A method for preparing lightweight, high-strength aluminum alloy profiles and a UAV base bracket
By optimizing the chemical composition and process flow of aluminum alloys, a Mg2Si strengthening phase is formed, which solves the problem of strength and plasticity matching of existing aluminum alloy materials in UAV structural components, and realizes the preparation of lightweight and high-strength aluminum alloy profiles, which are suitable for thin-walled structural components such as UAV base brackets.
Patent Information
- Application Number
- CN202611422956.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Existing 6XXX series aluminum alloys and their preparation processes suffer from problems such as poor strength-plasticity matching, lack of precise control over alloy composition design, wide process parameter windows, and poor microstructure uniformity, making it difficult to meet the lightweight and high-strength requirements of UAV structural components.
By optimizing the chemical composition of aluminum alloys, especially controlling the mass ratio of Mg to Si to be 0.9~1.0, and combining specific melting, refining, semi-continuous casting, homogenization treatment, extrusion forming and T6 heat treatment processes, including solution treatment and artificial aging treatment, a Mg2Si strengthening phase is formed, thereby improving the strength and plasticity of the alloy.
A lightweight aluminum alloy material with high strength and high elongation has been obtained, which is particularly suitable for thin-walled structural components such as drone base brackets, meeting the dual requirements of drones for lightweight and high strength.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of aluminum alloy profile processing technology, and in particular to a method for preparing lightweight, high-strength aluminum alloy profiles and a drone base bracket. Background Technology
[0002] As UAVs evolve towards longer endurance and larger payloads, the requirements for lightweight and high-strength materials in key structural components such as base brackets are increasing. Aluminum alloys have become the preferred choice due to their low density and high specific strength. However, existing 6XXX series (Al-Mg-Si) aluminum alloys and their preparation processes still have significant shortcomings: On the one hand, conventional 6061 aluminum alloys have poor strength-to-plasticity matching, making it difficult to meet the comprehensive mechanical requirements of thin-walled (≤5mm) load-bearing components; on the other hand, the design of alloy composition in existing processes lacks precise control, the process parameter windows for homogenization treatment, extrusion molding, and T6 heat treatment are wide, and the lack of synergistic optimization among various processes leads to insufficient precipitation of strengthening phases and poor microstructure uniformity. In particular, uneven cooling after extrusion can easily cause profile deformation and performance fluctuations. These problems restrict the effective application of lightweight, high-strength aluminum alloys in UAV structural components. Summary of the Invention
[0003] The purpose of this invention is to provide a method for preparing lightweight, high-strength aluminum alloy profiles, thus solving the problem of how to further improve the strength of aluminum alloys.
[0004] To achieve the above objectives, the technical solution adopted by the present invention is as follows: This invention provides a method for preparing lightweight, high-strength aluminum alloy profiles. The lightweight, high-strength aluminum alloy profiles, by weight percentage, have the following chemical composition: Si 0.7%~0.85%; Fe≤0.25%; Cu≤0.08%; Mn≤0.08%; Mg0.7%~0.8%; Cr≤0.07%; Zn≤0.06%; Ti≤0.09%; the balance being Al and unavoidable impurities. The preparation method includes the following steps: S1. Smelting: Prepare the ingredients according to the chemical composition described above. Heat the aluminum ingot to 730℃~780℃ to melt it. First, add the intermediate alloy containing Si, Mg, Cr and Ti in sequence, and then add the remaining chemical components. After it is completely melted, stir it thoroughly. S2. Refining: Argon or nitrogen gas is introduced into the aluminum alloy melt for refining and degassing. The refining temperature is 720℃~750℃ and the refining time is 10~30 minutes. After refining, the mixture is allowed to stand and slag is removed. S3. Casting: Semi-continuous casting is used for casting. The casting temperature is 680℃~720℃, the casting speed is 50~150mm / min, and the cooling water temperature is 15℃~35℃. S4. Homogenization treatment: The aluminum alloy ingots obtained by casting are kept at 540℃~580℃ for 6~12 hours for homogenization treatment, and then cooled in the furnace or air-cooled to room temperature. S5. Extrusion forming: The homogenized aluminum alloy ingot is heated to 450℃~520℃ for extrusion forming, and then cooled immediately after extrusion. S6 and T6 heat treatment: solution treatment temperature 515℃~540℃, hold for 2~6 hours, water quench to below 60℃, then perform artificial aging treatment at 170℃~185℃ for 4~12 hours.
[0005] Furthermore, the mass ratio of Mg to Si in the aluminum alloy material is 0.94~1.
[0006] Furthermore, after T6 heat treatment, the aluminum alloy material has a tensile strength ≥255MPa, a yield strength ≥215MPa, and an elongation ≥6%.
[0007] Furthermore, in the T6 heat treatment step, the artificial aging adopts a two-stage aging process: first, it is held at 170℃ for 2 hours, and then held at 180℃ for 1.5 hours.
[0008] Furthermore, in the extrusion forming step, the extrusion is either forward extrusion or reverse extrusion, the extrusion speed is 2.0 to 3.0 mm / s, the extrusion cylinder temperature is 495℃ to 505℃, and the extrusion die temperature is 445℃ to 455℃.
[0009] Furthermore, in the extrusion forming step, the temperature of the extruded profile when it exits the die is not lower than 520°C.
[0010] Furthermore, the cooling method is water mist cooling, which adopts annular spraying with air atomizing nozzles. The distance between the nozzles and the profile is 120mm-155mm, and the water flow rate of a single nozzle is >3L / min.
[0011] The present invention also provides a drone base bracket, which is made of the aluminum alloy profile obtained above by machining. The aluminum alloy profile is a hollow profile and its wall thickness is ≤5mm.
[0012] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art: The present invention discloses a method for preparing lightweight, high-strength aluminum alloy profiles. By optimizing the chemical composition of the aluminum alloy (especially controlling the mass ratio of Mg to Si within the range of 0.9 to 1.0) and combining it with specific melting, refining, semi-continuous casting, homogenization treatment, extrusion forming and T6 heat treatment processes, a lightweight aluminum alloy material with both high strength and high elongation is obtained, which is particularly suitable for the manufacture of thin-walled structural components such as UAV base brackets. Detailed Implementation
[0013] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0014] Furthermore, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0015] This invention provides a method for preparing a lightweight, high-strength aluminum alloy profile. The chemical composition, by weight percentage, is as follows: Si 0.7%~0.85%; Fe≤0.25%; Cu≤0.08%; Mn≤0.08%; Mg 0.7%~0.8%; Cr≤0.07%; Zn≤0.06%; Ti≤0.09%; the balance being Al and unavoidable impurities. Preferably, the mass ratio of Mg to Si in the aluminum alloy material is 0.94~1. In the above chemical composition of the aluminum alloy material, Si and Mg are the main strengthening elements. During heat treatment, they form the Mg2Si strengthening phase, which plays a decisive role in the strength of the alloy. Controlling the mass ratio of Mg to Si at 0.94~1 ensures the sufficient formation of the Mg2Si phase and avoids the adverse effects of excessive Si or Mg on the alloy's plasticity. Elements such as Fe, Cu, Mn, Cr, Zn, and Ti, as impurities or trace elements, must have their contents strictly controlled within the above range to avoid negatively impacting the alloy's corrosion resistance and processing performance. The preparation method of the present invention includes the following steps: S1, smelting; S2, refining; S3, casting; S4, homogenization treatment; S5, extrusion molding; S6, T6 heat treatment.
[0016] The following description elaborates on specific embodiments and comparative examples: Example 1
[0017] The lightweight, high-strength aluminum alloy profile prepared in this embodiment has the following chemical composition by weight percentage: Si 0.75%; Fe 0.20%; Cu 0.05%; Mn 0.05%; Mg 0.7%; Cr 0.04%; Zn 0.04%; Ti 0.06%; with the balance being Al and unavoidable impurities. In this embodiment, the mass ratio of Mg to Si is 0.93.
[0018] Its preparation method includes the following steps: S1. Smelting: Prepare the ingredients according to the above chemical composition. Add the aluminum ingots to the smelting furnace and heat them to 750°C until they are completely melted. Then, add the intermediate alloy containing Si, Mg, Cr and Ti in sequence, and then add the remaining chemical components. After all the components have melted, stir them thoroughly to ensure that the alloy elements are evenly distributed.
[0019] S2. Refining: High-purity argon gas (purity ≥99.99%) is introduced into the aluminum alloy melt for refining and degassing. The refining temperature is 735℃ and the refining time is 20 minutes. After refining, the mixture is allowed to stand for 15 minutes and then slag is removed.
[0020] S3. Casting: Semi-continuous casting is used, with a casting temperature of 700℃, a casting speed of 100mm / min, and a cooling water temperature of 25℃. The cooling water flow rate is controlled stably during the casting process to ensure a uniform internal structure of the ingot.
[0021] S4. Homogenization treatment: The cast aluminum alloy ingot is placed in a heating furnace and kept at 560℃ for 8 hours for homogenization treatment, and then cooled to room temperature with the furnace.
[0022] S5. Extrusion forming: The homogenized aluminum alloy ingot is heated to 480℃ and extruded on an extrusion press at a speed of 2.5mm / s. The extrusion barrel temperature is 500℃, and the extrusion die temperature is 450℃. The temperature of the extruded profile exiting the die is 525℃.
[0023] S6 and T6 heat treatment: solution treatment temperature 525℃, hold for 4 hours, then quickly transfer to water quenching tank for water quenching and cooling, transfer time not exceeding 15 seconds, cool to below 60℃; then perform artificial aging treatment, aging temperature 180℃, hold for 8 hours. Example 2
[0024] The lightweight, high-strength aluminum alloy profile prepared in this embodiment has the following chemical composition by weight percentage: Si 0.80%; Fe 0.18%; Cu 0.06%; Mn 0.04%; Mg 0.75%; Cr 0.05%; Zn 0.05%; Ti 0.07%; with the balance being Al and unavoidable impurities. In this embodiment, the mass ratio of Mg to Si is 0.94.
[0025] Its preparation method includes the following steps: S1. Smelting: Prepare the ingredients according to the above chemical composition. Add the aluminum ingots to the smelting furnace and heat them to 740°C until they are completely melted. Then, add the intermediate alloy containing Si, Mg, Cr and Ti in sequence, and then add the remaining chemical components. After all the components have melted, stir them thoroughly.
[0026] S2. Refining: Nitrogen gas is introduced into the aluminum alloy melt for refining and degassing. The refining temperature is 730℃ and the refining time is 25 minutes. After refining, the mixture is allowed to stand and slag is removed.
[0027] S3. Casting: Semi-continuous casting is used for casting, with a casting temperature of 690℃, a casting speed of 80mm / min, and a cooling water temperature of 20℃.
[0028] S4. Homogenization treatment: The cast aluminum alloy ingot is kept at 550℃ for 10 hours for homogenization treatment, and then air-cooled to room temperature.
[0029] S5. Extrusion forming: The homogenized aluminum alloy ingot is heated to 460℃ and extruded. The extrusion speed is 2.0mm / s, the extrusion barrel temperature is 495℃, and the extrusion die temperature is 445℃. The temperature of the extruded profile exiting the die is 520℃.
[0030] S6 and T6 heat treatment: solution treatment temperature 520℃, hold for 5 hours, water quenching to below 60℃; then artificial aging treatment, aging temperature 175℃, hold for 10 hours. Example 3
[0031] The lightweight, high-strength aluminum alloy profile prepared in this embodiment has the following chemical composition by weight percentage: Si 0.82%; Fe 0.22%; Cu 0.07%; Mn 0.06%; Mg 0.8%; Cr 0.06%; Zn 0.05%; Ti 0.08%; with the balance being Al and unavoidable impurities. In this embodiment, the mass ratio of Mg to Si is 0.98.
[0032] Its preparation method includes the following steps: S1. Smelting: Prepare the ingredients according to the above chemical composition. Add the aluminum ingots to the smelting furnace and heat them to 760°C until they are completely melted. Then, add the intermediate alloy containing Si, Mg, Cr and Ti in sequence, and then add the remaining chemical components. After all the components have melted, stir them thoroughly.
[0033] S2. Refining: High-purity argon gas is introduced into the aluminum alloy melt for refining and degassing. The refining temperature is 745℃ and the refining time is 15 minutes. After refining, the mixture is allowed to stand and slag is removed.
[0034] S3. Casting: Semi-continuous casting is used for casting. The casting temperature is 710℃, the casting speed is 120mm / min, and the cooling water temperature is 30℃.
[0035] S4. Homogenization treatment: The cast aluminum alloy ingot is kept at 570℃ for 7 hours for homogenization treatment, and then cooled to room temperature in the furnace.
[0036] S5. Extrusion forming: The homogenized aluminum alloy ingot is heated to 500℃ and extruded. The extrusion speed is 3.0mm / s, the extrusion barrel temperature is 505℃, and the extrusion die temperature is 455℃. The temperature of the extruded profile exiting the die is 530℃.
[0037] S6 and T6 heat treatment: solution treatment temperature 535℃, hold for 3 hours, water quenching to below 60℃; then artificial aging treatment, aging temperature 185℃, hold for 6 hours. Example 4
[0038] This embodiment is basically the same as Embodiment 1, except that the artificial aging process in the T6 heat treatment step adopts a two-stage aging process: first, holding at 170℃ for 2 hours, and then holding at 180℃ for 1.5 hours. The remaining steps are the same as in Embodiment 1.
[0039] Comparative Example 1 This comparative example is basically the same as Example 1, except that: Si 0.65%; Fe 0.35%; Cu 0.1%; Mn 0.1%; Mg 0.4%; Cr 0.1%; Zn 0.1%; Ti 0.1%; the balance is Al and unavoidable impurities.
[0040] Comparative Example 2 This comparative example is basically the same as Example 1, except that: Si 0.9%; Fe 0.35%; Cu 0.1%; Mn 0.1%; Mg 0.6%; Cr 0.1%; Zn 0.1%; Ti 0.1%; the balance being Al and unavoidable impurities.
[0041] Comparative Example 3 This comparative example is basically the same as Example 1, except that the homogenization treatment temperature is 500℃ and the holding time is 4 hours.
[0042] Comparative Example 4 This comparative example is basically the same as Example 1, except that the solution treatment temperature in the T6 heat treatment is 500℃.
[0043] Performance testing The aluminum alloy materials obtained in Examples 1-4 and Comparative Examples 1-4 were subjected to room temperature tensile mechanical properties and Brinell hardness tests according to GB / T6892-2023 standard. The test results are shown in Table 1.
[0044]
[0045] As shown in Table 1, the aluminum alloy materials prepared in Examples 1-4 all exhibited excellent comprehensive mechanical properties. Specifically, when the Mg / Si ratio was controlled within the range of 0.9-1.0, the tensile strength, specified non-proportional elongation strength, and elongation after fracture of the prepared aluminum profiles were significantly superior to those of the comparative examples. Example 1 demonstrated the best performance, achieving a tensile strength of 285 MPa, a specified non-proportional elongation strength of 245 MPa, an elongation after fracture of 10.5%, and a Brinell hardness of 105 HBW. This was attributed to its reasonable alloy composition design and optimized preparation process parameters.
[0046] The homogenization treatment temperature and time in Comparative Example 3 were too low and too short, failing to effectively eliminate component segregation inside the ingot and affecting the subsequent aging strengthening effect. The solution treatment temperature in Comparative Example 4 was too low, resulting in insufficient solution and weakened precipitation strengthening effect. The above comparative results further verify the necessity and superiority of the synergistic effect of each process step and parameter in the technical solution of this invention.
[0047] The aluminum alloy profile obtained in Example 1 of this invention is a hollow profile with a wall thickness of ≤ mm, specifically 4 mm. The aluminum alloy profile is machined into a drone base bracket. After testing, the base bracket has excellent lightweight and high strength characteristics, which can meet the dual requirements of drones for lightweight and high strength of structural components.
[0048] In summary, this invention optimizes the chemical composition of aluminum alloys (especially controlling the mass ratio of Mg to Si within the range of 0.9 to 1.0) and combines it with specific smelting, refining, semi-continuous casting, homogenization treatment, extrusion forming and T6 heat treatment processes to obtain a lightweight aluminum alloy material with both high strength and high elongation, which is particularly suitable for the manufacture of thin-walled structural components such as UAV base brackets.
[0049] The above embodiments are only for illustrating the technical concept and features of the present invention. Their purpose is to enable those skilled in the art to understand the content of the present invention and implement it accordingly. They should not be used to limit the scope of protection of the present invention. All equivalent changes or modifications made in accordance with the spirit and essence of the present invention should be covered within the scope of protection of the present invention.
Claims
1. A method for producing a lightweight high-strength aluminum alloy profile, characterized by, The lightweight, high-strength aluminum alloy profiles, by weight percentage, have the following chemical composition: Si 0.7%~0.85%; Fe≤0.25%; Cu≤0.08%; Mn≤0.08%; Mg 0.7%~0.8%; Cr≤0.07%; Zn≤0.06%; Ti≤0.09%; the balance being Al and unavoidable impurities. The preparation method includes the following steps: S1. Smelting: Prepare the ingredients according to the chemical composition described above. Heat the aluminum ingot to 730℃~780℃ to melt it. First, add the intermediate alloy containing Si, Mg, Cr and Ti in sequence, and then add the remaining chemical components. After it is completely melted, stir it thoroughly. S2. Refining: Argon or nitrogen gas is introduced into the aluminum alloy melt for refining and degassing. The refining temperature is 720℃~750℃ and the refining time is 10~30 minutes. After refining, the mixture is allowed to stand and slag is removed. S3. Casting: Semi-continuous casting is used for casting. The casting temperature is 680℃~720℃, the casting speed is 50~150mm / min, and the cooling water temperature is 15℃~35℃. S4. Homogenization treatment: The aluminum alloy ingots obtained by casting are kept at 540℃~580℃ for 6~12 hours for homogenization treatment, and then cooled in the furnace or air-cooled to room temperature. S5. Extrusion forming: The homogenized aluminum alloy ingot is heated to 450℃~520℃ for extrusion forming, and then cooled immediately after extrusion. S6 and T6 heat treatment: solution treatment temperature 515℃~540℃, hold for 2~6 hours, water quench to below 60℃, then perform artificial aging treatment at 170℃~185℃ for 4~12 hours.
2. The method of producing a light-weight high-strength aluminum alloy sectional material according to claim 1, characterized by, The mass ratio of Mg to Si in the aluminum alloy material is 0.94~1.
3. The method of producing a light weight high strength aluminum alloy profile according to claim 1 or 2, characterized in that, After T6 heat treatment, the aluminum alloy material has a tensile strength ≥255MPa, a yield strength ≥215MPa, and an elongation ≥7%.
4. The method of producing a light-weight high-strength aluminum alloy sectional material according to claim 1, characterized by, In the T6 heat treatment step, the artificial aging adopts a two-stage aging process: first, it is held at 170℃ for 2 hours, and then held at 180℃ for 1.5 hours.
5. The method of producing a light-weight high-strength aluminum alloy profile according to claim 1, characterized by, In the extrusion forming step, the extrusion is either forward extrusion or reverse extrusion, the extrusion speed is 2.0 to 3.0 mm / s, the extrusion cylinder temperature is 495℃ to 505℃, and the extrusion die temperature is 445℃ to 455℃.
6. The method of producing a light-weight high-strength aluminum alloy sectional material according to claim 1, characterized by In the extrusion forming step, the temperature of the extruded profile when it exits the die is not lower than 520°C.
7. The method for preparing lightweight high-strength aluminum alloy profiles according to claim 1, characterized in that, The cooling method is water mist cooling, which adopts an annular spray with air atomizing nozzles. The distance between the nozzle and the profile is 120mm-155mm, and the water flow rate of a single nozzle is >3L / min.
8. A drone base bracket, characterized in that, It is made by machining an aluminum alloy profile obtained by any one of the preparation methods described in claims 1 to 7, wherein the aluminum alloy profile is a hollow profile and its wall thickness is ≤5mm.