A high-strength, high-thermal-stability copper alloy with a dual nanostructure, its preparation method, and its applications.
Copper alloys were prepared by high-energy ball milling and discharge plasma sintering, which solved the contradiction between the strength and thermal stability of copper alloys and achieved high-strength, high-thermal-stability and good electrical conductivity copper alloys, suitable for high-performance conductive and thermally conductive structural components.
Patent Information
- Application Number
- CN202611627514.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies cannot simultaneously achieve high strength, thermal stability, and electrical conductivity in copper alloys. Traditional methods are complex and costly, making them unsuitable for large-scale industrial production.
Copper powder and tantalum hydride powder were ball-milled in an argon atmosphere to form nano-TaH/Cu composite powder, which was then sintered at high temperature and pressure in a discharge plasma sintering furnace to form uniformly distributed Ta2H, Ta2O5, TaO and Ta dispersion phases in a copper nanocrystalline matrix, combined with coherent nanotwins and 9R phase.
A copper alloy with high strength, high thermal stability and good electrical conductivity was prepared. The room temperature tensile strength reached 1.1 GPa and the softening temperature was higher than 1050 ℃, making it suitable for high-performance conductive and thermally conductive structural components.
Smart Images

Figure CN123108346A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-strength and heat-resistant copper alloy preparation technology, specifically relating to a dual-nanostructure high-strength and high-thermal-stability copper alloy, its preparation method, and its application. Background Technology
[0002] Copper and copper alloys are widely used in electronics, electrical engineering, and nuclear fusion due to their excellent thermal and electrical conductivity and good mechanical properties. However, there is a contradictory relationship between the strength, thermal stability, and thermal and electrical conductivity of copper alloys. For example, nanocrystalline copper and copper alloys prepared by large plastic deformation have high strength, but their grains exhibit intrinsic instability and tend to coarsen at high temperatures. Precipitation-strengthened copper alloys, such as Cu-Cr-Zr, Cu-Fe-P, and Cu-Ni-Si, exhibit high strength due to the in-situ formation of nanoscale dispersed phases; however, the precipitated phases coarsen or dissolve at high temperatures, resulting in a significant decrease in strength.
[0003] Introducing thermally stable particles, such as oxides (Al₂O₃, Y₂O₃), carbides (C, WC, SiC), and refractory metals (W, Ta, Nb), into a copper matrix can significantly improve the material's thermal stability. Simultaneously, the dispersed nanoparticles introduce numerous phase interfaces, which can act as radiation defect traps, enhancing the material's radiation resistance.
[0004] For dispersion-strengthened alloys, their properties are closely related to the size, number density, and distribution of the dispersed phase. Ideally, the number density of the dispersed phase should be greater than 10. 23 / m 3 The particles are smaller than 10 nm, uniformly dispersed, and have a coherent or semi-coherent orientation relationship with the matrix. However, due to the thermodynamic instability of nanoparticles and their tendency to aggregate at high temperatures, it is difficult to simultaneously achieve the above characteristics.
[0005] Traditional wet chemical methods can introduce uniform, fine, and high-number-density nano-dispersed phases, but this process is complex and costly, making it unsuitable for industrial production. Mechanical alloying, relying on high-energy impact, can also achieve high-number-density nano-dispersed phase dispersion. For brittle dispersed phases, Kadarling et al. used high-energy liquid nitrogen ball milling to prepare Cu-Ta alloys, where the average particle size of Ta clusters was only 3.18 nm, the average particle size of Ta particles was 32 nm, and the alloy tensile strength was close to 800 MPa. However, due to the harsh cryogenic conditions of liquid nitrogen, this process can only produce 10 g of powder per ball milling, which is also unsuitable for large-scale industrial applications.
[0006] Furthermore, some studies have indicated that high-energy ball milling, sintering, and deformation of copper powder and tantalum powder of different sizes can yield bimodal grain structure tantalum particle-reinforced copper composites. These composites exhibit tensile strengths exceeding 400 MPa and softening temperatures exceeding 650 °C. However, due to the good toughness of tantalum, the particle size is difficult to break down to below 10 nm during ball milling, which inhibits the strengthening and pinning effects of tantalum. Therefore, there is still significant room for improvement in the tensile strength and softening temperature of these composites. Other studies have shown that hydrides possess a certain degree of brittleness. Using hydrides as raw materials and ball milling them together with an oxidant, in-situ redox reactions can prepare metal oxide dispersion-reinforced copper alloys. However, the average size of the oxides is between 10-50 nm, and the highest tensile strength of the alloy is only 342 MPa. Studies have shown that tantalum hydride can improve the mechanical properties of sintered parts. By mixing tantalum hydride powder with metal powder through ordinary ball milling, tantalum hydride can decompose into hydrogen gas and active tantalum during hot pressing sintering. The high-temperature volatilization of hydrogen is conducive to the formation of sintered necks with good performance. At the same time, active tantalum can form compounds. However, the particle size of tantalum in the product is difficult to refine to the nanoscale, and it is also difficult to disperse evenly in copper crystals and on grain boundaries, resulting in low tensile strength of the alloy.
[0007] It is essential to provide a simple and low-cost method and material for preparing high-strength and high-thermal-stability copper alloys. Summary of the Invention
[0008] To address the aforementioned technical problems, this invention first provides a method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure.
[0009] The present invention employs the following technical means: A method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure includes the following steps: S1. Add copper powder and tantalum hydride powder to a hard ball milling jar according to a set ratio, add ethanol, and perform high-energy ball milling using hard alloy balls in an argon atmosphere to obtain nano-TaH / Cu composite powder; S2. The TaH / Cu composite powder is dried and then sintered under high temperature and pressure in a discharge plasma sintering furnace under vacuum or argon atmosphere. The sintering temperature is 800~950 ℃, the sintering pressure is 35~50 MPa, and the sintering time is 5~30 min. After sintering, the powder is cooled to room temperature to obtain the desired copper alloy.
[0010] In the TaH / Cu composite powder, TaH and Cu are intercalated, with TaH embedded inside copper nanocrystals.
[0011] Preferably, the average particle size of the copper powder and tantalum hydride powder is 1 μm, and the atomic ratio of the copper powder to the tantalum hydride powder is 95:5 to 99:1; the ethanol concentration is ≥99.5%, and the amount of ethanol used is 2 to 5 wt.% of the total mass of the copper powder and tantalum hydride powder.
[0012] Preferably, the diameter of the cemented carbide ball is 1 to 5 mm, the material is WC or TiC, and the weight of the cemented carbide ball is 10 times the total weight of the copper powder and tantalum hydride powder.
[0013] Preferably, the ball milling speed is 300~350 r / min and the ball milling time is 25~40 h.
[0014] Preferably, the drying process is performed by drying at 70-90 °C for 7-12 h in a vacuum environment.
[0015] Preferably, the heating rate of the high-temperature pressure sintering is 70~120 ℃ / min, and the cooling rate is 80~130 ℃ / min.
[0016] The present invention further provides a copper alloy with a dual nanostructure, which is a high-strength and high-thermal-stability copper alloy prepared by the preparation method described above.
[0017] Preferably, the copper alloy comprises a copper nanocrystalline matrix and a dispersed phase uniformly dispersed within the copper nanocrystalline grains and at the grain boundaries. The dispersed phase comprises Ta2H, Ta2O5, TaO, and Ta, wherein the volume fractions of Ta2H, Ta2O5, TaO, and Ta in the dispersed phase are 98-99%, 0.5-1.5%, 0.3-1.3%, and 0.2-1.2%, respectively.
[0018] Preferably, the copper nanocrystalline matrix also contains coherent nanotwins and a 9R phase.
[0019] It should be emphasized that since the distribution of coherent nanotwins and 9R phase is random and the amount generated is extremely small, the present invention does not make specific limitations on the ratio or distribution of the two. The presence of coherent nanotwins and 9R phase can bring some gains to the alloy properties. Even if the coherent nanotwins and 9R phase are not present, it does not affect the implementation of the basic technical solution of the present invention.
[0020] Preferably, in the copper alloy, the copper grain size is 50~200 nm, and the average particle size of the Ta2H particles is 4~5 nm.
[0021] This invention also provides the application of the above-mentioned dual-nanostructure high-strength and high-thermal-stability copper alloy in the preparation of high-performance conductive and thermally conductive structural components such as fusion reactor heat sink materials, continuous casting crystallizers, new energy vehicle connectors, and integrated circuit lead frames.
[0022] The beneficial effects of this invention are as follows: 1) This application provides a novel method for preparing dispersed phase copper alloys. First, copper powder, tantalum hydride powder, and alcohol are mixed in a specific ratio and then subjected to high-energy ball milling at room temperature under argon protection. Utilizing the high brittleness of TaH (TaH), it is refined to the nanoscale during high-energy ball milling and uniformly embedded within copper nanocrystals, forming a TaH / Cu intercalated composite powder. Then, sintering is performed. During spark plasma sintering, the physical encapsulation by copper effectively suppresses the dehydrogenation reaction of tantalum hydride. During this process, TaH undergoes a phase transformation, mainly converting to Ta2H and small amounts of Ta2O5, TaO, and Ta. Because Ta2H forms a low-interfacial-energy coherent interface with copper, Ta2H exhibits high thermal stability. The high-density grain boundaries and phase boundaries formed within the alloy effectively hinder dislocation movement, while the high-density dispersed particles strongly pin the grain boundaries, significantly improving the mechanical strength and thermal stability of the copper alloy. Compared to the complex liquid nitrogen high-energy ball milling method, this invention is simple, efficient, and requires no oxidant, making it suitable for large-scale industrial production.
[0023] 2) Microstructure characterization revealed that the dispersed phase-reinforced copper alloy prepared according to the method of this invention contains four dispersed phases: Ta₂H, Ta₂O₅, TaO, and Ta. Due to the presence of the TaH / Cu intercalation structure, only a small amount of TaH on the surface of the copper nanocrystals easily desorbs to form Ta, which then combines with O to form Ta₂O₅ and TaO. Therefore, the majority of the dispersed phases are Ta₂H. The average particle size of all four dispersed phases is less than 5 nm, and they are uniformly distributed within the copper nanocrystal grains and at the grain boundaries. All four phases refine the grains, pin grain boundaries, and impede dislocation movement, thereby improving the tensile strength and thermal stability of the alloy. Furthermore, the rapid heating and cooling rates during spark plasma sintering, combined with the localized distorted stress field induced by the introduction of nanoparticles, promote the emission of partial dislocations and the accumulation of stacking faults during sintering. This results in the presence of a small amount of beneficial coherent nanotwins and the 9R phase in the alloy microstructure. Coherent nanotwins effectively impede dislocation movement, providing material strength. Simultaneously, coherent nanotwins have low interfacial energy, which improves the thermal stability of the material. The 9R phase can also hinder dislocation movement, thereby improving the material's strength. Performance testing shows that the room temperature tensile strength of this dual-nanostructured tantalum hydride dispersion-strengthened copper alloy provided by this invention reaches 1.1 GPa. Simultaneously, the alloy exhibits extremely high resistance to high-temperature softening; after annealing at 1050 °C for 1 h, the alloy still retains 85% of its strength, and its softening temperature is higher than 1050 °C. Furthermore, the dual-nanostructured tantalum hydride dispersion-strengthened copper alloy of this invention also possesses good electrical conductivity, showing broad application prospects in electronics, electrical engineering, and nuclear fusion. Attached Figure Description
[0024] Figure 1The image shows a scanning electron microscope (SEM) image of the composite powder prepared in Example 1. In the image, (a) shows the morphology of the Cu-TaH composite powder after high-energy ball milling, (b) shows the copper element distribution in the corresponding region, and (c) shows the tantalum element distribution in the corresponding region.
[0025] Figure 2 The X-ray diffraction results of the copper alloy prepared in Example 1 are shown in the figure. (a) is the X-ray diffraction result of the composite powder, and (b) is the X-ray diffraction result of the sintered copper alloy.
[0026] Figure 3 The transmission Kikuchi diffraction results of the copper alloy prepared in Example 1 are shown in the figure. (a) is the inverse pole figure and (b) is the grain size frequency statistics of copper nanocrystals.
[0027] Figure 4 The figures show the microstructure characteristics and particle size statistics of the dispersed phase of the copper alloy prepared in Example 1. In the figure, (a) is a transmission electron microscope (TEM) image of the copper alloy matrix, (b) is an enlarged view of region A in (a), (c) is an enlarged view of region B in (a), (d) is an enlarged view of region C in (a), showing the 9R phase structure, and (e) is the size statistics of the dispersed phase.
[0028] Figure 5 The mechanical property test results are for the copper alloy prepared in Example 1.
[0029] Figure 6 The X-ray diffraction results are for the copper alloy prepared in Example 1 after high-temperature annealing.
[0030] Figure 7 The X-ray diffraction results are for the copper alloy prepared in Example 2.
[0031] Figure 8 The X-ray diffraction results are for the copper alloy prepared in Example 3. Detailed Implementation
[0032] Unless otherwise stated, the terms used herein have the meanings commonly understood by those skilled in the art. Unless otherwise specified, all experimental materials and reagents used in the experiments are commercially available. For experiments where specific techniques or conditions are not specified, the procedures described in the literature in this field or the product instructions should be followed.
[0033] The technical solution of the present invention will be described in more detail below with reference to the embodiments.
[0034] Example 1 A method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure includes the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm) and tantalum hydride powder (average particle size 1 μm) in sequence. The copper powder and tantalum hydride powder are weighed according to a copper to tantalum hydride atomic ratio of 95:5, and the total powder weight is weighed according to a ratio of 10:1 to the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then purge the jar with argon gas as a protective gas. At room temperature, place the jar in a ball mill, set the rotation speed to 350 r / min, and ball mill for 30 h for high-energy ball milling. The composite powder is obtained after ball milling.
[0035] Figure 1 The image shows a scanning electron microscope (SEM) image of the composite powder. After high-energy impact crushing, the particle size of TaH can be as small as nanometers. It can be seen that TaH is embedded in Cu crystals and has an intercalation structure, which is referred to as TaH / Cu composite powder.
[0036] S2. The TaH / Cu composite powder was dried in a vacuum drying oven at 70℃ for 7 hours. After drying, it was transferred to a graphite mold and sintered in a discharge plasma sintering furnace at an argon atmosphere and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at a rate of 100℃ / min, held for 5 minutes, and then decreased to room temperature at a rate of 100℃ / min to obtain the desired copper alloy.
[0037] Figure 2 The figures show the X-ray diffraction results. Figure (a) shows the X-ray diffraction results of the composite powder, and figure (b) shows the X-ray diffraction results of the sintered copper alloy. It can be seen that after discharge plasma sintering, TaH undergoes a phase transformation to Ta2H, Ta2O5, TaO, and Ta. The X-ray diffraction pattern was refined using the Rietveld full-spectrum fitting refinement method. The volume fractions of the four dispersed phases in the total dispersed phase were 99%, 0.5%, 0.3%, and 0.2%, respectively, with the majority being Ta2H.
[0038] Figure 3 The figures show the transmission Kikuchi diffraction results of the copper alloy. Figure (a) is the inverse pole figure, and (b) is the statistical result of grain size frequency. Different colors in (a) represent uniform grain orientation distribution. The uniform color distribution indicates that the prepared copper alloy exhibits an equiaxed crystal structure with an average grain size of only 89.7 nm, which belongs to nanocrystals.
[0039] Figure 4Figure 1 shows the microstructure characteristics of the copper alloy and the statistical results of the particle size of the dispersed phase. Figures (a)-(d) are transmission electron microscopy (TEM) images, and (e) shows the statistical results of the particle size of the dispersed phase. It can be seen that the alloy not only contains a dispersed second phase, but also coherent nanotwins and a 9R phase structure. Both structures belong to the ordered defect structures formed by the rearrangement of close-packed planes in the FCC matrix (Face-Centered Cubic).
[0040] Specifically, as can be seen from (a), a large number of fine precipitates are distributed in the copper alloy matrix. Regions A, B, and C in (a) correspond to the three figures in (b)-(d). As can be seen from (b), nano-precipitates are dispersed in the copper matrix. As can be seen from (c), the symmetrical coherent relationship of the lattices on both sides of the twin boundary is evident. The twin boundary is straight and has no obvious defects. The red box in (d) shows the 9R phase, and the periodic stripes correspond to the 9R stacking structure. In addition, the average particle size of the dispersed phase is only 4.3 nm.
[0041] The copper alloy was subjected to performance tests. Tensile strength was tested according to GB / T 228.1-2010 "Metallic Materials - Tensile Testing - Part 1: Tests at Room Temperature". Before tensile testing, the sample surface and sides were sanded. The softening temperature test was conducted according to GB / T 33370-2016 "Determination of Softening Temperature of Copper and Copper Alloys". The copper alloy was annealed at 700–1200 ℃ under an argon atmosphere for 1 hour, and then the sample surface was polished to a mirror finish. The hardness of the alloy after annealing was measured; the temperature at which the hardness decreased to 80% of the sintered state hardness value was defined as the softening temperature. Electrical conductivity was measured using an eddy current metal conductivity meter. Figure 5 As shown, the prepared copper alloy exhibits a room temperature tensile strength of 1115 MPa, a tensile strength of 1054 MPa after annealing at 900 °C for 1 h, and a tensile strength of 942 MPa after annealing at 1050 °C for 1 h. Furthermore, the alloy demonstrates excellent thermal stability with a softening temperature reaching 1050 °C. The X-ray diffraction results of the alloy after annealing at 1050 °C for 1 h are shown below. Figure 6 As shown, a large amount of Ta2H phase still exists in the alloy, with Ta2H, Ta2O5, TaO and Ta accounting for 99%, 0.6%, 0.35% and 0.05% of the total dispersed phase volume fractions, respectively. In addition, the dual nanostructured tantalum hydride reinforced copper alloy of this embodiment also has good electrical conductivity, with a room temperature conductivity of 51.2% IACS.
[0042] Example 2 A method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure includes the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm) and tantalum hydride powder (average particle size 1 μm) in sequence. The copper powder and tantalum hydride powder are weighed according to a copper to tantalum hydride atomic ratio of 95:5, and the total powder weight is weighed according to a ratio of 10:1 to the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then purge the jar with argon gas as a protective gas. At room temperature, place the jar in a ball mill, set the rotation speed to 350 r / min, and ball mill for 30 h for high-energy ball milling. After ball milling, TaH / Cu composite powder is obtained.
[0043] S2. The TaH / Cu composite powder was dried in a vacuum drying oven at 70℃ for 7 hours. After drying, it was transferred to a graphite mold and vacuum sintered in a discharge plasma sintering furnace at a vacuum degree of 5 Pa and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at 100℃ / min, held for 5 min, and then decreased to room temperature at 100℃ / min to obtain the desired copper alloy.
[0044] The X-ray diffraction of the copper alloy prepared in Example 2 is as follows: Figure 7 As shown, the copper alloy contains four phases in addition to the Cu matrix: Ta₂H, Ta₂O₅, TaO, and Ta, accounting for 99.1%, 0.6%, 0.1%, and 0.2% of the total dispersed phases, respectively. Performance testing revealed that the prepared copper alloy exhibits a room temperature tensile strength of 1073 MPa and a softening temperature of 1020 ℃.
[0045] Example 3 A method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure includes the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm) and tantalum hydride powder (average particle size 1 μm) in sequence. The copper powder and tantalum hydride powder are weighed according to a copper to tantalum hydride atomic ratio of 95:5, and the total powder weight is weighed according to a ratio of 10:1 to the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then purge the jar with argon gas as a protective gas. At room temperature, place the jar in a ball mill, set the rotation speed to 350 r / min, and ball mill for 30 h for high-energy ball milling. After ball milling, TaH / Cu composite powder is obtained.
[0046] S2. The TaH / Cu composite powder was dried in a vacuum drying oven at 80℃ for 5 hours. After drying, it was transferred to a graphite mold and sintered in a discharge plasma sintering furnace at an argon atmosphere and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at 100℃ / min, held for 30 min, and then decreased to room temperature at 100℃ / min to obtain the desired copper alloy.
[0047] The X-ray diffraction results of the copper alloy prepared in Example 3 are as follows: Figure 8 As shown, the copper alloy contains four phases in addition to the Cu matrix: Ta₂H, Ta₂O₅, TaO, and Ta. These four phases account for 99.1%, 0.5%, 0.3%, and 0.1% of the total dispersed phase volume, respectively. Performance testing revealed that the prepared copper alloy exhibits a room temperature tensile strength of 953 MPa and a softening temperature of 990 ℃.
[0048] Comparative Example 1 A method for preparing a copper alloy, comprising the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm) and tantalum powder (average particle size 1 μm) sequentially. The copper powder and tantalum powder are weighed according to a copper to tantalum atomic ratio of 95:5, and the total weight of the powder is weighed according to a ratio of 10:1 to the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then fill the ball milling jar with argon gas as a protective gas. At room temperature, place the ball milling jar in a ball mill, set the rotation speed to 350 r / min, and ball mill for 30 h for high-energy ball milling. After ball milling, Cu-Ta composite powder is obtained.
[0049] S2. The Cu-Ta composite powder was dried in a vacuum drying oven at 70℃ for 7 hours. After drying, it was transferred to a graphite mold and sintered in a discharge plasma sintering furnace at an argon atmosphere and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at 100℃ / min, held for 5 minutes, and then decreased to room temperature at 100℃ / min to obtain the desired copper alloy.
[0050] X-ray diffraction revealed that the copper alloy prepared in this comparative example contained a large amount of Ta and a small amount of Ta₂O₅ in addition to the Cu matrix. This was attributed to the direct addition of tantalum powder with strong oxygen affinity during ball milling. Performance tests showed that the copper alloy had a room temperature tensile strength of 600 MPa and a softening temperature of 900 ℃. Due to the high toughness of tantalum, conventional room temperature ball milling is insufficient to refine it to below 10 nm. This nanoscale size bottleneck directly restricts the high-density dispersion of tantalum particles in the matrix, thereby weakening its dislocation-hinding and pinning effects.
[0051] Comparative Example 2 A method for preparing a copper alloy, comprising the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm), tantalum hydride powder (average particle size 1 μm), and copper oxide powder (average particle size 1 μm) in sequence. The copper powder, tantalum hydride powder, and copper oxide powder are weighed and added in an atomic ratio of 80:5:15, and the total weight of the powder is weighed according to a 10:1 ratio with the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then purge the jar with argon gas as a protective gas. At room temperature, place the jar in a ball mill, set the rotation speed to 350 r / min, and ball mill for 30 h for high-energy ball milling. After ball milling, Cu-Ta2O5 composite powder is obtained.
[0052] S2. The Cu-Ta2O5 composite powder was dried in a vacuum drying oven at 70℃ for 7 hours. After drying, it was transferred to a graphite mold and sintered in a discharge plasma sintering furnace at an argon atmosphere and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at 100℃ / min, held for 5 minutes, and then decreased to room temperature at 100℃ / min to obtain the desired copper alloy.
[0053] Testing revealed that the copper alloy prepared in Comparative Example 2 consisted only of the matrix Cu and Ta2O5 phases; the alloy exhibited a room temperature tensile strength of 300 MPa and a softening temperature of 850 ℃. It is speculated that the intense exothermic reaction accompanying the in-situ oxidation accelerates local atomic diffusion, driving significant coarsening and agglomeration of the nascent Ta2O5 particles, thus weakening the dislocation-hinding and pinning effects of the Ta2O5 particles.
[0054] Comparative Example 3 A method for preparing a copper alloy, comprising the following steps: S1. First, add cemented carbide balls to the cemented carbide ball milling jar, then add copper powder (average particle size 1 μm) and tantalum hydride powder (average particle size 1 μm) in sequence. The copper powder and tantalum hydride powder are weighed according to a copper to tantalum hydride atomic ratio of 95:5, and the total powder weight is weighed according to a ratio of 10:1 to the cemented carbide balls. Add 5% (99.5% by volume) of alcohol to the cemented carbide ball milling jar, and then purge the jar with argon gas as a protective gas. At room temperature, place the jar in a ball mill, set the rotation speed to 100 r / min, and mill for 4 h. The composite powder is obtained after milling.
[0055] Tests showed that the composite powder did not form an intercalation structure and was a Cu-TaH composite powder. Ball milling did not cause tantalum hydride to undergo a phase transformation and it remained TaH. Furthermore, the average particle size of TaH did not become significantly finer and remained around 1 μm.
[0056] S2. The Cu-TaH composite powder was dried in a vacuum drying oven at 70℃ for 7 hours. After drying, it was transferred to a graphite mold and sintered in a discharge plasma sintering furnace at an argon atmosphere and a sintering pressure of 50 MPa. The temperature was increased to 950℃ at 100℃ / min, held for 5 minutes, and then decreased to room temperature at 100℃ / min to obtain the desired copper alloy.
[0057] Testing revealed that the copper alloy prepared in Comparative Example 3 consisted of a Cu matrix, a large amount of Ta, and a small amount of Ta₂O₅. The alloy exhibited a room temperature tensile strength of 300 MPa and a softening temperature of 650 °C. Conventional ball milling, with its low energy and short time, was insufficient to reduce the average particle size of TaH particles to below 10 nm. Furthermore, because the TaH particles were not integrated into the copper particles, complete hydrogen desorption and transformation into Ta occurred during sintering, ultimately resulting in coarse Ta particles with low number density within the copper matrix. These particles exhibited poor dislocation hindering and pinning effects, leading to inferior final material properties.
[0058] As can be seen from the above embodiments and comparative examples, this invention prepares a copper alloy with ultra-high strength, high structural thermal stability, high softening temperature resistance, and good electrical conductivity by introducing a specific dispersed phase into the copper matrix. This method utilizes the intrinsic brittleness of tantalum hydride, combined with the high energy input of high-energy ball milling, to form TaH / Cu intercalated powder through ball milling at room temperature. This powder is then sintered using discharge plasma under vacuum or argon atmosphere to achieve uniform dispersion of ultra-nano particles (less than 5 nm) in nanocrystalline copper, forming a specific double-nano structure. This results in a high density of ultra-nano particles pinning grain boundaries and hindering dislocations in the alloy. The prepared alloy exhibits performance far exceeding that of existing copper-tantalum alloys and has significant potential for widespread application.
[0059] The above are merely preferred embodiments of the present invention and are not intended to limit the scope of the invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A method for preparing a high-strength, high-thermal-stability copper alloy with a dual-nanostructure, characterized in that, Includes the following steps: S1. Add copper powder and tantalum hydride powder to a hard ball milling jar according to a set ratio, add ethanol, and perform high-energy ball milling using hard alloy balls in an argon atmosphere to obtain nano-TaH / Cu composite powder; S2. The TaH / Cu composite powder is dried and then sintered under high temperature and pressure in a discharge plasma sintering furnace under vacuum or argon atmosphere. The sintering temperature is 800~950 ℃, the sintering pressure is 35~50 MPa, and the sintering time is 5~30 min. After sintering, the temperature is lowered to room temperature to obtain the desired copper alloy.
2. The method for preparing a high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 1, characterized in that, The average particle size of the copper powder and tantalum hydride powder is 1 μm, and the atomic ratio of the copper powder and tantalum hydride powder is 95:5~99:1; the volume fraction of the ethanol is ≥99.5%, and the amount of ethanol used is 2~5 wt.% of the total mass of the copper powder and tantalum hydride powder.
3. The method for preparing a high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 1, characterized in that, The diameter of the cemented carbide ball is 1-5 mm, the material is WC or TiC, and the weight of the cemented carbide ball is 10 times the total weight of the copper powder and tantalum hydride powder.
4. The method for preparing a high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 1, characterized in that, The ball milling speed is 300~350 r / min, and the ball milling time is 25~40 h.
5. The method for preparing a high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 1, characterized in that, The drying process involves drying at 70-90 °C for 7-12 h in a vacuum environment.
6. The method for preparing a high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 1, characterized in that, The heating rate of the high-temperature pressure sintering is 70~120 ℃ / min, and the cooling rate is 80~130 ℃ / min.
7. A high-strength, high-thermal-stability copper alloy with a dual nanostructure, characterized in that, It is prepared by the preparation method described in any one of claims 1-6.
8. The high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 7, characterized in that, The copper alloy comprises a copper nanocrystalline matrix and a dispersed phase uniformly dispersed within the copper nanocrystalline grains and at the grain boundaries; the dispersed phase comprises Ta2H, Ta2O5, TaO and Ta, wherein the volume fractions of Ta2H, Ta2O5, TaO and Ta in the dispersed phase are 98~99%, 0.5~1.5%, 0.3~1.3% and 0.2~1.2%, respectively.
9. The high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in claim 8, characterized in that, The copper nanocrystalline matrix also contains coherent nanotwins and a 9R phase.
10. A high-strength, high-thermal-stability copper alloy with a dual nanostructure as described in any one of claims 7-9, characterized in that, In the copper alloy, the copper grain size is 50~200 nm, and the average particle size of Ta2H particles is 4~5 nm.