A method for low-temperature roasting, detoxification, and lithium extraction from aluminum electrolysis overhaul slag.
By using low-temperature composite roasting aids and a waste heat recovery system, the problem of high-temperature roasting in the treatment of aluminum electrolysis overhaul slag was solved, achieving low-energy consumption, high-efficiency lithium leaching and cyanide detoxification, and improving the efficiency of lithium resource recovery.
Patent Information
- Application Number
- CN202611442607.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-17
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aluminum electrolysis overhaul slag treatment processes involve high roasting temperatures, high energy consumption and carbon emissions, and it is difficult to simultaneously achieve low-temperature cyanide detoxification and conversion of sparingly soluble lithium salts, resulting in low lithium leaching conversion rates.
A low-temperature composite roasting aid (calcium carbonate, aluminum sulfate, and modified diatomaceous earth) is used to roast aluminum electrolysis overhaul slag at 550℃~680℃. Combined with a waste heat recovery system, cyanide detoxification and lithium salt conversion are completed simultaneously, and lithium is extracted by low-concentration acid leaching.
Significantly reduces energy consumption and carbon emissions, increases lithium leaching conversion rate to over 90%, reduces the production of fluorine-containing flue gas and high-fluorine wastewater, and lowers overall operating costs.
Smart Images

Figure CN123108319A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of solid waste resource utilization technology, specifically a method for low-temperature roasting and detoxification of lithium extraction from aluminum electrolysis overhaul slag. Background Technology
[0002] During the electrolytic aluminum production process, electrolytic cells require a major overhaul every 3 to 5 years. After removing the lining material of the electrolytic cells, aluminum electrolysis overhaul slag is generated. This slag is listed in the National Hazardous Waste List, numbered HW48. The slag contains toxic and harmful components such as soluble fluorides and cyanides, as well as valuable elements such as lithium, aluminum, and sodium. The lithium content is 0.1% to 1.5%, which has economic value for large-scale recycling. If the slag is directly stockpiled or landfilled, the fluorine and cyanide components in the slag can easily seep into the soil and groundwater after being leached by rainwater, posing a risk of ecological and environmental pollution.
[0003] Existing technologies for treating aluminum electrolysis overhaul slag generally employ high-temperature pyrometallurgical roasting processes, with roasting temperatures typically ranging from 850℃ to 1000℃. This process results in high fuel consumption, high carbon emissions, and severe corrosion of the rotary kiln lining due to prolonged operation at high temperatures, leading to high maintenance costs. One existing technology, similar to this invention, involves mixing crushed overhaul slag with sulfuric acid for aging, followed by roasting at 200℃ to 1000℃ to obtain clinker. After ball milling, water washing, and lime slurry purification, lithium salts are extracted. However, this method relies on concentrated sulfuric acid as a conversion agent and lacks a dedicated low-temperature roasting aid. The actual roasting temperature is generally higher than 800℃. The roasting and leaching processes are independent, and no waste heat recovery coupling system is implemented, resulting in a lithium leaching conversion rate of less than 70%. Cyanide degradation is incomplete in the low-temperature range, making it difficult to simultaneously achieve the dual goals of hazardous waste harmless treatment and lithium resource recovery. Summary of the Invention
[0004] The technical problem to be solved by this invention is: addressing the issues of high roasting temperature, high energy consumption and carbon emissions in existing aluminum electrolysis overhaul slag treatment processes, difficulty in simultaneously achieving low-temperature cyanide detoxification and conversion of sparingly soluble lithium salts, and low lithium leaching conversion rate. This invention provides a method for low-temperature roasting detoxification and lithium extraction from aluminum electrolysis overhaul slag, enabling simultaneous completion of cyanide detoxification and lithium salt activation conversion at a lower roasting temperature, and reducing overall energy consumption of the process through waste heat recovery coupling.
[0005] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is a method for low-temperature roasting, detoxification, and lithium extraction from aluminum electrolysis overhaul slag, comprising the following steps: The raw material pretreatment step involves sequentially crushing, ball milling, and sieving the aluminum electrolysis overhaul slag to obtain overhaul slag powder with a particle size not exceeding 200 mesh. A low-temperature composite roasting aid is then added to the overhaul slag powder and mixed evenly to obtain a mixture. The low-temperature composite roasting aid includes calcium carbonate, aluminum sulfate, and modified diatomaceous earth, and the amount of the low-temperature composite roasting aid added is 8% to 12% of the mass of the overhaul slag powder. In the low-temperature roasting step, the mixture is fed into a rotary kiln and roasted at a constant temperature of 550℃~680℃ for 1.5~3 hours, while air is introduced into the rotary kiln to obtain roasted clinker. During the roasting process, the waste heat of the flue gas is recovered through a waste heat boiler set at the kiln tail to obtain recovered hot water. The clinker washing step involves cooling the roasted clinker and then adding it to the recycled hot water for stirring and slurry preparation. The liquid-to-solid ratio is 5:1. The mixture is stirred at room temperature for 30 minutes and then filtered to obtain the washed filter residue and washing liquid. In the low-concentration acid leaching step, the water-washed filter residue is added to a sulfuric acid solution for leaching. The concentration of the sulfuric acid solution is 1.2–1.8 mol / L, the leaching temperature is 50°C–65°C, and the leaching time is 90–150 minutes. The heat source for leaching is the residual heat recovered in the low-temperature roasting step. After leaching, the residue is separated by pressure filtration to obtain a lithium-rich leaching solution and leaching residue.
[0006] In the low-temperature roasting step, the low-temperature composite roasting aid undergoes a solid-phase transformation reaction with lithium fluoride and lithium fluoroaluminate in the overhaul slag powder to generate water-soluble lithium sulfate. The cyanide in the overhaul slag powder is oxidized and decomposed into carbon dioxide and nitrogen at temperatures above 550°C. The soluble fluorine in the overhaul slag powder is converted into calcium fluoride and solidified in the roasted clinker, thereby inhibiting the generation of fluorine-containing flue gas.
[0007] Compared with the prior art, the beneficial effects of the present invention by adopting the above technical solution are as follows: First, energy consumption and carbon emissions are significantly reduced. The roasting temperature is reduced from 850℃~1000℃ in the existing technology to 550℃~680℃, reducing fuel consumption by more than 30%. The waste heat from roasting is recovered and used for clinker washing and acid leaching heating. No additional heating is required in the leaching section, and the overall energy consumption is reduced by about 22%. Secondly, cyanide detoxification and lithium salt conversion are completed simultaneously and efficiently. The low-temperature composite roasting aid can completely oxidize and decompose cyanide at temperatures above 550°C, while activating insoluble lithium fluoride and lithium fluoroaluminate to generate water-soluble lithium sulfate. The lithium leaching conversion rate can reach more than 90%, which is more than 20 percentage points higher than the existing wet process (conversion rate is less than 70%). Third, the output of fluorine-containing flue gas and high-fluorine wastewater is reduced. Soluble fluorine is converted into calcium fluoride and solidified in clinker during low-temperature roasting, which inhibits the volatilization of fluorides in flue gas. The clinker washing step removes free fluorine and soluble sodium salts in advance, reducing the consumption of sulfuric acid in the subsequent acid leaching step. Fourth, the process is highly integrated and coupled. The three processes of roasting, washing and acid leaching are coupled and utilized through the waste heat recovery system, which reduces lithium loss caused by multiple material transfers and lowers the overall operating cost. Attached Figure Description
[0008] Figure 1 This is a schematic diagram of the process flow for the low-temperature roasting, detoxification, and lithium extraction method for aluminum electrolysis overhaul slag described in this invention. Detailed Implementation
[0009] The following is in conjunction with the appendix Figure 1 The specific embodiments of the present invention will be further described below. It should be noted that the description of these embodiments is for the purpose of helping to understand the present invention, but does not constitute a limitation of the present invention.
[0010] Furthermore, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0011] I. Overall Process Flow The method described in this invention is carried out in the following order: raw material pretreatment, low-temperature roasting, clinker washing, and low-concentration acid leaching. The heat energy is coupled and utilized between each process through a waste heat recovery system, as detailed below.
[0012] (a) Raw material pretreatment steps After removing iron and refractory impurities from the aluminum electrolysis overhaul slag through manual sorting or magnetic separation, it is fed into a jaw crusher for coarse crushing, then into a ball mill for fine grinding, and finally screened by a vibrating screen to obtain overhaul slag powder with a particle size of no more than 200 mesh. The overhaul slag powder is precisely metered using a screw metering feeder, and a low-temperature composite calcination aid is added to it according to a predetermined mass ratio. The mixture is then mixed evenly by a mixer to obtain a mixture.
[0013] The low-temperature composite roasting aid is composed of three components: calcium carbonate, aluminum sulfate, and modified diatomaceous earth, in a mass ratio of 45–55:25–35:15–25. During roasting, calcium carbonate combines with soluble fluorine in the overhaul slag to form stable calcium fluoride, thus playing a role in fluorine fixation. Under roasting conditions, aluminum sulfate reacts with lithium fluoride and lithium fluoroaluminate in the overhaul slag, promoting the activation and conversion of lithium salts into water-soluble lithium sulfate. Modified diatomaceous earth has a large specific surface area and porous structure, which can improve the heat transfer efficiency of the mixture and reduce the activation energy required for the roasting reaction, thereby enabling the cyanide decomposition and lithium salt conversion reaction to take place at a lower temperature. The amount of the low-temperature composite roasting aid added is 8%–12% of the mass of the overhaul slag powder. If the amount added is too low, the aid will not be effective in activating and converting lithium salts and fixing fluorine; if the amount added is too high, it will increase the raw material cost and the effect of improving the lithium leaching conversion rate will tend to be gradual.
[0014] It is worth noting that while improving the heat transfer efficiency of materials, modified diatomaceous earth can reduce the activation energy required for the reaction of aluminum sulfate with lithium fluoride and lithium fluoroaluminate, so that the reaction can be carried out efficiently in the low temperature range of 550℃. The calcium oxide produced by the decomposition of calcium carbonate preferentially combines with and solidifies free fluorine, thus preventing free fluorine from interfering with the lithium salt conversion reaction; The three components form a synergistic mechanism of "heat transfer enhancement - solid fluoride inhibition of interference - lithium salt activation", which enables cyanide detoxification and lithium salt conversion to be completed simultaneously and efficiently in the range of 550℃ to 680℃, which is far lower than the roasting temperature of the prior art (850℃~1000℃). This synergistic effect is not a simple superposition of the individual functions of the three components, but a non-obvious technical effect that is difficult for those skilled in the art to predict based on the prior art.
[0015] (II) Low-temperature roasting step The mixture is fed into a modified medium-low temperature rotary kiln via a closed conveyor. The roasting temperature is controlled at 550℃~680℃ and roasted at a constant temperature for 1.5~3 hours. During the roasting process, a small amount of air is introduced into the kiln through a blower at the feed end of the rotary kiln to promote the complete oxidation and decomposition of cyanide into carbon dioxide and nitrogen in the presence of oxygen.
[0016] Under the above temperature conditions, aluminum sulfate in the low-temperature composite roasting aid undergoes a solid-phase transformation reaction with lithium fluoride and lithium fluoroaluminate in the overhaul slag to generate water-soluble lithium sulfate. The calcium oxide produced by the decomposition of calcium carbonate combines with the soluble fluorine in the overhaul slag to generate stable calcium fluoride, which is then solidified and retained in the roasted clinker, thereby significantly reducing the amount of fluoride volatilized in the roasting flue gas.
[0017] A waste heat boiler is installed at the tail of the rotary kiln. The high-temperature flue gas generated during the roasting process is introduced into the waste heat boiler for heat exchange to obtain steam and recover hot water. The steam and hot water are then transported through circulation pipelines to the subsequent clinker washing process and low-concentration acid leaching process to heat the washing water and the sulfuric acid solution used for leaching, thus realizing the cascade utilization of the roasting waste heat.
[0018] (III) Washing steps for clinker After the calcined clinker is discharged from the kiln outlet, it is cooled to room temperature by a cooling conveying device and sent to a water washing and stirring tank. The recovered hot water obtained from the aforementioned waste heat recovery is added to the water washing and stirring tank for slurry preparation. The liquid-to-solid ratio is controlled at 5:1. The mixture is stirred at room temperature for 30 minutes to fully dissolve the soluble sodium salts and free fluorine in the calcined clinker into the aqueous phase. After stirring, the mixture is filtered by a plate and frame filter press to obtain water-washed filter residue and water washing liquid.
[0019] The washing solution contains soluble sodium salts and free fluoride. After being concentrated and dried by a mechanical steam recompression device, sodium fluoride solid byproduct is obtained. The condensate generated during the concentration process is recycled for use in the slurry preparation step, realizing closed-loop recycling of water resources. The amount of sulfuric acid required for the subsequent acid leaching step is reduced accordingly after the water washing pre-removal of free fluoride and soluble sodium salts.
[0020] (iv) Low-concentration acid leaching step The washed filter residue is fed into a closed leaching reactor, and sulfuric acid solution is added for leaching. The concentration of the sulfuric acid solution is controlled at 1.2-1.8 mol / L, the leaching temperature is 50℃-65℃, and the leaching is carried out with stirring for 90-150 minutes. The outer wall of the leaching reactor is equipped with a heat-insulating jacket, and hot water provided by the aforementioned waste heat recovery system is circulated into the heat-insulating jacket as the heat source required for the leaching reaction. No additional steam heating device is required. After leaching, the residue is separated by pressure filtration to obtain lithium-rich leachate and leaching residue. The obtained lithium-rich leachate can be further processed into lithium carbonate products using conventional carbonate precipitation methods in the field. After the leaching residue is tested and found to meet the standards for fluorine, cyanide, sodium, and other indicators, it can be used as a building material raw material or cement aggregate.
[0021] II. Description of Supporting Equipment Modification To adapt to the aforementioned low-temperature roasting and low-concentration acid leaching process conditions, the existing rotary kiln and leaching equipment are modified as follows: The rotary kiln lining is made of 2205 stainless steel to adapt to long-term stable operation under conditions of 550℃~680℃ and improve corrosion resistance. Material lifting plates are installed along the axial direction on the inner wall of the rotary kiln, which drive the mixed materials to scatter during the rotation of the kiln, increasing the contact area between the materials and the air in the kiln, which is conducive to the full oxidation and decomposition of cyanide and the uniform heating of the materials. A waste heat boiler is installed at the kiln tail of the rotary kiln and connected to the heat-using equipment of the clinker washing process and the low-concentration acid leaching process through circulation pipelines. The leaching reactor is equipped with an insulation jacket and is linked to the waste heat recovery system for temperature control. An automatic metering and feeding device is installed throughout the process to accurately control the dosage of low-temperature composite roasting aids and sulfuric acid solution.
[0022] III. Examples Example 1
[0023] Pretreated overhaul slag powder was taken, and a low-temperature composite roasting aid was added at a ratio of 10% of the powder mass. The mass ratio of calcium carbonate, aluminum sulfate, and modified diatomaceous earth in the aid was 50:30:20. After being mixed evenly, the mixture was fed into a rotary kiln and roasted at 620℃ for 2 hours. A small amount of air was introduced during the roasting process. After the roasted clinker cooled, recycled hot water was added at a liquid-to-solid ratio of 5:1 to adjust the slurry. After stirring at room temperature for 30 minutes, the mixture was filtered. The washed filter residue was sent to a leaching reactor, and a sulfuric acid solution with a concentration of 1.6 mol / L was added. The leaching temperature was 60℃, and the mixture was stirred and leached for 120 minutes. The lithium-rich leachate was obtained by pressure filtration. The lithium leaching conversion rate in this embodiment was 92.3%, and no cyanide was detected in the leaching residue. The decyanation rate reached 100%.
[0024] Example 2
[0025] Pretreated overhaul slag powder was taken, and a low-temperature composite roasting aid was added at a ratio of 8% of the powder mass. The mass ratio of calcium carbonate, aluminum sulfate, and modified diatomaceous earth in the aid was 55:25:20. After being mixed evenly, the mixture was fed into a rotary kiln and roasted at 550°C for 3 hours. The subsequent water washing and acid leaching steps were the same as in Example 1, with a sulfuric acid solution concentration of 1.2 mol / L, a leaching temperature of 50°C, and a leaching time of 150 minutes. The lithium leaching conversion rate in this example was 90.1%, and cyanide was not detected in the leaching residue.
[0026] Example 3
[0027] Pretreated overhaul slag powder was taken, and a low-temperature composite roasting aid was added at a ratio of 12% of the powder mass. The mass ratio of calcium carbonate, aluminum sulfate, and modified diatomaceous earth in the aid was 45:35:20. After being mixed evenly, the mixture was fed into a rotary kiln and roasted at 680℃ for 1.5 hours. The subsequent water washing conditions were the same as in Example 1. In the acid leaching step, the sulfuric acid solution concentration was 1.8 mol / L, the leaching temperature was 65℃, and the leaching time was 90 minutes. The lithium leaching conversion rate in this example was 93.6%, and cyanide was not detected in the leaching residue.
[0028] The results of the above embodiments show that, within the range of roasting temperature, additive ratio and acid leaching parameters described in this invention, cyanide in aluminum electrolysis overhaul slag can be completely decomposed, and the lithium leaching conversion rate can be stably reached over 90%, verifying the feasibility and technical effect of the technical solution described in this invention.
[0029] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make possible changes and modifications without departing from the spirit and scope of the present invention. Therefore, any modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope defined by the claims of the present invention.
Claims
1. A method for low-temperature roasting, detoxification, and lithium extraction from aluminum electrolysis overhaul slag, characterized in that, Includes the following steps: The raw material pretreatment step involves sequentially crushing, ball milling, and sieving the aluminum electrolysis overhaul slag to obtain overhaul slag powder with a particle size not exceeding 200 mesh. A low-temperature composite roasting aid is then added to the overhaul slag powder and mixed evenly to obtain a mixture. The low-temperature composite roasting aid includes calcium carbonate, aluminum sulfate, and modified diatomaceous earth, and the amount of the low-temperature composite roasting aid added is 8% to 12% of the mass of the overhaul slag powder. In the low-temperature roasting step, the mixture is fed into a rotary kiln and roasted at a constant temperature of 550℃~680℃ for 1.5~3 hours, while air is introduced into the rotary kiln to obtain roasted clinker. During the roasting process, the waste heat of the flue gas is recovered through a waste heat boiler set at the kiln tail to obtain recovered hot water. The clinker washing step involves cooling the roasted clinker and then adding it to the recycled hot water for stirring and slurry preparation. The liquid-to-solid ratio is 5:
1. The mixture is stirred at room temperature for 30 minutes and then filtered to obtain the washed filter residue and washing liquid. In the low-concentration acid leaching step, the water-washed filter residue is added to a sulfuric acid solution for leaching. The concentration of the sulfuric acid solution is 1.2–1.8 mol / L, the leaching temperature is 50°C–65°C, and the leaching time is 90–150 minutes. The heat source for leaching is the residual heat recovered in the low-temperature roasting step. After leaching, the residue is separated by pressure filtration to obtain a lithium-rich leaching solution and leaching residue.
2. The method according to claim 1, characterized in that, In the low-temperature composite calcination aid, the mass ratio of calcium carbonate, aluminum sulfate, and modified diatomaceous earth is 45–55:25–35:15–25.
3. The method according to claim 1, characterized in that, In the low-temperature roasting step, the low-temperature composite roasting aid undergoes a solid-phase transformation reaction with lithium fluoride and lithium fluoroaluminate in the overhaul slag powder to generate water-soluble lithium sulfate. The cyanide in the overhaul slag powder is oxidized and decomposed into carbon dioxide and nitrogen. The soluble fluorine in the overhaul slag powder is converted into calcium fluoride and solidified in the roasted clinker.
4. The method according to claim 1, characterized in that, The recovered hot water obtained from the waste heat boiler includes steam and hot water, wherein the hot water is used to prepare the roasted clinker into a slurry in the clinker washing step, and the steam is used to heat the sulfuric acid solution in the low-concentration acid leaching step.
5. The method according to claim 1, characterized in that, The washing liquid obtained in the clinker washing step is concentrated and dried by a mechanical steam recompression device to obtain sodium fluoride solid byproduct. The condensate generated from the concentration and drying process is recycled for the slurry preparation process in the clinker washing step.
6. The method according to claim 1, characterized in that, In the raw material pretreatment step, the amount of the low-temperature composite roasting aid added is 10% of the mass of the overhaul slag powder; In the low-temperature roasting step, the roasting temperature is 620℃ and the constant-temperature roasting time is 2 hours.
7. The method according to claim 1, characterized in that, In the low-concentration acid leaching step, the concentration of the sulfuric acid solution is 1.5–1.8 mol / L, the leaching temperature is 60°C, and the leaching time is 120 minutes.
8. The method according to claim 1, characterized in that, The rotary kiln is lined with 2205 stainless steel, and the inner wall of the rotary kiln is equipped with material lifting plates, which are used to scatter the mixture during the operation of the rotary kiln.