A thin, high-density, high-temperature resistant aluminum alloy platter for hard disk drives and its preparation method.

By controlling the chemical composition and manufacturing process of aluminum alloy platters, the problem of insufficient structural stability of aluminum alloy platters under high temperature conditions has been solved, improving their strength and the adhesion of the magnetic coating, making them suitable for thin, high-density storage hard drives.

CN123108366APending Publication Date: 2026-11-17CHINALCO RUIMIN CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611390240.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing aluminum alloy platters lack structural stability under high-temperature conditions, leading to damage to the magnetic plating layer and failing to meet the thickness and strength requirements of thin, high-density storage hard drives.

Method used

By controlling the chemical composition and preparation process of aluminum alloys, including the proportion of alloying elements and heat treatment processes, aluminum alloy discs with high strength and uniform structure can be prepared, avoiding the shedding of intermetallic compounds and improving the adhesion and continuity of the magnetic coating.

Benefits of technology

It improves the structural stability and strength of aluminum alloy platters under high-temperature conditions, reduces surface defects, and is suitable for thin, high-density storage hard drives.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108366A_ABST
    Figure CN123108366A_ABST
Patent Text Reader

Abstract

This invention provides a thin, high-density, high-temperature resistant aluminum alloy disk for hard disk drives and its preparation method. The aluminum disk preparation steps are as follows: melting, refining and filtering, casting, hot rolling, cold rolling, cleaning and straightening, slitting, stamping and blanking, flattening and annealing to obtain aluminum disk blanks with a thickness of 0.400~0.650mm, a diameter of 95.0~98.2mm, a surface flatness of <5μm, a surface hardness of ≥64HV after O-state annealing, an average grain size of ≤20μm, and an Al-Fe-Mn intermetallic compound size of ≤10μm, meeting the technical requirements for thin aluminum disks for hard disk drives.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of alloy technology, specifically relating to a thin, high-density, high-temperature resistant aluminum alloy disk for hard disk storage and its preparation method. Background Technology

[0002] With the development of hard drive technology and the continuous increase in storage density, the requirements for aluminum alloy platters are constantly increasing. The thickness of the aluminum substrate has been continuously reduced, from the initial 1.775mm to 1.3mm, 0.66mm, 0.623mm, 0.53mm, and currently down to 0.46mm. Simultaneously, to further increase storage density, a better material substrate is needed to prevent damage to the magnetic plating layer during high-temperature operation. Previous aluminum substrate materials, on the one hand, lacked sufficient strength to meet the requirements of thinner thickness, and on the other hand, lacked sufficient structural stability, leading to structural changes under high-temperature conditions that resulted in the destruction of the magnetic plating layer. To adapt to these changes, new alloys need to be developed to improve strength and microstructure, while maintaining the size of intermetallic compounds in the aluminum substrate to ≤10μm to prevent the formation of tiny pits after intermetallic compounds detach, which would affect the continuity of the magnetic plating. Summary of the Invention

[0003] The purpose of this invention is to provide a thin, high-density, high-temperature resistant aluminum alloy disk for hard disk storage and its preparation method.

[0004] To achieve the above objectives, the present invention adopts the following technical solution: A thin, high-density, high-temperature resistant aluminum alloy platter for hard drives, with the following chemical composition by mass percentage: Si ≤0.02%, Fe ≤0.02%, Fe / Si >1, Cu 0.005~0.02%, Mn 0.05~0.30%, Mg 3.7~4.3%, Cr 0.15~0.35%, Zn 0.2~0.4%, Ti <0.001%, and the content of other elements is <0.01% individually. Low Fe and Si content, and Fe / Si > 1, can avoid the formation of needle-like or plate-like β phases. If the Fe content exceeds 0.02%, coarse AlFe phases will be formed, which will deteriorate the magnetic plating performance.

[0005] Adding a small amount of Mn can form an easily broken α-phase (Al) with Fe and Si. 12 (MnFe)3Si), while Mn precipitates the AlMnSi phase during heating, which can refine the grains, hinder dislocation movement, and improve strength. However, if the added Mn content exceeds 0.30%, a coarse AlMn6 phase will form, and due to Mn segregation, the grains will be coarse, deteriorating the magnetic plating performance. Therefore, the Mn content is controlled at 0.05~0.30%. In aluminum alloys, Cr forms the AlCr phase, which is very stable at high temperatures. This phase can improve high-temperature strength and creep resistance, while also refining the grain size and improving the stability of the passivation film on the aluminum surface. However, excessively high Cr content can lead to the formation of coarse phases; therefore, the Cr content is controlled between 0.15% and 0.35%.

[0006] The Mg content is controlled at 3.7~4.3% to maintain a high solid solution strengthening effect, while avoiding the formation of too much Mg2Si phase, which would affect the plasticity and processing performance of the material.

[0007] Maintaining a Zn content of 0.2-0.4% can improve the quality of subsequent surface treatments.

[0008] Controlling the Cu content to 0.005~0.02% can refine the grains and improve the strength, while avoiding the formation of coarse Al2Cu phases that would affect the material's corrosion resistance. In addition, trace amounts of Cu can improve the material's chemical polishing properties.

[0009] The Ti content should be controlled below 0.001% to avoid the formation of hard inclusions such as TiC and TiN, which could scratch the surface of the board during polishing.

[0010] Through the synergistic control of the above components, the alloy maintains high strength while improving the uniformity and adhesion of the magnetic plating layer, reducing surface defects caused by the shedding of intermetallic compounds. Simultaneously, by strictly controlling the content and proportion of elements such as Fe, Si, Mn, Cr, Mg, Zn, Cu, and Ti, the formation of harmful phases is effectively suppressed, and the microstructure uniformity of the alloy is optimized. Furthermore, this invention also relates to a method for preparing the above-mentioned aluminum alloy, comprising the following steps: 1) The chemical composition of the aluminum alloy disc is designed as follows: Si ≤0.02%, Fe ≤0.02%, Fe / Si>1, Cu 0.005~0.02%, Mn<0.05~0.30%, Mg 3.7~4.3%, Cr 0.15~0.35%, Zn 0.2~0.4%, Ti<0.001%, and the content of other elements <0.01%; 2) Prepare materials according to the chemical composition in step 1), using high-purity aluminum ingots of 99.97% or higher for batching, with the proportion of scrap materials of the same grade being <20%; 3) Add the material from step 2) to the smelting furnace, ignite and smelt after adding the material, and the temperature of the molten aluminum should not exceed 760℃; 4) After refining and settling the molten aluminum from step 3), filter it using a tubular filter. 5) Cast the molten aluminum obtained in step 4) with the following parameters: casting temperature 680~700℃, casting speed 45~60mm / min, and without using grain refiner. 6) Heat the ingot produced in step 5) to 460~520℃, hold for 1~24 hours, and then hot roll; the final thickness of hot rolling is 3~7mm, and the final rolling temperature is 270~320℃; 7) The hot-rolled coil from step 6) is rolled to the finished thickness using a cold rolling mill, with a total cold rolling processing rate of 50-90%; 8) After cleaning and straightening, the cold-rolled coil from step 7) is slit; 9) The slit roll material obtained in step 8) is stamped into round sheets on a special equipment; 10) After cleaning the discs from step 9), flatten and anneal them at a temperature of 300~360℃ for 1-6 hours with a heating rate not exceeding 100℃ / hour. Then cool them down to below 200℃ and remove them from the furnace with a cooling rate not exceeding 100℃ / hour.

[0011] Based on the above-mentioned processing technology and research results, this invention has conducted extensive research on the adjustment of the composition of aluminum-based discs. The results show that after flattening and annealing, the aluminum-based discs undergo sufficient stress relief treatment, which promotes complete recrystallization of the material and significantly improves the mechanical properties of the material.

[0012] The advantages of this invention are: 1. The thin aluminum disc for hard disk drives prepared by the technology of this invention improves the mechanical properties of the material by adjusting Mn and Cr, and there are no Al-Fe-Mn intermetallic compounds with a size >10μm.

[0013] 2. The preparation steps of the present invention are simple and reasonable, and it is easy to achieve mass production in industry. This technology is generally applicable to aluminum wafer products for mechanical hard drives. Attached Figure Description

[0014] Figure 1 Example 1: Scanning electron microscopy was used to observe the distribution of Al-Fe-Mn intermetallic compounds on the surface of aluminum. Detailed Implementation

[0015] To make the above features and advantages of the present invention more apparent and understandable, specific embodiments are provided below for detailed description. Unless otherwise specified, the methods of the present invention are conventional methods in the art.

[0016] A pit-free surface control technology for aluminum wafers used in hard disk drives includes the following steps: 1) The chemical composition is as follows: Si≤0.02%, Fe≤0.02%, Fe / Si>1, Cu 0.005~0.02%, Mn<0.05~0.30%, Mg 3.7~4.3%, Cr 0.15~0.35%, Zn 0.2~0.4%, Ti<0.001%, and the content of other elements <0.01%.

[0017] 2) Prepare raw materials according to the stated chemical composition, using high-purity aluminum ingots with a purity of 99.97% or higher, with the proportion of scrap of the same grade <20%; add the raw materials to the smelting furnace for heating and smelting, controlling the temperature of the molten aluminum to not exceed 760℃; after refining and settling, the molten aluminum is filtered through a tubular filter; the filtered molten aluminum is then cast at a casting temperature of 680℃ and a casting speed of 45mm / min, without adding grain refiners during the casting process; heat the ingot to 460℃ and... The material is held at the heat for 3 hours, then hot-rolled to a final thickness of 3 mm at a final rolling temperature of 300℃. The hot-rolled coil is then cold-rolled to a finished thickness of 0.46 mm. After cleaning, straightening, and slitting, the cold-rolled coil is stamped into round blanks. The round blanks are then cleaned and flattened for annealing at a temperature of 340℃ for 2 hours. The heating rate is no higher than 100℃ / h. After holding, the material is cooled to below 200℃ and removed from the furnace at a cooling rate no higher than 100℃ / h.

[0018] 3) Following the production method of industrial aluminum sheets, cast ingots according to the above steps, and hot-rolled them into 3.0mm thick hot-rolled sheets. These were then cold-rolled to a thickness of 0.46mm. After O-state annealing, mechanical property analysis was performed. Small 20*20mm squares were then ground sequentially using 200, 400, 800, and 1600 grit sandpaper, with the grinding direction rotated periodically. The grinding machine speed was controlled between 150 and 500 rpm. Rough and fine polishing were then performed. The morphology and distribution of Al-Fe-Mn intermetallic compounds in the samples were observed using a JSM7800F field emission electron microscope in backscatter mode. Four images (total area approximately 1mm²) were taken at 200x magnification. 2 The distribution of Al-Fe-Mn intermetallic compounds on the aluminum surface was statistically analyzed using Olycia m3 metallographic analysis software using BSD images. The statistical results of the distribution of Al-Fe-Mn intermetallic compounds in the aluminum material in this invention are shown in Table 1. Example 1

[0019] Example 1: The chemical composition is as follows: Si 0.011%, Fe 0.014%, Cu 0.013%, Mn 0.13%, Mg 3.98%, Cr 0.211%, Zn 0.337%, Ti < 0.001%, and the content of other elements < 0.01%. The resulting aluminum material, after O-state annealing, has a hardness of 66.4 HV, the size of the Al-Fe-Mn intermetallic compound is ≤10 μm, the compound area accounts for 0.05%, and the average grain size is 14.6 μm.

[0020] Comparative Example 1 The chemical composition of Comparative Example 1 is as follows: Si 0.009%, Fe 0.013%, Cu 0.014%, Mn 0.38%, Mg 4.12%, Cr 0.198%, Zn 0.333%, Ti < 0.001%, and the content of the remaining elements is < 0.01%. The obtained aluminum material has a hardness of 68.1 HV after O-temper annealing, the size of Al-Fe-Mn intermetallic compounds is > 10 μm, the area fraction of the compounds is 0.15%, and the average grain size is 25.6 μm.

[0021] Comparative Example 2 The chemical composition of Comparative Example 2 is as follows: Si 0.009%, Fe 0.017%, Cu 0.014%, Mn 0.001%, Mg 4.10%, Cr 0.189%, Zn 0.342%, Ti < 0.001%, and the content of the remaining elements is < 0.01%. The obtained aluminum material has a hardness of 63.3 HV after O-temper annealing, the size of Al-Fe-Mn intermetallic compounds is ≤ 10 μm, the area fraction of the compounds is 0.02%, and the average grain size is 16.9 μm.

[0022] Table 1 Hardness of aluminum sheet and size and distribution of Al-Fe intermetallic compounds on the surface

[0023] Note: It is qualified when the maximum size of the second phase is ≤ 10 μm and the hardness is ≥ 64 HV; otherwise, it is unqualified.

[0024] Finally, it should be noted that the above-described examples are only preferred results of the present invention, are not intended to limit the present invention, and are only used to describe the present invention in detail. For those skilled in the art, they can still make modifications to the technical solutions described in the foregoing examples, or make equivalent replacements to some of the technical features. All modifications, equivalent replacements, improvements and the like made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thin, high-density, high-temperature resistant aluminum alloy platter for a hard disk drive, characterized in that, The chemical composition, by mass percentage, includes: Si ≤0.02%, Fe ≤0.02%, and Fe / Si >1; Cu 0.005~0.02%; Mn 0.05~0.30%; Mg 3.7~4.3%; Cr 0.15~0.35%; Zn 0.2~0.4%; Ti <0.001%; ​​and the content of other impurity elements is <0.01%; after O-state annealing, the aluminum alloy disk has a surface hardness ≥64HV, an average grain size ≤20μm, and a maximum size of Al-Fe-Mn intermetallic compounds ≤10μm; the disk thickness is 0.400~0.650mm, the diameter is 95.0~98.2mm, and the surface flatness is <5μm.

2. The aluminum alloy disc according to claim 1, characterized in that, The mass percentage of Fe element is 0.001% to 0.020%.

3. The aluminum alloy disc according to claim 1, characterized in that, The mass percentage of the Mn element is 0.05% to 0.300%.

4. The aluminum alloy disc according to claim 1, characterized in that, The mass percentage of Cr element is 0.15% to 0.35%.

5. The aluminum alloy disc according to claim 1, characterized in that, The mass percentage of Mg is 3.7% to 4.3%.

6. The aluminum alloy disc according to claim 1, characterized in that, The thickness tolerance of a single disk is ≤±3μm, and the diameter tolerance is ≤±0.1mm.

7. A method for preparing a thin, high-density, high-temperature resistant aluminum alloy platter for a hard disk drive as described in any one of claims 1-6, characterized in that, Includes the following steps: (1) Raw material preparation: Prepare raw materials according to the chemical composition, using high-purity aluminum ingots with a purity of 99.97% or higher, and the proportion of waste materials of the same grade is <20%; (2) Smelting: Add the raw materials to the smelting furnace and heat them to smelt, controlling the temperature of the molten aluminum to not exceed 760℃; (3) Refining and filtration: After refining and settling, the molten aluminum is filtered through a tubular filter. (4) Casting: The filtered molten aluminum is cast at a temperature of 680~700℃ and a casting speed of 45~60mm / min. No grain refiner is added during the casting process. (5) Hot rolling: Heat the ingot to 460~520℃ and hold for 1~24h, then hot roll it. The final rolling thickness is 3~7mm and the final rolling temperature is 270~320℃. (6) Cold rolling: The hot-rolled coil is cold-rolled to the finished thickness, and the total cold rolling processing rate is 50%~90%; (7) Post-processing and forming: After cleaning, straightening and slitting, the cold-rolled coil is stamped into round blanks; (8) Flattening annealing: After cleaning the round blank, flatten it and anneal it. The annealing temperature is 300~360℃ and the holding time is 1~6h. The heating rate is not higher than 100℃ / h. After the holding time is completed, the temperature is lowered to below 200℃ and the blank is removed from the furnace. The cooling rate is not higher than 100℃ / h.

8. The preparation method according to claim 7, characterized in that, The inner and outer burrs of the stamped circular blank are not higher than the sample surface, and the overall flatness is <5μm after flattening and annealing.

9. The preparation method according to claim 7, characterized in that, The flattening annealing process allows the material to recrystallize fully and eliminates internal stress, ultimately obtaining an aluminum alloy disc in the O-state annealed condition.

10. The preparation method according to claim 7, characterized in that, After surface grinding and polishing, the aluminum alloy discs produced are free of surface pits caused by the shedding of intermetallic compounds.