A method for deep removal of chromium and titanium from cobalt sulfate solutions containing high levels of chromium and titanium.

By preparing basic chromium oxide composite crystal seeds and combining them with potential and pH control, deep removal of chromium and titanium from cobalt sulfate solution was achieved, solving the problems of cobalt loss and filtration difficulties, and achieving the purification effect of battery-grade cobalt salt.

CN123108325APending Publication Date: 2026-11-17GANZHOU HANRUI NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611620636.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve selective precipitation of chromium and titanium impurities when removing them from cobalt sulfate solutions under low pH conditions, resulting in significant cobalt loss and difficulty in filtering the precipitates, thus failing to meet the purification requirements for battery-grade cobalt salts.

Method used

By preparing basic chromium oxide composite crystal seed crystals under weakly acidic conditions and inducing chromium and titanium ions to precipitate directionally on the seed crystal surface through the synergistic control of potential and pH, and by adding alkaline precipitant in parallel flow, the local pH of the reaction system is ensured to be within the window where cobalt ions do not precipitate, thus achieving deep removal of chromium and titanium.

Benefits of technology

It achieves highly selective separation of chromium and titanium, with a cobalt recovery rate of up to 99.5%. The precipitate is easy to filter, solving the problems of cobalt loss and difficult filtration in traditional methods, and meeting the purification requirements of battery-grade cobalt salts.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium, belonging to the field of hydrometallurgical technology. The method includes: firstly, adding an alkaline precipitant solution to a cobalt salt solution containing chromium and titanium, controlling the system pH to 3.8-4.3 and the redox potential to 300-450 mV, to generate basic chromium oxide composite crystal seed crystals; then, maintaining the above conditions, adding the cobalt salt solution containing chromium and titanium and the alkaline precipitant solution in a co-current manner to the system containing the seed crystals, inducing chromium and titanium ions to precipitate directionally on the surface of the seed crystals; after the reaction, performing solid-liquid separation to obtain a filtrate and a filter residue containing chromium and titanium. This invention achieves highly selective removal of chromium and titanium and a high recovery rate of cobalt through precise control of potential and pH, utilizing a seed crystal induction mechanism, while simultaneously solving the precipitation and filtration problem. The process is simple, efficient, and suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of hydrometallurgical technology, and in particular to a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high chromium and high titanium. Background Technology

[0002] When recovering valuable cobalt from complex secondary resources such as scrap cemented carbide and high-temperature alloys, the raw materials often contain large amounts of alloying elements such as chromium and titanium. The resulting cobalt sulfate solution after acid leaching has a complex composition, with high levels of chromium (Cr(III)) and titanium (existing as Ti(IV)) (typically Cr 2-8 g / L, Ti 1-5 g / L). The presence of these impurities severely affects the quality of subsequent cobalt salt products (such as cobalt carbonate, cobalt tetroxide, and cobalt sulfate), especially for battery-grade cobalt salts, where chromium and titanium are harmful impurities that must be thoroughly removed.

[0003] Currently, traditional methods for removing chromium and titanium mostly employ hydroxide precipitation, which involves raising the pH of the solution to above 5.0 by adding alkalis such as sodium hydroxide or sodium carbonate, causing chromium and titanium to co-precipitate as hydroxides. However, this method has significant drawbacks: (1) At high pH, ​​cobalt ions (Co... 2+ (1) A large amount of cobalt hydroxide precipitate will be generated, resulting in serious loss of cobalt; (2) The formed hydroxide colloidal particles are fine, with extremely poor filtration performance and difficulty in solid-liquid separation; (3) It is difficult to remove chromium and titanium to the ppm level, and the purification effect is not ideal.

[0004] In summary, existing technologies for removing chromium and titanium impurities from cobalt sulfate solutions consistently face a difficult-to-resolve contradiction: using a higher precipitation pH to ensure complete precipitation of chromium and titanium inevitably leads to significant co-precipitation loss of cobalt; conversely, using a lower precipitation pH to reduce cobalt loss results in incomplete precipitation of chromium and titanium, making it difficult to achieve the required purification depth for battery-grade cobalt salts. Furthermore, in conventional direct alkali precipitation operations, the rapid precipitation reaction and lack of effective crystal growth control typically result in amorphous colloids with fine, viscous particles that are difficult to filter, severely limiting production efficiency. Moreover, existing technologies lack deep purification solutions for systems with high chromium and titanium coexistence, particularly effective methods to simultaneously achieve selective precipitation of chromium and titanium and high cobalt recovery rates under near-neutral conditions. Therefore, developing a purification method capable of selectively and deeply removing chromium and titanium under low pH conditions while maintaining high cobalt recovery rates and ensuring easy filtration of the precipitate has significant industrial application value. Summary of the Invention

[0005] To address the technical bottleneck of existing technologies where it is difficult to simultaneously achieve high chromium and titanium removal depth, high cobalt recovery rate, and high filtration performance, this invention provides a method for the deep and selective removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium. This method utilizes precise, coordinated control of potential and pH to pre-construct basic chromium oxide composite crystal seed crystals under weakly acidic conditions. These seed crystals then induce the directional precipitation of chromium and titanium ions onto the seed crystal surface, rather than forming homogeneous nucleations in the solution to create difficult-to-filter amorphous colloids. This fundamentally solves the problem of difficult solid-liquid separation. Simultaneously, the co-current addition of the pre-liquid and the alkaline precipitant ensures that the local pH of the reaction system remains stable within a window where cobalt ions do not precipitate while chromium and titanium ions continuously hydrolyze and crystallize. This achieves deep removal of chromium and titanium while minimizing cobalt loss and ensuring excellent solid-liquid separation performance.

[0006] The technical solution of the present invention is as follows: This invention provides a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium, comprising the following steps: S1. Seed preparation: Add an alkaline precipitant solution to a cobalt salt solution containing chromium and titanium, control the pH of the system to 3.8-4.3 and the redox potential to 300-450mV, and react to generate basic chromium oxide composite crystal seed. S2, Induced Precipitation: Maintaining the temperature, pH and redox potential conditions of S1, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added in a co-current manner to the system containing the seed crystals to induce the directional precipitation of chromium and titanium ions on the surface of the seed crystals. S3. Solid-liquid separation: After the reaction is completed, solid-liquid separation is performed to obtain filtrate and filter residue containing chromium and titanium.

[0007] Preferably, in step S1, an alkaline precipitant solution is added to a cobalt salt bottom solution containing chromium and titanium at a temperature of 60-85°C and a stirring speed of 200-400 rpm.

[0008] Preferably, in step S1, the total concentration of chromium and titanium in the cobalt salt bottom solution containing chromium and titanium is less than 1 g / L.

[0009] More preferably, the cobalt salt solution containing chromium and titanium has a cobalt concentration of 55-65 g / L, a chromium concentration of 0.3-0.6 g / L, a titanium concentration of 0.2-0.4 g / L, and a pH of 2.0-3.0.

[0010] More preferably, the chromium- and titanium-containing cobalt salt substrate is a chromium- and titanium-containing cobalt sulfate solution.

[0011] Preferably, in step S1, the reaction time is 20-40 minutes.

[0012] Preferably, in S1 and S2, the redox potential is controlled by introducing air or oxygen into the reaction system.

[0013] More preferably, the air or oxygen introduction rate is 8-12 mL / min.

[0014] Preferably, in S1 and S2, the concentration of the alkaline precipitant solution is 100-200 g / L, and the alkaline precipitant is selected from at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, or ammonia water.

[0015] More preferably, the alkaline precipitant solution is a sodium carbonate solution with a concentration of 100-200 g / L.

[0016] Preferably, in step S2, the cobalt salt pre-solution containing chromium and titanium has a cobalt concentration of 50-70 g / L, a chromium concentration of 2-8 g / L, a titanium concentration of 1-5 g / L, and a pH of 1.8-2.2.

[0017] More preferably, the cobalt salt pre-solution containing chromium and titanium is a cobalt sulfate solution containing chromium and titanium.

[0018] Further explanation of the present invention: In step S1, the pH is controlled at 3.8-4.3, and air or oxygen is introduced to maintain the redox potential at 300-450 mV. The purpose is to allow chromium ions in the substrate to hydrolyze, polymerize, and partially oxidize, generating basic chromium oxide composite crystals as seed crystals for subsequent precipitation. Although titanium ions in the substrate also hydrolyze under these conditions, the hydrolysis products are unlikely to form long-range ordered crystal nuclei; most remain in the solution, with only trace amounts of hydrolyzed titanium species physically adsorbed onto the surface of the seed crystal particles. Therefore, the seed crystals generated in this step are mixed-valence chromium-oxygen crystals containing trivalent chromium and some high-valence chromium, rather than a chromium-titanium eutectic solid solution. In this process, pH and potential each play different regulatory roles and cooperate with each other. The role of pH is to provide the necessary proton environment for the hydrolysis and polymerization of chromium ions, allowing the chromium-oxygen structural units to gradually condense to form basic salt crystals. Simultaneously, this pH value is far below the critical value at which cobalt ions begin to significantly hydrolyze and form cobalt hydroxide precipitate, thus ensuring that the cobalt ions in the substrate do not precipitate and are entirely retained in the solution. The role of the potential is to oxidize some trivalent chromium to a higher valence state under mild oxidation conditions of 300-450mV, promoting the formation of mixed-valence chromium-oxygen cluster structures. The regular arrangement of these structural units constitutes the crystallographic basis for the seed crystal's inductive activity. If the pH is below 3.8, the degree of chromium hydrolysis is insufficient, making it difficult to generate a sufficient number and size of seed crystals. If the pH is above 4.3, the system approaches the hydrolysis boundary of cobalt, posing a risk of cobalt co-precipitation. If the potential is too low, the ordered structure inside the seed crystal will not develop sufficiently, resulting in insufficient subsequent inductive activity. If the potential is too high, cobalt ions may be oxidized and enter the crystal lattice. Therefore, the synergistic control of pH and potential within the aforementioned specific ranges is crucial for obtaining basic chromium oxide composite seed crystals with good inductive activity.

[0019] Preferably, in step S2, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added to the system containing the seed crystals in a co-current manner, so that the addition rates of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are matched, and the local pH of the reaction system is controlled to be maintained in the range of 3.8-4.3.

[0020] Preferably, in step S2, the total time for adding the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution in parallel is 1-4 hours, and after the addition of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution, the reaction is continued for 20-40 minutes with heat preservation and stirring.

[0021] Preferably, in S1 and S2, the pH value is automatically controlled by linking an online pH meter with a metering pump, with a control accuracy of ±0.1.

[0022] Further explanation of the present invention: In step S2, while maintaining the temperature, pH, and redox potential conditions of step S1, the cobalt salt pre-solution containing chromium and titanium and the alkaline precipitant solution are continuously added to the reaction system containing the seed crystals in a co-current manner. The newly introduced chromium and titanium ions undergo directional adsorption and orderly growth at the active sites on the seed crystal surface. The free energy required for this heterogeneous nucleation is much lower than that for spontaneous nucleation in solution. Therefore, chromium and titanium preferentially deposit on the seed crystal surface rather than independently forming new crystal nuclei. The induced growth on the seed crystal surface causes the precipitate products to stack orderly along the crystal direction of the seed crystal, ultimately forming dense crystalline basic salt particles, rather than the amorphous hydroxide colloids of traditional methods. The co-current addition of the pre-solution and the precipitant ensures uniform mixing of the two in the seed crystal system and avoids drastic pH fluctuations due to excessively high local concentrations of the precipitant. If the precipitant is added all at once or added first and then introduced into the pre-solution, the sudden increase in local alkalinity will cause cobalt ions to hydrolyze and precipitate in that micro-region. At the same time, chromium and titanium will also rapidly nucleate homogeneously to form colloids due to a sudden increase in supersaturation. The co-current feeding ensures that the local pH remains stable within the range of 3.8-4.3 at any given time, thus guaranteeing the thermodynamic and kinetic controllability of the induced precipitation process. Simultaneously, because the system pH is far below the critical value at which cobalt ions begin to significantly hydrolyze and precipitate, the cobalt ions remain in a dissolved state throughout the entire process.

[0023] Preferably, in step S3, the filtrate contains less than 8 ppm of chromium and less than 3 ppm of titanium.

[0024] Preferably, in step S3, the recovery rate of cobalt in the filtrate is greater than 99.5%.

[0025] The present invention has the following beneficial effects: 1. Compared with existing technologies, this invention provides a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium. By pre-preparing basic chromium oxide composite crystals as seed crystals, an ordered growth template is provided for the precipitation of chromium and titanium. These seed crystals cause chromium and titanium ions to grow directionally on their surface as crystalline basic salts rather than amorphous colloids, fundamentally changing the traditional precipitation method where chromium and titanium precipitate as amorphous hydroxides, thus solving the problem of difficult solid-liquid separation. Simultaneously, this invention strictly controls the system pH at 3.8-4.3 and the redox potential at 300-450 mV, making the hydrolysis and precipitation tendency of chromium and titanium significantly stronger than that of cobalt ions. Under these conditions, cobalt ions remain essentially dissolved, achieving highly selective separation of chromium, titanium, and cobalt. The cobalt recovery rate provided by this invention is much higher than that of traditional hydroxide precipitation methods, avoiding the loss of large amounts of cobalt co-precipitation under high pH conditions and the loss of cobalt due to excessive oxidation. It ensures efficient cobalt recovery while deeply removing chromium and titanium. Furthermore, this invention precisely matches the addition rates of the pre-liquid and the alkaline precipitant through a co-current feeding method, ensuring that the local pH of the reaction system is always maintained within a set range. This avoids cobalt co-precipitation and amorphous mixed precipitation caused by local over-alkaliness, thus guaranteeing the stability of the purification depth and the repeatability of the process.

[0026] 2. Compared to existing technologies, the steps of this invention form a close synergistic relationship: the seed crystal preparation step pre-forms basic chromium oxide composite crystals with inductive activity under specific pH and potential conditions, providing a foundation for subsequent selective precipitation; the induced precipitation step, in the presence of these seed crystals, utilizes the same pH and potential conditions to directionally deposit chromium and titanium on the seed crystal surface, while maintaining system stability through co-current feeding, ensuring the uniformity and controllability of the precipitation process; the solid-liquid separation step is efficiently completed thanks to the crystalline precipitates formed in the first two steps. The process steps provided by this invention are mutually synergistic and indispensable, jointly achieving a deep purification effect with chromium content below 8 ppm and titanium content below 3 ppm in the purified liquid, while achieving a cobalt recovery rate of over 99.5%, and the precipitate is easily filtered and separated, providing an efficient, economical, and feasible purification solution for the production of battery-grade cobalt salts. Furthermore, the method of this invention is simple, uses conventional industrial raw materials, has mild reaction conditions, and pH and potential can be automatically controlled by online instruments, making it easy to achieve continuous industrial production. Detailed Implementation

[0027] The technical solutions described below in conjunction with the embodiments will be clearly and completely described. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0028] This invention provides a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium, comprising the following steps: S1. Seed preparation: Add an alkaline precipitant solution to a cobalt salt solution containing chromium and titanium, control the pH of the system to 3.8-4.3 and the redox potential to 300-450mV, and react to generate basic chromium oxide composite crystal seed. Specifically, the pH can be any one of 3.8, 3.9, 4.0, 4.1, 4.2, 4.3 or a range between two of them; the redox potential can be any one of 300mV, 320mV, 340mV, 350mV, 360mV, 380mV, 400mV, 420mV, 440mV, 450mV or a range between two of them. S2, Induced Precipitation: Maintaining the temperature, pH and redox potential conditions of S1, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added in a co-current manner to the system containing the seed crystals to induce the directional precipitation of chromium and titanium ions on the surface of the seed crystals. S3. Solid-liquid separation: After the reaction is completed, solid-liquid separation is performed to obtain filtrate and filter residue containing chromium and titanium.

[0029] Preferably, in step S1, an alkaline precipitant solution is added to a cobalt salt bottom solution containing chromium and titanium at a temperature of 60-85°C and a stirring speed of 200-400 rpm.

[0030] Specifically, the temperature can be any one of 60℃, 65℃, 70℃, 75℃, 80℃, 85℃ or a range between two of them; the stirring speed can be any one of 200rpm, 250rpm, 300rpm, 350rpm, 400rpm or a range between two of them.

[0031] Preferably, in step S1, the total concentration of chromium and titanium in the cobalt salt bottom solution containing chromium and titanium is less than 1 g / L.

[0032] More preferably, the cobalt salt solution containing chromium and titanium has a cobalt concentration of 55-65 g / L, a chromium concentration of 0.3-0.6 g / L, a titanium concentration of 0.2-0.4 g / L, and a pH of 2.0-3.0.

[0033] More preferably, the chromium- and titanium-containing cobalt salt substrate is a chromium- and titanium-containing cobalt sulfate solution.

[0034] Preferably, in step S1, the reaction time is 20-40 minutes.

[0035] Specifically, the reaction time can be any one of 20 min, 25 min, 30 min, 35 min, or 40 min, or a range between two of them.

[0036] Preferably, in S1 and S2, the redox potential is controlled by introducing air or oxygen into the reaction system.

[0037] More preferably, the air or oxygen introduction rate is 8-12 mL / min.

[0038] Specifically, the air or oxygen introduction rate can be any one of 8 mL / min, 9 mL / min, 10 mL / min, 11 mL / min, 12 mL / min, or a range between two of them.

[0039] Preferably, in S1 and S2, the concentration of the alkaline precipitant solution is 100-200 g / L, and the alkaline precipitant is selected from at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, or ammonia water.

[0040] Specifically, the concentration of the alkaline precipitant solution can be any one of 100 g / L, 120 g / L, 150 g / L, 160 g / L, 180 g / L, 200 g / L, or a range between two of them.

[0041] More preferably, the alkaline precipitant solution is a sodium carbonate solution with a concentration of 100-200 g / L.

[0042] Preferably, in step S2, the cobalt salt pre-solution containing chromium and titanium has a cobalt concentration of 50-70 g / L, a chromium concentration of 2-8 g / L, a titanium concentration of 1-5 g / L, and a pH of 1.8-2.2.

[0043] More preferably, the cobalt salt pre-solution containing chromium and titanium is a cobalt sulfate solution containing chromium and titanium.

[0044] Preferably, in step S2, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added to the system containing the seed crystals in a co-current manner, so that the addition rates of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are matched, and the local pH of the reaction system is controlled to be maintained in the range of 3.8-4.3.

[0045] Preferably, in step S2, the total time for adding the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution in parallel is 1-4 hours, and after the addition of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution, the reaction is continued for 20-40 minutes with heat preservation and stirring.

[0046] Specifically, the total time for the cobalt salt pre-solution containing chromium and titanium to be added in parallel with the alkaline precipitant solution can be any one of 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, or a range between the two; the time for continuing the heat preservation and stirring reaction can be any one of 20min, 25min, 30min, 35min, 40min, or a range between the two.

[0047] Preferably, in S1 and S2, the pH value is automatically controlled by linking an online pH meter with a metering pump, with a control accuracy of ±0.1.

[0048] Preferably, in step S3, the filtrate contains less than 8 ppm of chromium and less than 3 ppm of titanium.

[0049] Preferably, in step S3, the recovery rate of cobalt in the filtrate is greater than 99.5%.

[0050] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0051] Example 1

[0052] A method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium includes the following steps: S1. Take a 5L jacketed heating reactor, equipped with a mechanical stirrer, an online pH / ORP electrode, a thermometer, a dual-channel metering feed pump, and a subsurface aeration device; add 1L of cobalt sulfate bottom solution to the reactor, the bottom solution has a Co concentration of 60g / L, a Cr concentration of 0.5g / L, a Ti concentration of 0.3g / L, a total Cr and Ti concentration of 0.8g / L, and an initial pH of 2.0; heat to 75℃ and maintain a stirring speed of 200rpm, add 43mL of 150g / L sodium carbonate solution to the bottom solution through the linkage of the online pH meter and the metering pump, adjust the pH of the system to 4.0, and at the same time, introduce air under the liquid surface at a rate of 10 mL / min to stabilize the redox potential at 380±20mV; react under these conditions for 30min to form blue-green basic chromium oxide composite crystal seed crystals; S2. Maintaining the conditions of S1 temperature 75℃, stirring speed 200rpm, pH 4.0, and redox potential 380±20mV, 1L of cobalt sulfate pre-solution and 215mL of sodium carbonate solution with a concentration of 150g / L were simultaneously added to the reactor in parallel flow using two metering pumps. The feeding rate was controlled to ensure that the total feeding time was 2h, and the addition rates of the cobalt sulfate pre-solution and sodium carbonate solution were matched to maintain the local pH of the reaction system within the range of 3.8-4.3. The cobalt sulfate pre-solution had a Co concentration of 65g / L, a Cr concentration of 5.2g / L, a Ti concentration of 2.8g / L, and a pH of 2. After the feeding was completed, the reaction was continued to be stirred and kept at the same temperature for 30min. S3. After the reaction is complete, filter all the slurry while it is still hot to obtain 2.21L of filtrate and filter residue containing chromium and titanium.

[0053] The filtrate was tested, and the results showed that the concentration of chromium in the filtrate was 5.2 ppm, the concentration of titanium was 1.8 ppm, and the concentration of cobalt was 56.40 g / L. The cobalt recovery rate was 99.54% based on the cobalt balance.

[0054] Example 2

[0055] The difference between this embodiment and Example 1 lies in the composition of the cobalt sulfate pre-solution. The cobalt sulfate pre-solution contains 55 g / L Co, 7.5 g / L Cr, and 4.5 g / L Ti, with a pH of 2. The reaction conditions in steps S1 and S2 are different from those in Example 1. The reaction temperature is controlled at 80°C, the system pH is 4.2, and the redox potential is stabilized at 420 ± 20 mV. The remaining operation steps and parameters are the same as in Example 1.

[0056] In this embodiment, 2.18 L of filtrate was obtained. The filtrate was tested, and the results showed that the concentration of chromium in the filtrate was 7.1 ppm, the concentration of titanium was 2.5 ppm, and the concentration of cobalt was 52.60 g / L. The cobalt recovery rate was 99.6% according to the cobalt balance calculation.

[0057] Comparative Example 1 The difference between this comparative example and Example 1 is that the traditional hydroxide precipitation method was used. 1L of the same batch of cobalt sulfate pre-liquid as in Example 1 (Co concentration of 65g / L, Cr concentration of 5.2g / L, Ti concentration of 2.8g / L, pH of 2) was taken, and solid NaOH was added to adjust the pH of the system to 5.5 at a temperature of 75°C and a stirring speed of 200rpm. It was observed that a large amount of viscous colloidal precipitate was immediately generated in the solution, the viscosity of the slurry increased significantly, and solid-liquid separation was extremely difficult, taking up to 4 hours using vacuum filtration.

[0058] The comparative example yielded 0.84 L of filtrate. The filtrate after filtration was tested, and the results showed that the concentration of chromium in the filtrate was 125 ppm, the concentration of titanium was 45 ppm, and the concentration of cobalt was 73.06 g / L. According to the cobalt balance calculation, the cobalt recovery rate was only 94.1%.

[0059] Comparative Example 2 The difference between this comparative example and Example 1 is that basic chromium oxide composite crystal seeds are not prepared in step S1; the remaining operation steps and parameters are the same as in Example 1. Step S1 specifically involves: Take a 5L jacketed heating reactor, equipped with mechanical stirring, online pH / ORP electrode, thermometer, dual-channel metering feed pump and subsurface aeration device; add 1L of cobalt sulfate solution with a cobalt concentration of 60g / L and free of chromium and titanium impurities to the reactor, with an initial pH of 2.0; heat to 75℃ and maintain stirring speed at 200rpm, and adjust the pH of the system to 4.0 through the linkage control of online pH meter and metering pump, while simultaneously purging air under the liquid surface at a rate of 10 mL / min to stabilize the redox potential at 380±20mV.

[0060] The comparative example yielded 2.14 L of filtrate. The filtrate was tested, and the results showed that the chromium concentration was 42.6 ppm, the titanium concentration was 18.3 ppm, and the cobalt concentration was 56.77 g / L. According to the cobalt balance calculation, the cobalt recovery rate was 97.21%. During the reaction, a large amount of fine, viscous amorphous colloidal precipitate was generated, the slurry viscosity increased, the filtration time was 85 min, and the solid-liquid separation efficiency deteriorated significantly.

[0061] Comparative Example 3 The difference between this comparative example and Example 1 is that the pH of the system in step S1 is adjusted to 3.5, and in step S2, the conditions of temperature 75°C, stirring speed 200 rpm, pH 3.5 and redox potential 380±20 mV are maintained in S1. 1 L of cobalt sulfate pre-solution and 215 mL of sodium carbonate solution with a concentration of 150 g / L are simultaneously added to the reactor in parallel flow using two metering pumps, and the local pH of the reaction system is always maintained in the range of 3.4-3.6. The remaining operating steps and parameters are the same as in Example 1.

[0062] The comparative example yielded 2.22 L of filtrate. Analysis of the filtrate revealed a chromium concentration of 36.8 ppm, a titanium concentration of 15.7 ppm, and a cobalt concentration of 55.98 g / L. Cobalt balance calculations showed a cobalt recovery rate of 99.47%. While the filtration performance of the slurry in this comparative example was acceptable, the high levels of residual chromium and titanium impurities failed to meet the impurity control requirements for battery-grade cobalt salts.

[0063] Comparative Example 4 The difference between this comparative example and Example 1 is that the redox potential in step S1 is stabilized at 250±20mV, and in step S2 the conditions of temperature 75℃, stirring speed 200rpm, pH 4.0 and redox potential 250±20mV are maintained in S1. 1L of cobalt sulfate pre-solution and 215mL of sodium carbonate solution with a concentration of 150g / L are added to the reactor simultaneously in parallel flow using two metering pumps. The remaining operating steps and parameters are the same as in Example 1.

[0064] This comparative example yielded 2.21 L of filtrate. Analysis of the filtrate revealed a chromium concentration of 31.4 ppm, a titanium concentration of 13.6 ppm, and a cobalt concentration of 56.22 g / L. Cobalt balance calculations showed a cobalt recovery rate of 99.49%. The precipitated particles in this comparative example were finer than those in Example 1, resulting in a lower filtration rate and higher levels of residual chromium and titanium impurities in the filtrate, failing to meet the impurity control requirements for battery-grade cobalt salts.

[0065] In summary, this invention provides a method for deep removal of chromium and titanium from a cobalt sulfate solution containing high levels of chromium and titanium. The method first involves precisely controlling the pH of the cobalt salt solution containing chromium and titanium to 3.8-4.3 and the redox potential to 300-450 mV, causing a controlled partial oxidation and hydrolysis reaction of trivalent chromium to form a basic chromium oxide composite crystal seed with a stable crystal structure. Subsequently, under the same conditions, the cobalt salt pre-solution containing chromium and titanium and an alkaline precipitant solution are added to the seed-containing system in a co-current manner. This allows the newly introduced chromium and titanium ions to preferentially adsorb onto the seed surface and grow oriented along the crystal lattice, forming a coarse-grained, dense crystalline composite precipitate. This method, through the close coordination of three steps—seed preparation, induced precipitation, and solid-liquid separation—transforms the precipitation of chromium and titanium from homogeneous nucleation in traditional amorphous colloids to ordered crystal growth on the seed surface, fundamentally solving the problem of difficult filtration. Simultaneously, by synergistically controlling potential and pH, the hydrolysis and precipitation tendency of chromium and titanium is significantly stronger than that of cobalt ions, achieving highly selective separation of chromium, titanium, and cobalt and avoiding significant co-precipitation loss of cobalt. The co-current feeding method ensures that the local pH of the reaction system is consistently maintained within the set range, further guaranteeing the stability and repeatability of the purification process. This invention achieves efficient cobalt recovery while deeply removing chromium and titanium impurities, and the precipitate is easily separated by filtration. The process is simple, controllable, and suitable for industrial applications, providing reliable technical support for the green and efficient production of battery-grade cobalt salts.

[0066] The above description is merely a preferred embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural transformations made using the contents of the present invention under the inventive concept of the present invention, or direct / indirect applications in other related technical fields, are included within the patent protection scope of the present invention.

Claims

1. A method for deeply removing chromium and titanium from a cobalt sulfate solution containing high chromium and high titanium, characterized in that, Includes the following steps: S1. Seed preparation: Add an alkaline precipitant solution to a cobalt salt solution containing chromium and titanium, control the pH of the system to 3.8-4.3 and the redox potential to 300-450mV, and react to generate basic chromium oxide composite crystal seed. S2, Induced Precipitation: Maintaining the temperature, pH and redox potential conditions of S1, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added in a co-current manner to the system containing the seed crystals to induce the directional precipitation of chromium and titanium ions on the surface of the seed crystals. S3. Solid-liquid separation: After the reaction is completed, solid-liquid separation is performed to obtain filtrate and filter residue containing chromium and titanium.

2. The method of claim 1, wherein, In step S1, an alkaline precipitant solution is added to a cobalt salt bottom solution containing chromium and titanium at a temperature of 60-85℃ and a stirring speed of 200-400rpm.

3. The method of claim 1, wherein, In S1, the total concentration of chromium and titanium in the cobalt salt bottom solution containing chromium and titanium is less than 1 g / L.

4. The method of claim 1, wherein, In S1, the reaction time is 20-40 min.

5. The method of claim 1, wherein, In S1 and S2, the concentration of the alkaline precipitant solution is 100-200 g / L, and the alkaline precipitant is selected from at least one of sodium carbonate, sodium bicarbonate, sodium hydroxide, and ammonia water.

6. The method of claim 1, wherein, In step S2, the cobalt salt pre-solution containing chromium and titanium has a cobalt concentration of 50-70 g / L, a chromium concentration of 2-8 g / L, a titanium concentration of 1-5 g / L, and a pH of 1.8-2.

2.

7. The method of claim 1, wherein, In step S2, the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are added to the system containing the seed crystals in a co-current manner, so that the addition rates of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution are matched, and the local pH of the reaction system is controlled to be maintained in the range of 3.8-4.

3.

8. The method of claim 1, wherein, In step S2, the total time for adding the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution in parallel is 1-4 hours. After the addition of the cobalt salt pre-liquid containing chromium and titanium and the alkaline precipitant solution, the reaction is continued for 20-40 minutes with heat preservation and stirring.

9. The method of claim 1, wherein, In step S3, the filtrate contains less than 8 ppm of chromium and less than 3 ppm of titanium.

10. The method of claim 1, wherein, In step S3, the cobalt recovery rate in the filtrate is greater than 99.5%.