S4, the slab heating temperature, rough rolling temperature, and coiling temperature are controlled according to the finished product thickness as follows: Slab heating temperature: When the finished product thickness is 1.2-3.99mm, the slab heating temperature is 1200±30℃; when the finished product thickness is 4-6mm, the slab heating temperature is 1180±30℃. Rough rolling temperature: When the finished product thickness is 1.2-3.99mm, the rough rolling temperature is 1100±30℃; when the finished product thickness is 4-6mm, the rough rolling temperature is 1080±30℃. Winding temperature: When the finished product thickness is 1.2-3mm, the winding temperature is 590±20℃; when the finished product thickness is 3.01-6mm, the winding temperature is 600±20℃.
[0010] Option 4 is the preferred option of the basic option. In S6, the specific control of process curve No. 103 is as follows: Heating stage: Heat the steel coil to the annealing process temperature of 680-710℃ at a heating rate of 45-60℃ / h, maintaining a hydrogen flow rate of 10-25m³ / h during the heating process. 3 / h; Insulation stage: Insulate at 680-710℃ for 8-12 hours. For the first 2 hours of high-temperature insulation, purge hydrogen at a flow rate of 8-10 m³ / h. 3 / h is used for control.
[0011] Option 5, which is the preferred option of the basic option, involves controlling the flatness elongation rate based on the finished product thickness in S7 as follows: When the finished product thickness is 0.15-0.35mm, the flatness rate is 0.4%-0.6%, with a target value of 0.5%. When the finished product thickness is 0.351-0.45mm, the flatness rate is 0.5%-0.7%, with a target value of 0.6%. When the finished product thickness is 0.451-0.75mm, the flatness rate is 0.7%-0.9%, with a target value of 0.8%. When the finished product thickness is 0.751-0.85mm, the flatness rate is 0.8%-1.0%, with a target value of 0.9%. When the finished product thickness is 0.851-0.95mm, the flatness rate is 0.9%-1.1%, with a target value of 1.0%. When the finished product thickness is 0.951-1.05mm, the flatness rate is 1.0%-1.2%, with a target value of 1.1%. When the finished product thickness is 1.051-1.15mm, the flatness rate is 1.1%-1.3%, with a target value of 1.2%. When the finished product thickness is 1.151-1.25mm, the flatness rate is 1.2%-1.4%, with a target value of 1.3%. When the finished product thickness is 1.251-1.49mm, the flatness rate is 1.3%-1.6%, with a target value of 1.5%. When the finished product thickness is 1.491-1.8mm, the flatness rate is 1.5%-1.7%, with a target value of 1.6%. When the finished product thickness is ≥1.801mm, the flatness rate is 1.8%-2.0%, with a target value of 1.9%.
[0012] Option 6, the preferred option of the basic option, requires St37-2G cold-rolled carbon structural steel with a yield strength ≥235MPa, tensile strength of 360-510MPa, elongation after fracture ≥36%, surface roughness Ra is tested at one-quarter of the plate width, finished product roughness is controlled to 0.7-1.2μm, and plate straightness ≤3IU. Detailed Implementation
[0013] The present invention will be further described in detail below through specific embodiments: Example 1
[0014] A method for preparing St37-2G cold-rolled carbon structural steel, wherein the chemical composition of the St37-2G cold-rolled carbon structural steel, by weight percentage, includes C: 0.14%-0.16%, Si: ≤0.04%, Mn: 0.78%-0.84%, P: ≤0.015%, S: ≤0.008%, Al: 0.025%-0.035%, N: ≤0.005%, residual elements Cr ≤0.05%, Ni ≤0.05%, Cu ≤0.05%, Mo ≤0.05%, As ≤0.04%, V ≤0.010%, with the balance being Fe and unavoidable impurities; the method further includes the following steps: S1. Converter control: The endpoint [C] is 0.08%-0.12%, the endpoint [P] is ≤0.015%, the endpoint [S] is ≤0.025%, the tapping temperature is 1620-1660℃, the tapping time is 3.5-6min, and a dual slag-blocking measure of sliding plate slag blocking and slag detection is adopted. The phosphorus return of molten steel in the ladle is ≤0.003%. Deoxidation and alloying are added in the order of composite deoxidizer, aluminum ferroalloy, and low-carbon ferromanganese. Low-carbon ferromanganese and aluminum ferroalloy are added when the steel is 1 / 3 to 1 / 2 tapped. S2, LF furnace refining control: LF furnace refining adopts white slag operation, the white slag holding time is not less than 12 minutes, the soft blowing time is not less than 8 minutes, the killing time is not less than 6 minutes, the sulfur content of molten steel before leaving the LF furnace is controlled at ≤0.008%, the temperature at the furnace outlet is controlled according to the continuous casting requirements, and aluminum iron must not be added. S3. Slab continuous casting control: Continuous casting adopts full argon protection pouring, using carbon-free protective slag and carbon-free ladle covering agent. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The superheat of molten steel in the tundish is controlled as follows: first heat ≤42℃, continuous casting heats ≤32℃. The target slab casting speed is 1.4±0.1m / min. Constant casting speed is used, with casting speed fluctuation ≤0.05m / min. The liquid level fluctuation in the crystallizer is controlled within ±3mm. The arc of the continuous casting machine head is ≤0.05mm. The streamline arc of the continuous casting machine is ≤1±0.3mm. The slab straightening temperature is not lower than 950℃. The number of continuous casting heats in the tundish is not more than 25. Slag is removed once every 4-5 heats. S4. Slab Heating and Hot Rolling Control: The slab heating temperature, roughing rolling temperature, and coiling temperature are all controlled according to the finished product thickness. Slab heating temperature: 1200±30℃ for finished product thickness of 1.2-3.99mm; 1180±30℃ for finished product thickness of 4-6mm. Roughing rolling temperature: 1100±30℃ for finished product thickness of 1.2-3.99mm; 1100±30℃ for finished product thickness of 4-6mm. When the thickness is m, the roughing temperature is 1080±30℃; the coiling temperature is 590±20℃ when the finished product thickness is 1.2-3mm, and 600±20℃ when the finished product thickness is 3.01-6mm; the slab heating time in the furnace is ≥160min, the temperature difference between the head and tail of the slab is ≤20℃, the final rolling temperature is 860±20℃, the descaling pressure is ≥18.5MPa, the laminar flow cooling adopts the front-stage low-pressure sparse cooling mode, and the failure valve ratio is ≤10%; S5. Cold rolling process control: HCl concentration in acid tank #1 is ≥45g / L, iron ion concentration is ≤120g / L, temperature of acid tanks #1-#4 is 65-80℃, acid specific gravity in acid tank #4 is controlled at 1.09-1.15, cold rolling mill stands F1-F5 are allocated according to differentiated reduction rate, total reduction rate is controlled at 60%-75%, deformation of rolling mill #5 is controlled at 8%-10%, and plate surface roughness is controlled at 0.8-1.5μm; S6. Bell-type annealing process control: All-hydrogen bell-type annealing is adopted, and the annealing curve uses process curve No. 103. The specific control of process curve No. 103 is as follows: Heating stage: Heat the steel coil to the annealing process temperature of 680-710℃ at a heating rate of 45-60℃ / h, maintaining a hydrogen flow rate of 10-25m³ / h during the heating process. 3 / h; Heat preservation stage: heat preservation at 680-710℃ for 8-12 hours, with hydrogen blowing flow rate of 8-10 m³ / h for the first 2 hours of high-temperature heat preservation. 3 The temperature is controlled by / h, and the furnace exit temperature is ≤95℃; S7. Leveling Process Control: An elongation rate model is adopted, controlling the leveling elongation rate based on the finished product thickness. The specific control method for the leveling elongation rate based on the finished product thickness is as follows: When the finished product thickness is 0.15-0.35mm, the flatness rate is 0.4%-0.6%, with a target value of 0.5%. When the finished product thickness is 0.351-0.45mm, the flatness rate is 0.5%-0.7%, with a target value of 0.6%. When the finished product thickness is 0.451-0.75mm, the flatness rate is 0.7%-0.9%, with a target value of 0.8%. When the finished product thickness is 0.751-0.85mm, the flatness rate is 0.8%-1.0%, with a target value of 0.9%. When the finished product thickness is 0.851-0.95mm, the flatness rate is 0.9%-1.1%, with a target value of 1.0%. When the finished product thickness is 0.951-1.05mm, the flatness rate is 1.0%-1.2%, with a target value of 1.1%. When the finished product thickness is 1.051-1.15mm, the flatness rate is 1.1%-1.3%, with a target value of 1.2%. When the finished product thickness is 1.151-1.25mm, the flatness rate is 1.2%-1.4%, with a target value of 1.3%. When the finished product thickness is 1.251-1.49mm, the flatness rate is 1.3%-1.6%, with a target value of 1.5%. When the finished product thickness is 1.491-1.8mm, the flatness rate is 1.5%-1.7%, with a target value of 1.6%. When the finished product thickness is ≥1.801mm, the flatness rate is 1.8%-2.0%, with a target value of 1.9%; S8. Oiling and Straightening: Oil application amount 0.6-1.1 g / m 2 The elongation of the tension leveler is controlled at 0.6%-1.1%.
[0015] St37-2G cold-rolled carbon structural steel has a yield strength ≥235MPa, a tensile strength of 360-510MPa, an elongation after fracture ≥36%, a surface roughness Ra measured at one-quarter of the plate width, a finished product roughness controlled to 0.7-1.2μm, and a plate straightness ≤3IU.
[0016] Example 2
[0017] A method for preparing St37-2G cold-rolled carbon structural steel includes the following steps: Step 1, Hot metal pretreatment: The original hot metal has [Si]≤0.80%, [P]≤0.140%, [S]≤0.06%, and the hot metal temperature is ≥1280℃. After desulfurization, the hot metal entering the converter has [S]≤0.008%. After desulfurization, the slag is removed. Step 2, Converter smelting: A 120t converter was used for smelting, with the final control values of [C] being 0.10%, [P] being 0.012%, and [S] being 0.020%; the tapping temperature was 1640℃, the tapping time was 4.5min, and a double slag-blocking system of sliding plate slag blocking and slag detection was used; the phosphorus return in the ladle steel was 0.002%; when 1 / 3 of the steel was tapped, composite deoxidizer, ferroaluminum, and low-carbon ferromanganese were added sequentially for deoxidation and alloying. Step 3, LF refining: white slag holding time 13min, soft blowing time 8.5min, settling time 7min, LF outlet sulfur content 0.006%, outlet temperature controlled according to continuous casting requirements; Step 4, Slab Continuous Casting: Continuous casting is carried out under full argon protection, with no carbon protective slag and a slag moisture content (H2O) ≤ 0.5%; the superheat of the tundish in the first heat is 40℃, and the superheat of the tundish in subsequent heats is 30℃; the target casting speed is 1.4 m / min, with a casting speed fluctuation of 0.03 m / min; the liquid level fluctuation in the crystallizer is ±2 mm; the die head arc is 0.04 mm, and the streamline arc is 0.9 mm; the slab straightening temperature is 980℃; 20 heats are continuously cast from the tundish, with slag removal every 5 heats; Step 5, Slab Heating and Hot Continuous Rolling: Slab heating temperature 1200℃, furnace time 170min, head-to-tail temperature difference 15℃; roughing temperature 1100℃, finishing temperature 860℃, coiling temperature 590℃; descaling pressure 19.5MPa; layer cooling adopts front-stage low-pressure sparse cooling mode, fault valve ratio 6%; Step 6, Pickling and Cold Rolling: HCl concentration in acid tank #1 is 50 g / L, iron ion concentration is 80 g / L, and acid tank temperature is 72℃; total reduction rate of five-stand continuous rolling is 68%, and the surface roughness is 1.0 μm; Step 7, Bell-type annealing: Bell-type annealing with all-hydrogen gas is used, with a heating rate of 50℃ / h, heating to the annealing temperature of 700℃, and holding for 10 hours; the hydrogen flow rate is 8m³ / h for the first 2 hours of the high-temperature holding stage. 3 / h, furnace exit temperature 94℃; Step 8, Leveling: Using the elongation rate model, the finished product thickness is 1.0mm, the target elongation rate for leveling is 1.1%, and the actual control is 1.08%; Step 9, Oiling and Straightening: Straightening machine elongation 0.65%, light oiling 0.8g / m. 2 .
[0018] The St37-2G cold-rolled carbon structural steel plate obtained in this embodiment was tested and found to have the following mechanical properties: yield strength 265MPa, tensile strength 395MPa, elongation after fracture 35%; plate flatness 3IU; surface reflectivity 78%; metallographic structure is ferrite + a small amount of pearlite, grain size 9.5 grade, and no banded structure.
[0019] Example 3
[0020] A method for preparing St37-2G cold-rolled carbon structural steel. The difference between this embodiment and Embodiment 2 lies in the adjustment of process parameters.
[0021] Steps 1-3 are the same as in Example 2; Step 4, slab continuous casting: the superheated temperature of the tundish in the first heat is 38℃, and the superheated temperature of the tundish in the subsequent heats is 28℃; the target casting speed is 1.45m / min, and the casting speed fluctuation is 0.04m / min; the liquid level fluctuation in the crystallizer is ±3mm; 22 heats are continuously cast from the tundish; Step 5, Slab heating and hot continuous rolling: Slab heating temperature 1190℃, furnace time 165min; rough rolling temperature 1090℃, final rolling temperature 855℃, coiling temperature 595℃; descaling pressure 19.0MPa; Step 6, pickling and cold rolling: total reduction 72%, surface roughness 1.1μm; Step 7, bell-type annealing: heating rate 55℃ / h, annealing temperature 690℃, holding time 11h; hydrogen flow rate 8m³ / h for the first 2 hours of the high-temperature holding stage. 3 / h, furnace exit temperature 95℃; Step 8, Leveling: Finished product thickness 0.6mm, target leveling elongation 0.6%, actual control 0.58%; Step 9, Oiling and Straightening: Straightening machine elongation 0.79%, light oiling 0.7g / m. 2 .
[0022] The St37-2G cold-rolled carbon structural steel plate obtained in this embodiment was tested and found to have the following mechanical properties: yield strength 258MPa, tensile strength 388MPa, elongation after fracture 39%; plate flatness 2IU; surface reflectivity 76%; metallographic structure is ferrite + a small amount of pearlite, grain size 9.0 grade, and no banded structure.
[0023] Example 4
[0024] A method for preparing St37-2G cold-rolled carbon structural steel. The difference between this embodiment and Embodiment 2 lies in the adjustment of process parameters.
[0025] Steps 1-3 are the same as in Example 2; Step 4, slab continuous casting: the superheated temperature of the tundish in the first heat is 42℃, and the superheated temperature of the tundish in the subsequent heats is 32℃; the target casting speed is 1.35m / min, the casting speed fluctuation is 0.05m / min; the liquid level fluctuation in the crystallizer is ±3mm; Step 5, Slab heating and hot continuous rolling: Slab heating temperature 1210℃, furnace time 175min; rough rolling temperature 1110℃, final rolling temperature 865℃, coiling temperature 585℃; Step 6, pickling and cold rolling: total reduction rate 65%; Step 7, bell-type annealing: heating rate 60℃ / h, annealing temperature 710℃, holding time 9h; hydrogen flow rate is the same as in Example 2; Step 8, Leveling: Finished product thickness 1.5mm, target leveling elongation 1.6%, actual control 1.58%; Step 9, Oiling and Straightening: Straightening machine elongation 0.85%, light oiling 0.8g / m. 2 .
[0026] The St37-2G cold-rolled carbon structural steel plate obtained in this embodiment was tested and found to have the following mechanical properties: yield strength 272 MPa, tensile strength 402 MPa, elongation after fracture 29%; plate flatness 2 IU; surface reflectivity 77%; metallographic structure is ferrite + a small amount of pearlite, grain size 9.2 grade, and no banded structure.
[0027] In summary, this invention improves the mechanical property stability and surface quality consistency of St37-2G cold-rolled carbon structural steel plates through coordinated control of parameters in all processes.
[0028] The above descriptions are merely embodiments of the present invention, and common knowledge regarding specific structures and characteristics is not elaborated upon here. It should be noted that those skilled in the art can make various modifications and improvements without departing from the structure of the present invention, and these should also be considered within the scope of protection of the present invention. These modifications and improvements will not affect the effectiveness of the present invention or the practicality of the patent. The scope of protection claimed in this application should be determined by the content of its claims, and the specific embodiments described in the specification can be used to interpret the content of the claims.
Claims
1. A method for preparing St37-2G cold-rolled carbon structural steel, characterized in that, The chemical composition of St37-2G cold-rolled carbon structural steel, by weight percentage, includes C: 0.14%-0.16%, Si: ≤0.04%, Mn: 0.78%-0.84%, P≤0.015%, S≤0.008%, Al: 0.025%-0.035%, N≤0.005%, residual elements Cr≤0.05%, Ni≤0.05%, Cu≤0.05%, Mo≤0.05%, As≤0.04%, V≤0.010%, with the balance being Fe and unavoidable impurities; It also includes the following steps: S1. Converter control: The endpoint [C] is 0.08%-0.12%, the endpoint [P] is ≤0.015%, the endpoint [S] is ≤0.025%, the tapping temperature is 1620-1660℃, the tapping time is 3.5-6min, and a dual slag-blocking measure of sliding plate slag blocking and slag detection is adopted. The phosphorus return of molten steel in the ladle is ≤0.003%. Deoxidation and alloying are added in the order of composite deoxidizer, aluminum ferroalloy, and low-carbon ferromanganese. Low-carbon ferromanganese and aluminum ferroalloy are added when the steel is 1 / 3 to 1 / 2 tapped. S2, LF furnace refining control: LF furnace refining adopts white slag operation, the white slag holding time is not less than 12 minutes, the soft blowing time is not less than 8 minutes, the killing time is not less than 6 minutes, the sulfur content of molten steel before leaving the LF furnace is controlled at ≤0.008%, the temperature at the furnace outlet is controlled according to the continuous casting requirements, and aluminum iron must not be added. S3. Slab continuous casting control: Continuous casting adopts argon protection throughout the process, using carbon-free protective slag and carbon-free ladle covering agent. The water content (H2O) of the protective slag and covering agent is ≤0.5%. The target slab casting speed is 1.4±0.1m / min. Constant casting speed is used, with casting speed fluctuation ≤0.05m / min. The liquid level fluctuation in the crystallizer is controlled within ±3mm. The arc of the continuous casting machine head is ≤0.05mm, the streamline arc of the continuous casting machine is ≤1±0.3mm, the slab straightening temperature is not lower than 950℃, and the number of tundish continuous castings is not more than 25. Slag is removed once every 4-5 heats. S4. Slab heating and hot continuous rolling control: The slab heating temperature, roughing rolling temperature and coiling temperature are all controlled according to the finished product thickness. The slab heating time in the furnace is ≥160min, the temperature difference between the head and tail of the slab is ≤20℃, the final rolling temperature is 860±20℃, the descaling pressure is ≥18.5MPa, the laminar flow cooling adopts the front-end low-pressure sparse cooling mode, and the failure valve ratio is ≤10%. S5. Cold rolling process control: HCl concentration in acid tank #1 is ≥45g / L, iron ion concentration is ≤120g / L, temperature of acid tanks #1-#4 is 65-80℃, acid specific gravity in acid tank #4 is controlled at 1.09-1.15, cold rolling mill stands F1-F5 are allocated according to differentiated reduction rate, total reduction rate is controlled at 60%-75%, deformation of rolling mill #5 is controlled at 8%-10%, and plate surface roughness is controlled at 0.8-1.5μm; S6. Bell-type annealing process control: All-hydrogen bell-type annealing is adopted, the annealing curve adopts process curve No. 103, and the furnace exit temperature is ≤95℃. S7. Leveling process control: The elongation rate mode is adopted to control the leveling elongation rate according to the thickness of the finished product. S8. Oiling and Straightening: Oil application amount 0.6-1.1 g / m 2 The elongation of the tension leveler is controlled at 0.6%-1.1%.
2. The method for preparing St37-2G cold-rolled carbon structural steel according to claim 1, characterized in that, In S3, the superheat of molten steel in the tundish is controlled as follows: first heat ≤ 42℃, subsequent heats ≤ 32℃.
3. The method for preparing St37-2G cold-rolled carbon structural steel according to claim 1, characterized in that, In S4, the slab heating temperature, rough rolling temperature, and coiling temperature are controlled according to the finished product thickness as follows: Slab heating temperature: When the finished product thickness is 1.2-3.99mm, the slab heating temperature is 1200±30℃; when the finished product thickness is 4-6mm, the slab heating temperature is 1180±30℃. Rough rolling temperature: When the finished product thickness is 1.2-3.99mm, the rough rolling temperature is 1100±30℃; when the finished product thickness is 4-6mm, the rough rolling temperature is 1080±30℃. Winding temperature: When the finished product thickness is 1.2-3mm, the winding temperature is 590±20℃; when the finished product thickness is 3.01-6mm, the winding temperature is 600±20℃.
4. The method for preparing St37-2G cold-rolled carbon structural steel according to claim 1, characterized in that, In S6, the specific control of process curve No. 103 is as follows: Heating stage: Heat the steel coil to the annealing process temperature of 680-710℃ at a heating rate of 45-60℃ / h, maintaining a hydrogen flow rate of 10-25m³ / h during the heating process. 3 / h; Insulation stage: Insulate at 680-710℃ for 8-12 hours. For the first 2 hours of high-temperature insulation, purge hydrogen at a flow rate of 8-10 m³ / h. 3 / h is used for control.
5. The method for preparing St37-2G cold-rolled carbon structural steel according to claim 1, characterized in that, In S7, the specific control method for controlling the flatness elongation rate based on the finished product thickness is as follows: When the finished product thickness is 0.15-0.35mm, the flatness rate is 0.4%-0.6%, with a target value of 0.5%. When the finished product thickness is 0.351-0.45mm, the flatness rate is 0.5%-0.7%, with a target value of 0.6%. When the finished product thickness is 0.451-0.75mm, the flatness rate is 0.7%-0.9%, with a target value of 0.8%. When the finished product thickness is 0.751-0.85mm, the flatness rate is 0.8%-1.0%, with a target value of 0.9%. When the finished product thickness is 0.851-0.95mm, the flatness rate is 0.9%-1.1%, with a target value of 1.0%. When the finished product thickness is 0.951-1.05mm, the flatness rate is 1.0%-1.2%, with a target value of 1.1%. When the finished product thickness is 1.051-1.15mm, the flatness rate is 1.1%-1.3%, with a target value of 1.2%. When the finished product thickness is 1.151-1.25mm, the flatness rate is 1.2%-1.4%, with a target value of 1.3%. When the finished product thickness is 1.251-1.49mm, the flatness rate is 1.3%-1.6%, with a target value of 1.5%. When the finished product thickness is 1.491-1.8mm, the flatness rate is 1.5%-1.7%, with a target value of 1.6%. When the finished product thickness is ≥1.801mm, the flatness rate is 1.8%-2.0%, with a target value of 1.9%.
6. The method for preparing St37-2G cold-rolled carbon structural steel according to claim 1, characterized in that, St37-2G cold-rolled carbon structural steel has a yield strength ≥235MPa, a tensile strength of 360-510MPa, an elongation after fracture ≥36%, a surface roughness Ra measured at one-quarter of the plate width, a finished product roughness controlled to 0.7-1.2μm, and a plate straightness ≤3IU.