A high-nitrogen titanium-aluminum alloy and its preparation method
By directly introducing nitrogen gas during the preparation stage of low-valent titanium chloride and combining it with magnesium thermal reduction and vacuum distillation purification, the problems of low nitrogen content and uneven distribution in titanium-aluminum alloys were solved, and high-nitrogen titanium-aluminum alloys were prepared, which significantly improved the toughness and mechanical properties of the material and made it suitable for industrial applications.
Patent Information
- Application Number
- CN202611387255.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing methods for increasing nitrogen content in titanium-aluminum alloys suffer from low nitrogen content, uneven nitrogen distribution, long nitriding cycles, and limited overall toughness improvement, making it difficult to achieve the preparation of titanium-aluminum alloys with high and uniform nitrogen content.
Nitrogen gas is directly introduced into the low-valent titanium chloride preparation stage for nitridation, combined with magnesothermic reduction and vacuum distillation purification. Nitrogen-containing low-valent titanium chloride is generated in situ in the low-valent titanium chloride slurry, followed by magnesothermic reduction and vacuum distillation purification to obtain a titanium-aluminum alloy with uniform nitrogen distribution.
A titanium-aluminum alloy with high and uniform nitrogen content was achieved, which significantly improved the toughness and comprehensive mechanical properties of the material. The process is highly controllable and suitable for industrial production.
Smart Images

Figure CN123108294A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of titanium alloy material preparation technology, and specifically relates to a method for preparing a high-nitrogen titanium-aluminum alloy and the high-nitrogen titanium-aluminum alloy prepared by the method. Background Technology
[0002] Titanium-aluminum alloys (TiAl) possess excellent properties such as low density, high specific strength, good high-temperature oxidation resistance, and corrosion resistance, making them promising for applications in aerospace, automotive, and energy fields. However, room-temperature brittleness and low toughness are major bottlenecks limiting the large-scale application of TiAl alloys. Nitriding is one of the important ways to improve the mechanical properties of TiAl alloys. The introduction of nitrogen can form nitride phases or solid solutions such as TiN, TiAlN, and Ti2AlN, which play a role in grain refinement, second-phase strengthening, and solid solution strengthening, thereby significantly improving the hardness, strength, and high-temperature performance of TiAl alloys.
[0003] In existing technologies, nitrogen enrichment of titanium-aluminum alloys mainly employs vapor-phase nitriding. For example, US Patent 5,152,960 discloses a titanium-aluminum intermetallic compound in which nitrogen exists in a solid solution state and its preparation method. First, metallic titanium is heated in a nitrogen atmosphere at 800°C to the melting point of titanium, allowing nitrogen to dissolve into the titanium. Then, aluminum is added in a vacuum or inert atmosphere for alloying, yielding a titanium-aluminum intermetallic compound with a nitrogen content of 0.2wt% to 1.0wt%. However, this type of vapor-phase nitrogen enrichment method requires long-term nitriding at high temperatures (≥800°C), resulting in a narrow control range for nitrogen content. When the nitrogen content exceeds 1.0wt%, the plasticity deteriorates significantly. Furthermore, nitrogen diffuses inward from the surface, leading to insufficient nitrogen enrichment in the core, making it difficult to achieve uniform nitrogen enrichment of the entire titanium-aluminum alloy. The problems of a thin nitrided layer and low nitrogen content in the core are prominent.
[0004] In addition, some studies have employed powder metallurgy methods for nitrogen enrichment. For example, Chinese patent CN102418000B discloses a method for preparing a TiAl-based composite material with a three-dimensional network distribution of Ti2AlN particles. This method involves nitriding titanium powder in flowing nitrogen at 500–600°C for 12–48 hours to obtain nitrided titanium powder, which is then mixed with aluminum powder and hot-pressed and sintered in situ to generate the Ti2AlN reinforcing phase. However, this method has a long nitriding cycle, nitriding only occurs on the surface of the powder, and is limited by the powder particle size and nitriding depth. The nitrogen content and distribution uniformity are difficult to control precisely, and the interfacial bonding strength between the nitrided titanium powder and the aluminum powder is limited, affecting the overall performance of the composite material.
[0005] In the field of titanium metallurgy, low-valent titanium chloride (titanium trichloride and / or titanium dichloride) is an important intermediate product in the preparation of metallic titanium by electrolysis and magnesothermic reduction. Chinese patent CN103882476B discloses an electrolyte containing low-valent titanium chloride and a method for preparing metallic titanium. This method involves reacting a mixture of metallic magnesium powder and liquid titanium tetrachloride in molten salt under a non-oxidizing atmosphere to prepare low-valent titanium chloride. However, this method uses molten salt as the reaction medium and the target product as the electrolyte for electrolytic preparation of metallic titanium, without introducing nitrogen throughout the process, and does not provide any technical guidance on in-situ nitrogen addition during the preparation of low-valent titanium chloride. Other studies have explored directly introducing nitrogen gas during the smelting of titanium-aluminum alloys for nitrogen addition. However, due to the limited solubility of nitrogen in the titanium-aluminum melt and the tendency of nitrogen gas to form pores and other defects in the melt, it is difficult to obtain titanium-aluminum alloys with high and uniform nitrogen content.
[0006] Therefore, developing a method for preparing titanium-aluminum alloys that can achieve high nitrogen content, uniform distribution, and controllable process is of great significance for improving the comprehensive performance of titanium-aluminum alloys and expanding their application fields. Summary of the Invention
[0007] The technical problem to be solved by the present invention is to overcome the defects of nitrogen addition in the prior art of titanium-aluminum alloys, such as low nitrogen content, uneven distribution, long nitriding cycle and limited improvement in overall toughness. The present invention provides a high-nitrogen titanium-aluminum alloy and its preparation method that directly adds nitrogen from the source of low-cost titanium chloride. The method can obtain titanium-aluminum alloy products with high nitrogen content and uniform nitrogen distribution, and significantly improve the toughness and comprehensive mechanical properties of the material.
[0008] To solve at least one of the above-mentioned technical problems, the present invention adopts the following technical solution: According to one aspect of the present invention, a method for preparing a high-nitrogen titanium-aluminum alloy is provided, comprising the following steps: S10, preparation of nitrogen-containing low-valent titanium chloride slurry: aluminum powder, aluminum trichloride and titanium tetrachloride are stirred and mixed and heated, nitrogen gas is introduced into the mixture, and the reaction is carried out at a temperature of 80~136°C to obtain a nitrogen-containing low-valent titanium chloride slurry; S20, magnesothermic reduction: the nitrogen-containing low-valent titanium chloride slurry obtained in step S10 is introduced into molten metallic magnesium, and a reduction reaction is carried out under argon protection at a reaction temperature of 660~900°C. After complete reduction, a nitrogen-containing titanium-aluminum alloy reduction product is obtained; S30, vacuum distillation purification: the reduction product obtained in step S20 is placed in a vacuum distillation furnace to separate and remove the reduction byproduct magnesium chloride and excess metallic magnesium. The distillation temperature is 700~1200°C, and the vacuum degree is ≤0.1Pa to obtain a high-nitrogen titanium-aluminum alloy product.
[0009] According to one embodiment of the present invention, in step S10, the liquid-solid mass ratio is controlled to be 100:(8~50), and the mass ratio of aluminum powder to aluminum trichloride is 100:(5~50).
[0010] According to one embodiment of the present invention, in step S10, the nitrogen flow rate is 1~4 L / min, and the heat preservation reaction time is 3~6 hours.
[0011] According to one embodiment of the present invention, in step S10, the stirring speed is 250~350 rpm.
[0012] According to one embodiment of the present invention, in step S20, the mass ratio of titanium tetrachloride to molten magnesium metal is 100:(40~85), and the nitrogen-containing low-valent titanium chloride slurry is continuously fed into the molten magnesium metal at a rate of 80~150 mL / min.
[0013] According to one embodiment of the present invention, in step S20, after the reduction reaction is completed, the product is naturally cooled to room temperature to obtain a nitrogen-containing titanium-aluminum alloy reduction product.
[0014] According to one embodiment of the present invention, in step S30, the distilled product is crushed and sieved to obtain nitrogen-containing titanium-aluminum alloy powder.
[0015] According to one embodiment of the present invention, the nitrogen gas is high-purity nitrogen gas with a purity of ≥99.999%.
[0016] According to another aspect of the present invention, a high-nitrogen titanium-aluminum alloy prepared by any of the above-described embodiments is provided, wherein the high-nitrogen titanium-aluminum alloy has a nitrogen content of 0.3wt% to 4wt%, an aluminum content of 5wt% to 45wt%, and the balance is titanium and unavoidable impurities.
[0017] According to one embodiment of the present invention, nitrogen is uniformly distributed in the high-nitrogen titanium-aluminum alloy, and the relative deviation of nitrogen content is ≤5%.
[0018] By adopting the above technical solution, the present invention has at least one of the following advantages compared with the prior art: (1) High nitrogen content and uniform distribution: This invention directly increases nitrogen from the source of low-cost titanium chloride preparation, and achieves atomic-level uniform nitriding in the chloride system. Nitrogen is uniformly distributed in the final product, and the relative deviation of nitrogen content is ≤5%, which is far superior to traditional surface nitriding or powder mixing methods. (2) Significantly improved mechanical properties: The uniform distribution of nitrogen can give full play to the synergistic effect of fine grain strengthening, solid solution strengthening and second phase strengthening, which can increase the room temperature compressive strength of titanium-aluminum alloy by more than 20%, increase the plasticity by more than 15%, and significantly improve the toughness of the material. (3) Good process controllability: By controlling parameters such as liquid-solid mass ratio, aluminum powder to aluminum trichloride ratio, reaction temperature, and nitrogen flow rate, the present invention can accurately control the nitrogen and aluminum content of the product to meet the needs of different application scenarios. (4) Short preparation cycle and simple process: Compared with traditional gas phase nitriding which requires high temperature and long time treatment and powder metallurgy nitriding which requires 12 to 48 hours, the present invention can complete the preparation of slurry and in-situ nitrogen addition at low temperature and normal pressure of 80 to 136℃. The process is short and energy consumption is low, making it suitable for industrial production. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0020] Figure 1 This is a schematic diagram of the process flow for preparing a high-nitrogen titanium-aluminum alloy according to an embodiment of the present invention. Detailed Implementation
[0021] To make the objectives, technical solutions, and advantages of the present invention clearer, the embodiments of the present invention will be further described in detail below with reference to specific examples and the accompanying drawings.
[0022] It should be understood that the embodiments of the invention shown in the exemplary embodiments are merely illustrative. Although only a few embodiments have been described in detail in this invention, those skilled in the art will readily recognize that various modifications are possible without substantially departing from the teachings of the invention. Accordingly, all such modifications should be included within the scope of the invention. Other substitutions, modifications, variations, and deletions can be made to the design, operating conditions, and parameters of the following exemplary embodiments without departing from the spirit of the invention.
[0023] According to one aspect of the present invention, a method for preparing a high-nitrogen titanium-aluminum alloy is provided. Nitrogen gas is directly introduced during the preparation stage of low-valent titanium chloride for nitridation. The active low-valent titanium ions generated during the reduction of titanium tetrachloride by aluminum powder react with the nitrogen gas, achieving direct nitrogen enrichment from the source. Compared with traditional surface nitriding or powder mixing methods, the present invention achieves uniform nitrogen introduction in an atomic-level chloride system, resulting in a nitrogen-containing low-valent titanium chloride precursor with high and uniform nitrogen content. Subsequently, the nitrogen-containing low-valent titanium chloride is reduced to a nitrogen-containing titanium-aluminum alloy via magnesothermal reduction, and then purified by vacuum distillation to obtain the final product. The nitrogen element in the nitrogen-containing titanium-aluminum alloy prepared by this method is uniformly distributed, fully utilizing the strengthening effect of nitrogen and significantly improving the toughness and comprehensive mechanical properties of the titanium-aluminum alloy.
[0024] like Figure 1 As shown, a method for preparing a high-nitrogen titanium-aluminum alloy according to an embodiment of the present invention includes the following steps: S10, Preparation of nitrogen-containing low-valent titanium chloride slurry: Aluminum powder, aluminum trichloride and titanium tetrachloride are stirred and mixed and heated, the liquid-solid mass ratio is controlled at 100:(8~50), the mass ratio of aluminum powder to aluminum trichloride is 100:(5~50), nitrogen gas is introduced into the mixture, and the mixture is fully reacted at a temperature of 80~136℃ to obtain nitrogen-containing low-valent titanium chloride slurry; S20, Magnesium reduction: The nitrogen-containing low-valent titanium chloride slurry obtained in step S10 is passed into molten magnesium metal and a reduction reaction is carried out under argon protection. The reaction temperature is 660~900℃. After complete reduction, a nitrogen-containing titanium aluminum alloy reduction product is obtained. S30, Vacuum distillation purification: The reduction product obtained in step S20 is placed in a vacuum distillation furnace to separate and remove the reduction byproduct magnesium chloride and excess metallic magnesium. The distillation temperature is 700~1200℃ and the vacuum degree is ≤0.1Pa to obtain a high-nitrogen titanium-aluminum alloy product.
[0025] In an embodiment of the present invention, step S10 requires controlling the liquid-to-solid mass ratio to be 100:(8~50) and the mass ratio of aluminum powder to aluminum trichloride to be 100:(5~50) to ensure that the aluminum powder and aluminum trichloride solid phases are uniformly dispersed in the titanium tetrachloride liquid phase of the reaction medium, so that the slurry has a suitable viscosity, ensuring both sufficient contact of the reactants and good stirring and mass transfer effects. Preferably, the liquid-to-solid mass ratio can be controlled to be 100:(11~45) and the mass ratio of aluminum powder to aluminum trichloride to be 100:(15~30). The reaction temperature can be maintained at 100~135℃, the nitrogen flow rate is 1~4L / min, the heat preservation reaction time is 3~6 hours, and the stirring speed is 250~350rpm; the nitrogen is high-purity nitrogen with a purity ≥99.999%.
[0026] In embodiments of the present invention, the reaction temperature of the magnesium thermal reduction in step S20 is preferably 750~850℃, so that the metallic magnesium is completely melted into a liquid state, exhibiting optimal reducing activity and fluidity. The mass ratio of titanium tetrachloride to molten metallic magnesium is preferably 100:(40~85), and the nitrogen-containing low-valent titanium chloride slurry is preferably continuously fed into the molten metallic magnesium at a rate of 80~150mL / min. After the reduction reaction is completed, the mixture is naturally cooled to room temperature to obtain the nitrogen-containing titanium-aluminum alloy reduction product.
[0027] In embodiments of the present invention, the distillation temperature in step S30 is preferably 950~1050℃, and the vacuum degree is 0.02~0.04Pa. The boiling point of magnesium chloride decreases significantly under vacuum conditions. The above-mentioned distillation temperature combined with the vacuum degree range allows magnesium chloride to fully evaporate and sublimate, while excess metallic magnesium also evaporates under these conditions. Meanwhile, the titanium-aluminum alloy remains solid within this temperature range, facilitating selective separation and purification. The distilled product is crushed and sieved to obtain nitrogen-containing titanium-aluminum alloy powder.
[0028] According to another aspect of the present invention, a high-nitrogen titanium-aluminum alloy prepared by the above preparation method is also provided, wherein the nitrogen content in the high-nitrogen titanium-aluminum alloy is 0.3wt%~4wt%, the aluminum content is 5wt%~45wt%, and the balance is titanium and unavoidable impurities, and the nitrogen element in the high-nitrogen titanium-aluminum alloy is uniformly distributed, and the relative deviation of the nitrogen content is ≤5%.
[0029] The following are specific embodiments and process parameters of the preparation method of high-nitrogen titanium-aluminum alloy according to the present invention.
[0030] Example 1 This embodiment provides a method for preparing a high-nitrogen titanium-aluminum alloy, including the following steps: S10, Preparation of Nitrogen-Containing Low-Valence Titanium Chloride Slurry: In a reactor equipped with a stirrer and a venting device, add 1000g of liquid titanium tetrachloride, then add 200g of aluminum powder and 40g of aluminum trichloride, controlling the liquid-to-solid mass ratio at 100:24 and the aluminum powder to aluminum trichloride mass ratio at 100:20. Start stirring at 300rpm, heat to 120℃, then introduce high-purity nitrogen gas (purity ≥99.999%) at a flow rate of 2L / min, and maintain the reaction temperature for 4 hours.
[0031] After the reaction was completed, a nitrogen-containing low-valent titanium chloride slurry was obtained. Analysis showed that the nitrogen content in the slurry was 2.1 wt%, and the low-valent titanium chloride was mainly titanium trichloride.
[0032] S20, Magnesium thermal reduction: In an argon-protected reduction furnace, 600g of metallic magnesium is added and heated to 800℃ to completely melt the magnesium. The nitrogen-containing low-valent titanium chloride slurry prepared in step S10 is continuously fed into the molten magnesium at a rate of 100mL / min, with stirring maintained at 200rpm during the feeding process. After the feeding is complete, the reaction is continued at 800℃ for 5 hours to ensure the reduction reaction proceeds fully.
[0033] After the reaction was completed, the mixture was naturally cooled to room temperature to obtain the nitrogen-containing titanium-aluminum alloy reduction product.
[0034] S30, Vacuum Distillation Purification: The reduction product obtained in step S20 is crushed and placed in a vacuum distillation furnace for vacuum distillation. The distillation temperature is 1000℃, the vacuum degree is 0.03Pa, and the distillation time is 10 hours. During the distillation process, magnesium chloride and excess metallic magnesium evaporate and are collected in the condensation zone. After distillation, the furnace is cooled to room temperature, and the distillation product is taken out, crushed, and sieved to obtain nitrogen-containing titanium-aluminum alloy powder with a mesh size of less than 100 mesh.
[0035] Testing revealed that the nitrogen-containing titanium-aluminum alloy prepared in this embodiment contained 1.8 wt% nitrogen and 32 wt% aluminum, with the remainder being titanium and unavoidable impurities. X-ray diffraction analysis showed that the product contained a TiAl matrix phase, a TiAlN phase, and a small amount of Ti2AlN MAX phase. Scanning electron microscopy and elemental surface distribution analysis showed that nitrogen was uniformly distributed in the alloy, with a relative deviation of 3.2% in nitrogen content.
[0036] Mechanical property tests show that the nitrogen-containing titanium-aluminum alloy prepared in this embodiment has a room temperature compressive strength of 1850 MPa and a compression ratio of 28.5%. Compared with the nitrogen-free titanium-aluminum alloy, the compressive strength is increased by 26.7% and the compression ratio is increased by 22.8%, demonstrating excellent strength and toughness matching.
[0037] Example 2 This embodiment provides a method for preparing a high-nitrogen titanium-aluminum alloy, including the following steps: S10, Preparation of Nitrogen-Containing Low-Valence Titanium Chloride Slurry: In a reactor equipped with a stirrer and a venting device, add 1000g of liquid titanium tetrachloride, then add 100g of aluminum powder and 15g of aluminum trichloride, controlling the liquid-to-solid mass ratio at 100:11.5 and the aluminum powder to aluminum trichloride mass ratio at 100:15. Start stirring at 250rpm, heat to 100℃, then introduce high-purity nitrogen gas at a flow rate of 1L / min, and maintain the reaction temperature for 6 hours.
[0038] After the reaction was completed, a nitrogen-containing low-valent titanium chloride slurry was obtained. Testing revealed that the nitrogen content in the slurry was 1.2 wt%.
[0039] S20, Magnesium thermal reduction: In an argon-protected reduction furnace, 450g of metallic magnesium is added and heated to 750℃ until the magnesium is completely melted. The nitrogen-containing low-valent titanium chloride slurry prepared in step S10 is continuously fed into the molten magnesium at a rate of 80mL / min. After the feeding is complete, the reaction is continued at 750℃ for 8 hours.
[0040] After the reaction was completed, the mixture was naturally cooled to room temperature to obtain the nitrogen-containing titanium-aluminum alloy reduction product.
[0041] S30, Vacuum distillation purification: The reduction product obtained in step S20 is crushed and placed in a vacuum distillation furnace. The distillation temperature is 950℃, the vacuum degree is 0.04Pa, and the distillation time is 12 hours. After distillation, the product is cooled to room temperature in the furnace, and then the distillation product is taken out, crushed, and sieved to obtain nitrogen-containing titanium-aluminum alloy powder.
[0042] Testing revealed that the nitrogen-containing titanium-aluminum alloy prepared in this embodiment contained 1.0 wt% nitrogen, 25 wt% aluminum, with the remainder being titanium and unavoidable impurities. Nitrogen was uniformly distributed, with a relative deviation of 4.1%. The room temperature compressive strength was 1680 MPa, and the compression ratio was 26.8%. Compared to the nitrogen-free titanium-aluminum alloy, the compressive strength increased by 21.7%, and the compression ratio increased by 17.5%.
[0043] Example 3 This embodiment provides a method for preparing a high-nitrogen titanium-aluminum alloy, including the following steps: S10, Preparation of Nitrogen-Containing Low-Valence Titanium Chloride Slurry: In a reactor equipped with a stirrer and a venting device, 1000g of liquid titanium tetrachloride was added, followed by 350g of aluminum powder and 105g of aluminum trichloride, controlling the liquid-to-solid mass ratio at 100:45.5 and the aluminum powder to aluminum trichloride mass ratio at 100:30. Stirring was started at 350rpm, and the temperature was raised to 135℃. High-purity nitrogen gas was then introduced at a flow rate of 4L / min, and the reaction was maintained at this temperature for 3 hours. After the reaction, a nitrogen-containing low-valence titanium chloride slurry was obtained. The nitrogen content in the slurry was measured to be 3.5wt%.
[0044] S20, Magnesium thermal reduction: In an argon-protected reduction furnace, 800g of metallic magnesium was added and heated to 850℃ until the magnesium was completely melted. The nitrogen-containing low-valent titanium chloride slurry prepared in step S10 was continuously fed into the molten magnesium at a rate of 150mL / min. After the feeding was complete, the reaction was continued at 850℃ for 4 hours. After the reaction was completed, the mixture was naturally cooled to room temperature to obtain the nitrogen-containing titanium-aluminum alloy reduction product.
[0045] S30, Vacuum distillation purification: The reduction product obtained in step S20 is crushed and placed in a vacuum distillation furnace. The distillation temperature is 1050℃, the vacuum degree is 0.02Pa, and the distillation time is 8 hours. After distillation, the product is cooled to room temperature in the furnace, and then the distillation product is taken out, crushed, and sieved to obtain nitrogen-containing titanium-aluminum alloy powder.
[0046] Testing revealed that the nitrogen-containing titanium-aluminum alloy prepared in this embodiment contained 3.1 wt% nitrogen and 42 wt% aluminum, with the remainder being titanium and unavoidable impurities. X-ray diffraction analysis showed high contents of TiAlN and Ti2AlN MAX phases. Nitrogen was uniformly distributed, with a relative deviation of 3.8%. The room temperature compressive strength was 2100 MPa, and the compression ratio was 25.2%. Compared with the nitrogen-free titanium-aluminum alloy, the compressive strength was increased by 43.8%, and the compression ratio was increased by 10.5%.
[0047] Comparative Example 1 This comparative example uses a traditional powder metallurgy method to prepare nitrogen-containing titanium-aluminum alloys by mixing titanium nitride. Titanium powder, aluminum powder, and TiN powder are mixed in a certain proportion, with the amount of TiN powder added being 5 wt%. The mixture is then ball-milled under argon protection, and finally sintered by vacuum hot pressing to prepare the titanium-aluminum alloy.
[0048] Testing revealed that the nitrogen content in the titanium-aluminum alloy prepared in this comparative example was approximately 1.2 wt%, but the nitrogen distribution was uneven, exhibiting significant TiN particle agglomeration, with a relative deviation in nitrogen content as high as 28.5%. The room temperature compressive strength was 1580 MPa, and the compression ratio was 21.5%. Compared to the example, although the nitrogen content was similar, the improvement in mechanical properties was significantly worse due to the uneven distribution.
[0049] Comparative Example 2 In this comparative example, a gas nitriding method was used to nitrid the surface of the titanium-aluminum alloy. The titanium-aluminum alloy sample was nitrided at 1000℃ for 10 hours in a nitrogen atmosphere.
[0050] Testing revealed that the titanium-aluminum alloy prepared in this comparative example had a surface nitriding layer thickness of approximately 80 μm and a surface nitrogen content of approximately 2.5 wt%, but a core nitrogen content of less than 0.1 wt%, with an overall average nitrogen content of approximately 0.3 wt%. Due to the limited surface nitriding, the overall toughness improvement of the material was limited.
[0051] Regarding nitrogen content and distribution uniformity, the high-nitrogen titanium-aluminum alloys prepared in Examples 1-3 of this invention have a nitrogen content of 1.0-3.1 wt%, with a relative deviation of only 3.2%-4.1%. Comparative Example 1, using a powder metallurgy method to mix TiN powder, achieved a nitrogen content of 1.2 wt%, but the relative deviation was as high as 28.5%, indicating significant TiN particle agglomeration. Comparative Example 2, employing gas nitriding surface treatment, achieved an overall average nitrogen content of only about 0.3 wt%, a surface nitriding layer thickness of about 80 μm, and a core nitrogen content of less than 0.1 wt%. It is evident that this invention directly increases nitrogen from the source of low-valent titanium chloride preparation, achieving uniform introduction of nitrogen into the atomic-level chloride system. Its nitrogen content and distribution uniformity are significantly superior to traditional surface nitriding and powder mixing methods.
[0052] Regarding mechanical properties, the room temperature compressive strength of Examples 1-3 of this invention is 1680-2100 MPa, and the compression ratio is 25.2%-28.5%. Compared with nitrogen-free titanium-aluminum alloys, the compressive strength is increased by more than 20%, and the compression ratio is increased by more than 10%. Although the nitrogen content of Comparative Example 1 is similar to that of Example 2, due to the uneven distribution of nitrogen, the room temperature compressive strength is only 1580 MPa, and the compression ratio is only 21.5%, resulting in significantly poorer mechanical properties. This invention, through the uniform distribution of nitrogen, can fully utilize the synergistic effects of fine grain strengthening, solid solution strengthening, and second-phase strengthening, avoiding stress concentration in local nitrogen-rich and nitrogen-poor regions, thereby achieving a good match between high strength and high plasticity.
[0053] In summary, this invention achieves a high-nitrogen titanium-aluminum alloy with high nitrogen content, uniform nitrogen distribution, and excellent comprehensive mechanical properties by in-situ nitrogen addition during the preparation of low-valent titanium chloride, combined with magnesothermic reduction and vacuum distillation purification. Furthermore, the process is short and parameters are highly controllable, demonstrating significant industrial application value. The high-nitrogen titanium-aluminum alloy prepared by this invention can be used as a raw material for TiAlN coatings, Ti2AlN / Ti3AlN MAX phases, and nitrided reinforced TiAl composites, and is widely applied in high-temperature structural components such as cutting tools and molds, aero-engines, and automotive turbochargers. It can also be used in emerging fields such as energy storage, catalysis, and sensing, possessing significant industrial application value and broad market prospects.
[0054] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Any modifications or equivalent substitutions made to the present invention without departing from the spirit and scope thereof should be covered within the protection scope of the claims of the present invention.
[0055] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the disclosed embodiments of the present invention is limited to these examples; within the framework of the embodiments of the present invention, the technical features of the above embodiments or different embodiments can also be combined, and there are many other variations of different aspects of the embodiments of the present invention as described above, which are not provided in detail for the sake of brevity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the embodiments of the present invention should be included within the protection scope of the embodiments of the present invention.
Claims
1. A method for preparing a high-nitrogen titanium-aluminum alloy, characterized in that, Includes the following steps: S10, Preparation of nitrogen-containing low-valent titanium chloride slurry: Aluminum powder, aluminum trichloride and titanium tetrachloride are stirred and mixed and heated. Nitrogen gas is introduced into the mixture and the mixture is fully reacted at a temperature of 80~136℃ to obtain nitrogen-containing low-valent titanium chloride slurry; S20, Magnesium reduction: The nitrogen-containing low-valent titanium chloride slurry obtained in step S10 is passed into molten magnesium metal and a reduction reaction is carried out under argon protection. The reaction temperature is 660~900℃. After complete reduction, a nitrogen-containing titanium aluminum alloy reduction product is obtained. S30, Vacuum distillation purification: The reduction product obtained in step S20 is placed in a vacuum distillation furnace to separate and remove the reduction byproduct magnesium chloride and excess metallic magnesium. The distillation temperature is 700~1200℃ and the vacuum degree is ≤0.1Pa to obtain a high-nitrogen titanium-aluminum alloy product.
2. The preparation method according to claim 1, characterized in that, In step S10, the liquid-solid mass ratio is controlled to be 100:(8~50), and the mass ratio of aluminum powder to aluminum trichloride is 100:(5~50).
3. The preparation method according to claim 1, characterized in that, In step S10, the nitrogen flow rate is 1~4 L / min, and the reaction time is 3~6 hours.
4. The preparation method according to claim 1, characterized in that, In step S10, the stirring speed is 250~350 rpm.
5. The preparation method according to claim 1, characterized in that, In step S20, the mass ratio of titanium tetrachloride to molten magnesium metal is 100:(40~85), and the nitrogen-containing low-valent titanium chloride slurry is continuously fed into the molten magnesium metal at a rate of 80~150 mL / min.
6. The preparation method according to claim 1, characterized in that, In step S20, after the reduction reaction is completed, the mixture is naturally cooled to room temperature to obtain the nitrogen-containing titanium-aluminum alloy reduction product.
7. The preparation method according to claim 1, characterized in that, In step S30, the distilled product is crushed and sieved to obtain nitrogen-containing titanium-aluminum alloy powder.
8. The preparation method according to claim 1, characterized in that, The nitrogen gas is high-purity nitrogen with a purity of ≥99.999%.
9. A high-nitrogen titanium-aluminum alloy prepared by the preparation method according to any one of claims 1 to 8, characterized in that, The high-nitrogen titanium-aluminum alloy contains 0.3wt% to 4wt% nitrogen, 5wt% to 45wt% aluminum, and the balance is titanium and unavoidable impurities.
10. The high-nitrogen titanium-aluminum alloy according to claim 9, characterized in that, The nitrogen element is uniformly distributed in the high-nitrogen titanium-aluminum alloy, and the relative deviation of nitrogen content is ≤5%.
Citation Information
Patent Citations
Preparation method of three-dimensional network distributed Ti2AlN particle reinforced TiAl-based composite material
CN102418000B
A kind of electrolyte containing low-valent titanium chloride and the preparation method of metal titanium
CN103882476B
Titanium-Aluminum intermetallic having nitrogen in solid solution
US5152960A