A method for improving the properties of oxide pellets, mainly composed of Bayan Obo iron concentrate, using Indian iron concentrate.

By rationally combining Indian iron ore concentrate and Bayan Obo iron ore concentrate, and optimizing the pellet preparation process, the performance problems of Bayan Obo iron ore concentrate in the preparation of oxidized pellets were solved, the compressive strength of the pellets was improved and the reduction expansion rate was reduced, thus meeting the production requirements of blast furnace ironmaking.

CN123108288APending Publication Date: 2026-11-17INNER MONGOLIA BAOTOU STEEL UNION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611024779.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-10
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The preparation of oxide pellets from Bayan Obo iron concentrate suffers from increased porosity due to the volatilization of impurities such as fluorine and sulfur, poor intergranulation of iron mineral particles, low cold compressive strength of finished pellets, insufficient drum strength, high low-temperature reduction pulverization rate, and small specific surface area, making it difficult to form green pellets and failing to meet the requirements of high-efficiency blast furnace smelting.

Method used

Oxidized iron ore pellets were prepared by mixing Indian iron concentrate and Bayan Obo iron concentrate in a certain proportion, combined with disc pelletizing, drying, preheating and roasting processes, and the raw material ratio was optimized to improve the pellet strength and metallurgical performance.

Benefits of technology

It improved the compressive strength of oxidized pellets and reduced the reduction expansion rate, meeting the requirements of blast furnace ironmaking production and enabling the large-scale application of Bayan Obo iron concentrate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention discloses a method for improving the performance of oxide pellets, primarily composed of Bayan Obo iron concentrate, using Indian iron concentrate. The method involves first mixing 95-100% Bayan Obo iron concentrate, 0-5% Indian iron concentrate, and 2.5% bentonite by mass percentage. The mixture is then subjected to a pelletizing process on a disc pelletizer. After a certain time, green pellets are obtained. Green pellets of 10-16 mm are screened out. These green pellets are further dried, preheated, and roasted to obtain the finished pellets. This invention can effectively improve the compressive strength of oxide pellets used in blast furnace ironmaking and reduce the reduction expansion rate, providing theoretical guidance for meeting the requirements of blast furnace production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of blast furnace ironmaking raw material pelletizing technology, and particularly relates to a method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate. Background Technology

[0002] The Bayan Obo iron ore mine is an important polymetallic symbiotic iron ore deposit in my country, and its iron concentrate is a core raw material for blast furnace ironmaking in large steel enterprises in northern China. Bayan Obo iron concentrate is characterized by high total iron content and high natural alkalinity, but it also has inherent defects such as high content of harmful impurities such as fluorine, potassium, and sodium, low SiO2 content, small specific surface area of ​​mineral particles, and poor sphericity.

[0003] When using a single Bayan Obo iron concentrate to prepare oxide pellets, impurities such as fluorine and sulfur volatilize at high temperatures during the preheating roasting process, leading to a significant increase in the internal porosity of the pellets and poor intergranulation between iron mineral particles. This directly results in a series of performance problems in the finished pellets, such as low cold compressive strength, insufficient drum strength, high low-temperature reduction pulverization rate, and excessive reduction expansion rate, which cannot meet the raw material requirements for efficient blast furnace smelting. At the same time, its low specific surface area makes it difficult to form green pellets, and the green pellets' drop strength and compressive strength do not meet the standards. During the production process, they are prone to breakage and pulverization, affecting the stable operation of the pellet production line.

[0004] Currently, the industry typically improves the performance of Bayan Obo iron concentrate pellets by adding other common iron concentrates, adding modifiers, or optimizing the roasting process. However, existing technologies have many shortcomings. The modification effect of common iron concentrates is limited, failing to effectively suppress reduction expansion and reduce reduction pulverization rate. Some modifiers are costly and introduce new impurities, affecting pellet grade. Simply optimizing the roasting process significantly increases energy consumption, resulting in poor production economics, and fails to fundamentally address the defects in the ore phase itself.

[0005] Indian iron ore concentrate, as a high-quality imported iron ore, possesses characteristics such as moderate SiO2 content, stable Al2O3 content, extremely low harmful impurities, reasonable particle size distribution, and excellent pelletizing properties. Its mineral composition and physicochemical properties can complement those of Bayan Obo iron ore concentrate. Based on this, this invention addresses the performance shortcomings of Bayan Obo iron ore concentrate oxidized pellets by precisely matching the ratio of the two iron ore concentrates and combining them with an optimized pelletizing process. This addresses the performance shortcomings of Bayan Obo iron ore concentrate oxidized pellets at the raw material ratio level, eliminating the need for expensive modifiers and achieving a comprehensive improvement in pellet strength and metallurgical properties. Summary of the Invention

[0006] The purpose of this invention is to provide a method for improving the performance of oxide pellets, primarily composed of Bayan Obo iron ore concentrate, using Indian iron concentrate. The method involves uniformly mixing Indian iron concentrate, Bayan Obo iron ore concentrate, and bentonite in a specific ratio, followed by pelletizing on a disc pelletizer. After a certain time, green pellets are obtained. These green pellets are then dried, preheated, and roasted to obtain the finished oxide pellets. This invention can effectively improve the compressive strength of oxide pellets used in blast furnace ironmaking and reduce the reduction expansion rate, providing theoretical guidance for meeting the requirements of blast furnace production.

[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution: This invention discloses a method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate. The method involves first mixing 95-100% Bayan Obo iron concentrate, 0%-5% Indian iron concentrate, and 2.5% bentonite by mass percentage. The mixture is then subjected to a pelletizing process on a disc pelletizer. After a certain time, green pellets are obtained. Green pellets of 10-16 mm are screened out. The green pellets are further dried, preheated, and roasted to obtain the finished pellets. The drying conditions for the green pellets include: a temperature of 130-150℃ and a time of 40-60 minutes; the preheating conditions include: a temperature of 600-800℃ and a time of 10-15 minutes; and the roasting conditions include: a temperature of 1200-1250℃ and a time of 15-30 minutes.

[0008] Furthermore, the chemical composition of the Bayan Obo iron concentrate, by mass percentage, includes 64.00–68.00% TFe, 26.00–30.00% FeO, 0.50–2.00% CaO, 1.50–4.50% SiO2, 0.20–1.00% MgO, 0.10–1.00% Al2O3, 0.05–0.25% K2O, 0.10–0.30% Na2O, 0.20–0.40% F, and 0.30–0.90% S, with 75–95% of the iron concentrate having a particle size less than 0.074 mm.

[0009] Furthermore, the Indian iron concentrate contains 51.00–55.00% TFe, 1.00–3.00% FeO, 0.10–0.20% CaO, 14.0–15.00% SiO2, 0.13–0.15% MgO, 5.10–6.20% Al2O3, and 0.20–0.30% TiO2.

[0010] Furthermore, the bentonite binder comprises, by mass percentage: 1.30–3.50% CaO, 60.00–69.00% SiO2, 1.50–4.00% MgO, 12.00–16.00% Al2O3, 1.00–3.00% K2O, and 1.00–3.00% Na2O, with bentonite particles smaller than 0.074 mm accounting for more than 98%.

[0011] Furthermore, the chemical composition of the Bayan Obo iron concentrate, by mass percentage, includes: 66.80% TFe, 28.90% FeO, 0.76% CaO, 2.52% SiO2, 0.56% MgO, 0.48% Al2O3, 0.13% K2O, 0.15% Na2O, 0.32% F, and 0.74% S, with 85% of the iron concentrate having a particle size less than 0.074 mm.

[0012] Furthermore, the chemical composition of the Indian iron concentrate, by mass percentage, includes: 51.24% TFe, 1.93% FeO, 0.092% CaO, 14.15% SiO2, 0.136% MgO, 5.78% Al2O3, 0.125% K2O, 0.073% Na2O, 0.050% F, and 0.034% S.

[0013] Furthermore, the bentonite binder comprises, by mass percentage: 1.30–3.50% CaO, 60.00–69.00% SiO2, 1.50–4.00% MgO, 12.00–16.00% Al2O3, 1.00–3.00% K2O, and 1.00–3.00% Na2O, with bentonite particles smaller than 0.074 mm accounting for more than 98%.

[0014] Compared with the prior art, the beneficial technical effects of the present invention are as follows: This invention prepares oxidized pellets by rationally combining Indian iron concentrate and Bayan Obo iron concentrate. The produced oxidized pellets have a TFe content greater than 62.00%, a compressive strength greater than 2700 N / pellet, and a reduction expansion rate less than 20%, meeting the quality indicators of pellets. This invention effectively solves the problem of high reduction expansion rate when Bayan Obo iron concentrate is used alone to prepare oxidized pellets, and realizes the large-scale application of Bayan Obo iron concentrate in the pellet production process. Detailed Implementation

[0015] The present invention will be further described below with reference to embodiments: In this invention, three raw materials—Bayan Obo iron concentrate, Indian iron concentrate, and bentonite binder—were selected for different proportion tests to prepare pellets. The chemical composition of the Bayan Obo iron concentrate, by mass percentage, includes: 66.80% TFe, 28.90% FeO, 0.76% CaO, 2.52% SiO2, 0.56% MgO, 0.48% Al2O3, 0.13% K2O, 0.15% Na2O, 0.32% F, and 0.74% S, with 85% of the iron concentrate having a particle size less than 0.074 mm. The chemical composition of the Indian iron concentrate, by mass percentage, includes: 51.24% TFe, 1.93% FeO, 0.092% CaO, 14.15% SiO2, 0.136% MgO, 5.78% Al2O3, 0.125% K2O, 0.073% Na2O, 0.050% F, and 0.034% S. The bentonite binder comprises, by mass percentage: 2.52% CaO, 66.63% SiO2, 3.76% MgO, 14.49% Al2O3, 1.68% K2O, and 1.96% Na2O, with 100% of the bentonite particles having a size less than 0.074 mm. The chemical composition and proportioning scheme of the raw materials used in the preparation experiments of oxidized pellets in each embodiment are shown in Tables 1 and 2.

[0016] Table 1 Chemical composition of raw materials used in the preparation of oxidized pellets for each implementation scheme / %

[0017] Table 2 Experimental Batching Scheme for Oxidized Pellet Preparation

[0018] According to the raw materials described in Table 1 and the batching scheme shown in Table 2, the pelletizing raw materials were mixed evenly, and then rolled into green pellets by spraying water on a disc pelletizer. The particle size of the green pellets was controlled at 10-16 mm, the moisture content was controlled at 8-10%, and the compressive strength was 9-18 N / pellet. The green pellets were further dried at 130℃ for 40 min to obtain dry pellets. The dry pellets were further preheated at 800℃ for 10 min to obtain preheated pellets. The preheated pellets were further oxidized and roasted at 1200℃ for 15 min to obtain the finished oxidized pellet ore. The compressive strength of the finished oxidized pellet ore was determined according to GB / T 14201-93 "Method for Determination of Compressive Strength of Iron Ore Pellets", and the reduction expansion rate was determined according to GB / T 13240-91 "Method for Determination of Relative Free Expansion Index of Iron Ore Pellets".

[0019] Table 3 Chemical composition, compressive strength, and reduction expansion rate of the finished oxide pellets prepared according to each implementation scheme The chemical composition, compressive strength, and reduction expansion rate of the finished oxidized pellets prepared according to each implementation scheme were analyzed, as shown in Table 3. It can be seen that the TFe content of the oxidized pellets prepared according to each implementation scheme is higher than 62.00%. With the addition of Indian iron concentrate, the compressive strength of the finished oxidized pellets shows an increasing trend, while the reduction expansion rate remains basically stable. When the proportion of Indian iron concentrate in the pelletizing raw materials is 2.5%-5%, the compressive strength of the finished oxidized pellets is higher than 2700 N / pellet, and the reduction expansion rate is lower than 20%, which fully meets the requirements of blast furnace ironmaking production.

[0020] This invention prepares oxidized pellets by rationally combining Indian iron concentrate and Bayan Obo iron concentrate. The produced oxidized pellets have a TFe content greater than 62.00%, a compressive strength greater than 2700 N / pellet, and a reduction expansion rate less than 20%, meeting the quality indicators of pellets. This invention effectively solves the problem of high reduction expansion rate when Bayan Obo iron concentrate is used alone to prepare oxidized pellets, and realizes the large-scale application of Bayan Obo iron concentrate in the pellet production process.

[0021] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.

Claims

1. A method for improving the performance of oxidized pellets mainly based on Baiyunebo iron ore concentrate by using Indian iron ore concentrate, characterized in that: According to the mass percentage, firstly, 95-100% of Bayan Obo iron concentrate, 0%-5% of Indian iron concentrate, and 2.5% of bentonite are mixed evenly. Then, the pelletizing process is carried out on a disc pelletizer. After a certain period of time, green pellets are obtained. Green pellets of 10-16mm are screened out. The green pellets are further dried, preheated, and roasted to obtain the finished pellet ore. The drying conditions for green pellets include: a temperature of 130–150℃ and a time of 40–60 min; the preheating conditions include: a temperature of 600–800℃ and a time of 10–15 min; and the calcination conditions include: a temperature of 1200–1250℃ and a time of 15–30 min.

2. A process of using Indian iron ore fines to improve the performance of oxidized pellets mainly of Bayan Obo iron ore concentrate according to claim 1, characterized in that: The chemical composition of the Bayan Obo iron concentrate, by mass percentage, includes 64.00–68.00% TFe, 26.00–30.00% FeO, 0.50–2.00% CaO, 1.50–4.50% SiO2, 0.20–1.00% MgO, 0.10–1.00% Al2O3, 0.05–0.25% K2O, 0.10–0.30% Na2O, 0.20–0.40% F, and 0.30–0.90% S, with 75–95% of the iron concentrate having a particle size less than 0.074 mm.

3. The method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate according to claim 1, characterized in that: The Indian iron concentrate contains 51.00–55.00% TFe, 1.00–3.00% FeO, 0.10–0.20% CaO, 14.0–15.00% SiO2, 0.13–0.15% MgO, 5.10–6.20% Al2O3, and 0.20–0.30% TiO2.

4. The method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate according to claim 1, characterized in that: The bentonite binder comprises, by mass percentage: 1.30–3.50% CaO, 60.00–69.00% SiO2, 1.50–4.00% MgO, 12.00–16.00% Al2O3, 1.00–3.00% K2O, and 1.00–3.00% Na2O, with bentonite particles smaller than 0.074 mm accounting for more than 98%.

5. The method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate according to claim 2, characterized in that: The chemical composition of the Bayan Obo iron concentrate, by mass percentage, includes: 66.80% TFe, 28.90% FeO, 0.76% CaO, 2.52% SiO2, 0.56% MgO, 0.48% Al2O3, 0.13% K2O, 0.15% Na2O, 0.32% F, and 0.74% S. The proportion of iron concentrate particles smaller than 0.074 mm is 85%.

6. The method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate according to claim 3, characterized in that: The chemical composition of the Indian iron concentrate, by mass percentage, includes: 51.24% TFe, 1.93% FeO, 0.092% CaO, 14.15% SiO2, 0.136% MgO, 5.78% Al2O3, 0.125% K2O, 0.073% Na2O, 0.050% F, and 0.034% S.

7. The method for improving the performance of oxide pellets mainly composed of Bayan Obo iron concentrate using Indian iron concentrate according to claim 4, characterized in that: The bentonite binder comprises, by mass percentage: 1.30–3.50% CaO, 60.00–69.00% SiO2, 1.50–4.00% MgO, 12.00–16.00% Al2O3, 1.00–3.00% K2O, and 1.00–3.00% Na2O, with bentonite particles smaller than 0.074 mm accounting for more than 98%.