Self-limiting nanoporous austenitic stainless steel, its preparation method and application

By utilizing the spontaneous anodic dissolution of the AlN phase in dilute sulfuric acid solution to form a nanoporous structure in situ, the problems of high equipment cost, high environmental risk and interface failure in the preparation of existing nanoporous stainless steel are solved, realizing the preparation of zero-energy-consumption and environmentally friendly nanoporous austenitic stainless steel.

CN123108409APending Publication Date: 2026-11-17CHENGDU ADVANCED METAL MATERIALS IND TECH RES INST CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202611501947.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-24
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing nanoporous stainless steel preparation technologies rely on external energy, resulting in high equipment costs, significant environmental risks, and the risk of interface failure in multilayer structures. Furthermore, the process parameters are sensitive and complex, making it difficult to achieve zero-energy preparation.

Method used

By utilizing the natural electrode potential difference between the AlN precipitate in austenitic stainless steel containing nano-AlN phase and the stainless steel matrix, spontaneous anodic dissolution of the AlN phase is achieved in dilute sulfuric acid solution, forming a nanoporous structure in situ, thus preparing self-limiting nanoporous austenitic stainless steel.

Benefits of technology

It achieves zero-energy preparation without the need for external energy, simplifies the process, is environmentally friendly, and the porous layer is metallurgically bonded to the matrix, eliminating the risk of interface failure and reducing production costs and complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108409A_ABST
    Figure CN123108409A_ABST
Patent Text Reader

Abstract

This invention discloses a self-limiting nanoporous austenitic stainless steel, its preparation method, and its applications, belonging to the field of porous metal materials technology. To overcome the AlN defect in stainless steel and achieve spontaneous, zero-energy pore formation, this invention provides a method for preparing self-limiting nanoporous austenitic stainless steel. By internally controlling Al, and utilizing the natural electrode potential difference between the AlN precipitate phase in the austenitic stainless steel containing nano-AlN phase and the stainless steel matrix, spontaneous anodic dissolution of the AlN phase is achieved in a dilute sulfuric acid aqueous solution, thereby forming a nanoporous structure in situ on the stainless steel surface. This method achieves pore formation with zero energy consumption and without the need for an external power source, without damaging the mechanical properties of the matrix, resulting in an ultrathin nanoporous austenitic stainless steel. It can be used as a catalyst support and in fields such as microfiltration and ultrafiltration membranes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of porous metal materials technology, specifically relating to a self-limiting nanoporous austenitic stainless steel, its preparation method, and its application. Background Technology

[0002] Nanoporous stainless steel offers unique advantages as a catalyst support. Compared to ceramic supports, stainless steel supports exhibit better thermal conductivity, higher mechanical strength, and easier regeneration. Nanoporous stainless steel can also be used in the microfiltration / ultrafiltration membrane market, including petrochemical catalysts, environmental catalysts (VOC treatment, denitrification), and new energy catalysts (hydrogen production via water electrolysis). Compared to polymer membranes, metal membranes are more resistant to high temperatures and corrosion, and can be backwashed and regenerated. Currently, nanoporous stainless steel preparation technology is developing towards greater simplicity and cost-effectiveness, with mainstream preparation technologies including dealloying (LMD, VPD), anodizing, and additive manufacturing.

[0003] CN102268713A discloses a nanoporous array film on a stainless steel surface and its preparation method. The method involves using pre-treated stainless steel as the anode, placing it in a phosphate buffer solution (concentration 0.01~2 mol / L, pH 2~8) for electrochemical anodizing treatment. The treatment voltage is 10~80V, the temperature is -5~40℃, and the time is 0.1~4h, thereby obtaining a nanoporous array film on the stainless steel surface. The nanoporous array prepared by this method has advantages such as ordered structure, high density, controllable pore size and depth, and strong adhesion to the substrate.

[0004] CN106521604A discloses a method for preparing nanoporous structures on the surface of stainless steel and cobalt alloys. The method involves placing a pretreated sample in an electrolyte solution containing ammonium fluoride (0.075~1 mol / L), water, and ethylene glycol, and performing constant-voltage anodic oxidation at 0~30℃ and 5~60V. This process can prepare nanoporous structures with pore sizes ranging from 20~60 nm on the sample surface. This method has the advantages of simple equipment, convenient operation, and a relatively environmentally friendly electrolyte solution. The resulting porous structures have uniform pore sizes and stable performance, making it suitable for industrial production.

[0005] CN105268247B discloses a nanoscale porous metal filter medium and its preparation method. The medium employs a three-layer composite structure: a stainless steel microporous membrane with a pore size of 1-5 μm serves as the support, upon which a micron-sized metal powder transition layer (particle size 1-20 μm) and a nanoscale metal powder control layer (particle size 30-80 nm) are sequentially coated. The medium is then calcined at high temperature (600-1500℃) to form the filter. This filter medium exhibits advantages such as high filtration accuracy, good corrosion resistance, and good stability.

[0006] CN106825547B discloses an additive manufacturing method for porous metal materials by selectively laser melting a solution of mixed metal micro / nano particles in an air environment. The method involves mixing stainless steel micron-sized powder (average particle size approximately 46.85 wt%) with nano-metal powders (such as copper, gold, silver, titanium, nickel, etc., 17.56 wt%) in a dispersion solution containing polyvinylpyrrolidone (8.19 wt%). This mixture is then coated onto a stainless steel substrate. Selective laser melting is performed near a 40-micron laser spot, causing the metal powder and substrate to melt and connect, forming a porous structure. This method can be performed in an air environment, offering advantages such as low environmental requirements, low cost, high controllability, and low equipment requirements. Furthermore, the resulting structure exhibits uniformly distributed nanoparticles on its surface, possessing superhydrophilic and underwater superoleophobic properties.

[0007] Although the above methods have made progress in preparing nanoporous structures on stainless steel surfaces, the following technical limitations still exist: (1) They rely on external energy. The anodizing method (CN102268713A, CN106521604A) requires an external power supply to provide a driving voltage (10~80V) to promote the formation of nanoporous structures. The additive manufacturing method (CN106825547B) requires a dedicated laser device to provide a high-energy-density heat source. High-temperature calcination (CN105268247B) requires a high-temperature environment. This makes these preparation processes require sophisticated electrochemical equipment, laser systems, vacuum devices or high-temperature furnaces, increasing equipment investment and energy consumption costs. (2) The electrolyte / additive system poses environmental risks. CN106521604A uses an electrolyte solution containing ammonium fluoride. Although it claims to be "relatively environmentally friendly", fluoride ions still have certain corrosiveness and environmental risks, and the waste liquid treatment requirements are high. The preparation of the transition layer and control layer of CN105268247B requires the addition of organic additives such as polyvinyl alcohol, glycerol, and sodium alginate, and the calcination process may release organic decomposition products. (3) The multilayer structure has the risk of interface failure. CN105268247B adopts a three-layer composite structure of support-transition layer-control layer, and there are physical interfaces between the transition layer and control layer, and between the transition layer and support. Under long-term use or thermal cycling conditions, the difference in thermal expansion coefficients between different layers may cause the coating to peel off or the interface to crack, affecting the stability and service life of the filter medium. (4) Complex pretreatment or post-treatment processes are required. The above methods all require strict surface pretreatment of stainless steel, including mechanical polishing, cleaning, electrochemical polishing and other steps. CN105268247B also needs to undergo multiple coating, drying and high-temperature calcination (600~1500℃), and the calcination needs to be carried out in a vacuum or protective atmosphere. CN106825547B requires the pre-preparation of dispersion solution and metal micro-nano mixed solution, and laser scanning and subsequent cleaning. The overall process is relatively long, which increases the complexity of operation and production costs. ⑤ It is sensitive to process parameters and has a narrow control window. The anodizing method has high requirements for the control accuracy of parameters such as voltage (5~80V), temperature (0~40℃), and time, and the process window is narrow. The additive manufacturing method is sensitive to factors such as laser power, scanning speed, powder ratio, and coating uniformity. The multilayer composite filter media method has strict limitations on parameters such as coating thickness, drying conditions, heating rate (1~5℃ / min), and sintering temperature (600~1500℃). (6) The pore structure formation mechanism is simple and it is difficult to achieve "zero energy consumption" preparation.

[0008] In summary, all existing technologies rely on external energy input (electrical energy, laser energy, thermal energy) to drive the pore-forming process, and there are no reports of spontaneous, zero-energy-consumption pore-forming using the material's own micro-battery effect. Summary of the Invention

[0009] This invention aims to overcome the shortcomings of existing technologies and provide a self-limiting nanoporous austenitic stainless steel and its preparation method. Unlike existing technologies that require external power supply, special laser equipment, high-temperature calcination, or complex pretreatment, this invention utilizes the natural electrode potential difference between the AlN precipitate phase in the nano-AlN phase austenitic stainless steel and the stainless steel matrix to achieve spontaneous anodic dissolution of the AlN phase in dilute sulfuric acid solution, thereby forming a nanoporous structure in situ on the stainless steel surface.

[0010] To achieve the above objectives, this invention provides a method for preparing self-limiting nanoporous austenitic stainless steel, particularly 21Cr-6Ni-9Mn high-strength austenitic stainless steel. This method involves introducing nano-sized AlN precipitates into the steel and utilizing their selective anodic dissolution in dilute sulfuric acid to construct an in-situ surface nanoporous layer. The method specifically includes the following steps:

[0011] A. Ingredients: Ingredients are prepared according to the chemical composition of austenitic stainless steel;

[0012] B. Smelting: The process involves electric furnace melting + AOD reduction + LF refining + electroslag remelting.

[0013] B1. Electric furnace melting: The raw materials are melted by passing electricity through them. After melting, the slag is removed, and the steel is tapped into the AOD furnace.

[0014] B2. AOD Reduction: The process involves AOD oxidation and decarburization, AOD reduction period nitrogen blowing alloying, primary reduction, and secondary reduction.

[0015] B2.1, AOD oxidation and decarbonization;

[0016] B2.2, Nitrogen blowing alloying during the AOD reduction period;

[0017] B2.3, Primary reduction: Add 15~25kg / t steel of ferrosilicon and 5~15kg / t steel of Al ingot for primary reduction. After primary reduction, measure the temperature and take samples for full analysis. When (FeO+MnO) in the slag is ≤1.0wt% and [O] in the molten steel is ≤30ppm, the primary reduction is considered sufficient.

[0018] B2.4 Secondary Reduction: Add 4~6 kg / t of Al ingots and 5~8 kg / t of fluorite to the steel for secondary reduction. After the secondary reduction is completed, measure the temperature and take samples for full analysis. When the Al content of the molten steel is 0.20~0.80 wt%, N is 0.15~0.40 wt%, [O] ≤30 ppm, S ≤0.005 wt%, P ≤0.015 wt%, and the temperature is ≥1500℃, the secondary reduction is deemed qualified.

[0019] B3, LF Refining: Enter the LF refining process, feed aluminum wire, adjust Al to 0.20~0.80wt%, add active lime or lime powder, add pre-melted refining slag and fluorite, send electrolytic slag, deep deoxidation and desulfurization, temperature ≥1500℃, temperature measurement and sampling full analysis, the qualified standard is: C≤0.04wt%, Si≤1.0wt%, Mn 8.0~10.0wt%, Cr 19.0~23.0wt%, Mo≤0.05wt%, Ni 5.5~7.5wt%, N 0.15~0.40wt%, Al 0.20~0.80wt%, P≤0.015wt%, S≤0.001wt%, [O]≤30ppm, temperature ≥1500℃; after passing the test, cast into φ400~φ600mm electrode rods;

[0020] B4. Electroslag remelting: Electroslag remelting of φ400~φ600mm electrode rods is carried out to obtain φ500~φ800mm electroslag steel ingots.

[0021] C. Hot forming: Homogenization treatment + forging and rolling processes are adopted;

[0022] C1. Homogenization treatment;

[0023] C2. Forging blanking: The thickness of the forging blank to the intermediate blank is 100~200mm;

[0024] C3. Rolling: After rough rolling and finish rolling, the plate is rolled to a thickness of 3.5±10% mm;

[0025] D. Intermediate annealing;

[0026] E. Cold deformation: 3.5±10%mm sheet is cold rolled to 0.20±25%mm, lap rolled to 0.01±25%mm and then subjected to solution heat treatment.

[0027] E1, Cold rolled to 0.20±25%mm: The 3.5±10%mm sheet after intermediate annealing is cold rolled to a thickness of 0.20±25%mm.

[0028] E2. Rolling to 0.01±25%mm: Take 4~8 sheets of 0.20±25%mm sheet and roll them together for the first round of rolling, 15~22 passes, with an average deformation rate of 5%~10% per pass, until the single sheet thickness is 0.04~0.06mm, then anneal and separate; Take 4~8 sheets of 0.04~0.06mm sheet and roll them together for the second round of rolling, 15~22 passes, until the single sheet thickness is 0.018~0.022mm, then anneal and separate; Take 2~4 sheets of 0.018~0.022mm sheet and roll them together for the third round of rolling, 15~22 passes, until the single sheet thickness is 0.01±25%mm foil.

[0029] E3, solution heat treatment;

[0030] F. Time-sensitive processing;

[0031] G. Self-limiting pore formation: Immerse the aged 0.01±25%mm foil in a 5~15wt% dilute sulfuric acid aqueous solution at a temperature of 20~50℃. After immersion, remove, rinse, and dry to obtain self-limiting nanoporous austenitic stainless steel.

[0032] In the above preparation method, in step A, the austenitic stainless steel is 21Cr-6Ni-9Mn, and its composition by mass percentage is: C≤0.04%, Si≤1.0%, Mn: 8.0~10.0%, Cr: 19.0~23.0%, Mo≤0.05%, Ni: 5.5~7.5%, N: 0.15~0.40%, Al: 0.20~0.80%, P≤0.015%, S≤0.001%, with the remainder being Fe and unavoidable impurities.

[0033] In the above preparation method, step A consists of recycled scrap steel, high-carbon ferrochrome, low-carbon ferrochrome, high-nitrogen ferrochrome, metallic manganese, ferrosilicon, electrolytic nickel, pure iron, and Al ingots.

[0034] In the above preparation method, in step B1, the melting temperature is controlled at 1520~1545℃.

[0035] In the above preparation method, in step B2.1, oxygen is blown into the AOD furnace to decarbonize to C≤0.05wt%, and the temperature is controlled at 1500~1530℃.

[0036] In the above preparation method, in step B2.2, the AOD reduction period begins, and nitrogen is blown to alloy the material until the N content is ≥0.30wt%.

[0037] In the above preparation method, in step B2.3, the reduction time for one reduction is 5-8 minutes.

[0038] In the above preparation method, in step B2.3, after determining that the reduction is sufficient, the slag is removed, and the amount of residual slag in the furnace is controlled to be ≤40kg / t steel.

[0039] In the above preparation method, in step B2.4, the secondary reduction time is 3~5 min.

[0040] In the above preparation method, in step B2.4, after the secondary reduction is deemed qualified, nitrogen blowing alloying is carried out to a temperature of 1500~1530℃.

[0041] In the above preparation method, in step B3, the amount of active lime added is 5~10 kg / t steel.

[0042] In the above preparation method, in step B3, the amount of lime powder added is 6~12 kg / t steel.

[0043] In the above preparation method, in step B3, the amount of pre-melted refining slag added is 3~6 kg / t steel.

[0044] In the above preparation method, in step B3, the amount of fluorite added is 1~3 kg / t steel.

[0045] In the above preparation method, in step B3, the pre-melted refining slag is 80 refining slag.

[0046] In the above preparation method, in step B4, the melting rate is controlled to be 3~8 kg / min.

[0047] In the above preparation method, in step B4, the electroslag composition is 50±10wt%CaF2-25±5wt%CaO-25±5wt%Al2O3, totaling 100%.

[0048] In the above preparation method, in step B4, the protective atmosphere is an Ar+N2 mixture.

[0049] In the above preparation method, in step C1, an electroslag steel ingot with a diameter of φ500~φ800mm is heated to 1150~1250℃ and held at that temperature for 24~30h.

[0050] In the above preparation method, in step C2, the billet temperature is 1150~1250℃.

[0051] In the above preparation method, in step C2, a longitudinal-transverse rolling strategy is adopted, with 3-4 longitudinal rolling passes, 90° rotation of the steel, and 3-5 transverse rolling passes, for a total of about 7-10 passes, and a reduction of not less than 40 mm per pass.

[0052] In the above preparation method, in step C2, the final rolling temperature is ≥950℃.

[0053] In the above preparation method, in step C2, after the billet is opened, it is stacked and slowly cooled at a temperature ≥400℃ for 48~72h.

[0054] In the above preparation method, in step C2, if the billet temperature is below 1000℃ during the forging process, it is reheated to 1150~1200℃ and held for 25~35 minutes before rolling.

[0055] In the preparation method described above, in step C3, the 100-200mm intermediate billet is reheated to 1150-1200℃ for 6-8 hours, and the homogenization time is 2.5-7.0 hours.

[0056] In the above preparation method, in step C3, the rough rolling temperature is ≥1150℃, the reduction rate of the first two passes is ≥20%, the reduction rate of subsequent passes is ≤15%, and the rough rolling is completed to 20~30mm.

[0057] In the above preparation method, in step C3, after rough rolling, the temperature is reheated to 1150~1200℃, the initial rolling temperature of finish rolling is ≥1050℃, the final rolling temperature is ≥950℃, the reduction rate of each finish rolling pass is ≤20%, and the plate is rolled to 3.5±10mm.

[0058] In the above preparation method, step C3 involves a total of 10 to 14 passes for roughing and finishing rolling.

[0059] In the above preparation method, in step C3, the material is immediately water-cooled after rolling.

[0060] In the above preparation method, step D involves subjecting the 3.5±10mm sheet to intermediate annealing at 1050~1100℃.

[0061] In the above preparation method, in step D, the annealing and holding time is 2-4 minutes.

[0062] In the above preparation method, step D is performed under full argon protection with a cooling rate ≥10℃ / s.

[0063] In the above preparation method, in step E1, the 3.5±10%mm plate after intermediate annealing is cold rolled in 4 to 6 passes. The first and second passes use a large deformation with a deformation rate of 12% to 15% per pass, and the cumulative reduction rate of each pass is 60% to 70%. The third and fourth passes use a small deformation with a deformation rate of 5% to 10% per pass, and the cumulative reduction rate of each pass is 35% to 45%. The fifth and sixth passes use a leveling process with a deformation rate of ≤0.5% per pass, and the cumulative reduction rate of each pass is ≤2.0%.

[0064] In the above preparation method, in step E1, intermediate annealing is performed after each rolling pass, with an annealing temperature of 1050~1100℃ and a holding time of 2~5min.

[0065] In the above preparation method, during intermediate annealing after each rolling pass in step E1, a full argon protective atmosphere is used, and the cooling rate is ≥10℃ / s.

[0066] In the above preparation method, in step E2, the annealing temperature is 1050~1100℃.

[0067] In the above preparation method, in step E2, the annealing time is 2~5 min.

[0068] In the above preparation method, in step E3, the temperature of the solution heat treatment is 1050~1100℃.

[0069] In the above preparation method, in step E3, the heat treatment holding time is 1~3 min.

[0070] In the above preparation method, step E3 is performed under full argon protection with a cooling rate ≥30℃ / s.

[0071] In the above preparation method, in step F, the aging treatment temperature is 650~700℃.

[0072] In the above preparation method, the aging treatment time in step F is 1~2 hours.

[0073] In the above preparation method, in step G, the concentration of the dilute sulfuric acid aqueous solution is 8~12wt%.

[0074] In the above preparation method, in step G, the soaking temperature is 25~40℃.

[0075] In the above preparation method, in step G, the soaking time is 5~30 min.

[0076] In the above preparation method, in step G, during the soaking process, static soaking or slight stirring is used to make the solution concentration and temperature uniform.

[0077] In the above preparation method, step G yields a self-limiting nanoporous austenitic stainless steel with a tensile strength ≥680MPa, a yield strength ≥340MPa, and an elongation ≥40%. Its pore structure is as follows: average pore size 50~300nm, pore size distribution 50~300nm, and pore density 30~60 pores / μm. 2 Pore ​​depth 100~800nm, specific surface area 10~30m² 2 / g, pore volume 0.03~0.06cm 3 / g.

[0078] The present invention also provides a self-limiting nanoporous austenitic stainless steel, which is prepared by the above-described preparation method.

[0079] The present invention also provides the application of the above-mentioned self-limiting nanoporous austenitic stainless steel in catalyst supports, microfiltration membranes or ultrafiltration membranes.

[0080] The beneficial effects of this invention are:

[0081] This invention utilizes the natural electrode potential difference between the AlN precipitate in austenitic stainless steel containing nano-AlN phase and the stainless steel matrix to achieve spontaneous anodic dissolution of the AlN phase in dilute sulfuric acid solution, thereby forming a nanoporous structure in situ on the stainless steel surface. It offers the following advantages: no external energy is required, as the material's own micro-battery effect drives pore formation, achieving "zero energy consumption" preparation; the process is extremely simple, requiring only immersion of the material in dilute sulfuric acid solution, eliminating the need for electrochemical equipment, laser systems, or high-temperature furnaces; it is environmentally friendly, using only low-concentration dilute sulfuric acid, with no fluorides, organic additives, or heavy metal pollution; its limiting feature is that the reaction automatically terminates after the formation of the surface nanoporous layer, without damaging the mechanical properties of the matrix; it forms in situ without interfaces, with the porous layer metallurgically bonded to the matrix, eliminating the risk of coating peeling and overcoming the interface defects of multilayer composite filter media methods; and it eliminates the need for complex pretreatment, omitting the powder preparation steps of additive manufacturing and the multilayer coating / high-temperature calcination steps of filter media methods. The limited nanoporous austenitic stainless steel obtained by this invention can be used as a catalyst carrier, with good market prospects and high added value. It can also be used in multiple fields such as the microfiltration / ultrafiltration membrane market. Attached Figure Description

[0082] Figure 1 The image shows a metallographic image of the AlN nonmetallic inclusions before the self-limiting pore formation in Example 1.

[0083] Figure 2 This is an electron microscope image of the AlN non-metallic inclusions before self-limiting pore formation in Example 1.

[0084] Figure 3 The image shows an electron microscope (EM) image of the stainless steel after self-limiting pore formation in Example 1. Detailed Implementation

[0085] Specifically, a method for preparing a self-limiting nanoporous austenitic stainless steel includes the following steps: ingredient preparation... electric furnace melting AOD oxidation decarbonization AOD reduction period nitrogen blowing alloying One-time restoration Secondary restoration LF Refining Electroslag remelting homogenization treatment Forging billet Rolling Intermediate annealing Cold rolled to 0.20±25%mm Rolled to 0.01±25%mm Solution heat treatment Timeliness processing The self-limiting hole-forming process is as follows:

[0086] A. Batching: Batching is performed according to the chemical composition of (21Cr-6Ni-9Mn high-strength austenitic stainless steel). The alloy material consists of recycled scrap steel, high-carbon ferrochrome (GB / T 5683, FeCr55C10.0), low-carbon ferrochrome (GB / T 5683, FeCr55C0.25), high-nitrogen ferrochrome (YB / T 4135, FeCrN8), metallic manganese, ferrosilicon, electrolytic nickel, pure iron, and Al ingots. The designed composition is: C≤0.04wt%, Si≤1.0wt%, Mn: 8.0~10.0%, Cr: 19.0~23.0wt%, Mo≤0.05%, Ni: 5.5~7.5wt%, N: 0.15~0.40wt%, Al: 0.20~0.80wt%, P≤0.015%, S≤0.001%, with the remainder being Fe and unavoidable impurities.

[0087] In this invention, Cr provides corrosion resistance and passivation film formation capability; Mn, high manganese content helps dissolve more nitrogen, stabilizes austenite, and improves work hardening rate; N, high nitrogen content is key to the high strength of this steel grade; and the key additive element Al is used to combine with N in the steel. This invention utilizes the naturally occurring high nitrogen (N) content in the 21Cr-6Ni-9Mn matrix, combined with additionally added aluminum (Al), to generate diffusely distributed nanoscale AlN particles. These AlN particles form nano-microcells with the stainless steel matrix. In an acidic environment, the AlN phase preferentially dissolves, leaving nanoscale pores. Before the improvement, although the composition range of 21Cr-6Ni-9Mn was also used, strict internal control of Al was not implemented in the preparation process, and AlN was not included in the rating. This invention, however, strictly limits the subsequent process.

[0088] In this invention, high-carbon ferrochrome conforms to the national standard GB / T 5683-2024 "Ferrochrome". A commonly used grade is FeCr55C10.0, with typical chemical composition requirements of Cr ≥ 52%, C ≤ 10.0%, Si ≤ 5.0%, P ≤ 0.06%, and S ≤ 0.06%. "C10.0" indicates an upper limit of carbon content of 10.0%, falling into the high-carbon category. Low-carbon ferrochrome also conforms to the national standard GB / T5683-2024 "Ferrochrome". The carbon content range for low-carbon ferrochrome is 0.15%~0.50%, with commonly used grades such as FeCr55C0.25 (carbon content ≤ 0.25%) or FeCr55C0.50 (carbon content ≤ 0.50%). High-nitrogen ferrochrome: The industry standard YB / T 4135-2016 "High-nitrogen ferrochrome" shall be followed. Common grades include FeCrN8(Ⅰ). The typical chemical composition requirements are Cr≥60.0%, N≥8.0%, C≤0.05%, Si≤1.0%, S≤0.040%, and P≤0.025%.

[0089] B. Smelting: The process involves electric furnace melting + AOD reduction + LF refining + electroslag remelting.

[0090] B1. Electric furnace melting: Add the above ingredients to the electric furnace, turn on the power to melt, and control the melting temperature at 1520~1545℃. After melting, remove the slag and tap the steel into the AOD furnace.

[0091] B2, AOD reduction: (1) AOD oxidation and decarburization: blow oxygen into the AOD furnace to decarburize to C≤0.05wt%, and control the temperature at 1500~1530℃.

[0092] (2) Nitrogen blowing alloying during AOD reduction period: During the AOD reduction period, nitrogen blowing alloying is started until the N content is ≥0.30wt%.

[0093] (3) Primary reduction: Add 15~25 kg / t of Si-Fe (i.e., ferrosilicon) and 5~15 kg / t of Al ingots to the furnace for primary reduction, with a reduction time of 5~8 min. After primary reduction, measure the temperature and take samples for full analysis. When (FeO+MnO) in the slag is ≤1.0 wt% and [O] in the molten steel is ≤30 ppm, the primary reduction is considered sufficient. After the molten steel is well deoxidized, remove the slag, and control the amount of residual slag in the furnace to ≤40 kg / t of steel.

[0094] The endpoint of a single reduction is determined by a combination of two indicators: slag and molten steel. After the first reduction, a full analysis is performed on a sample. The main indicators for determining sufficient reduction are: (FeO+MnO) in the slag ≤ 1.0 wt%, preferably ≤ 0.5 wt%; molten steel oxygen content [O] ≤ 30 ppm, preferably ≤ 20 ppm. The secondary indicators are: Cr2O3 in the slag ≤ 1.5 wt%, preferably ≤ 1.0 wt%; the slag is grayish-white or light green, without obvious black oxide slag; the residual Al and residual Si content in the molten steel meets the on-site internal control requirements. If any main indicator fails to meet the standard, the reduction is considered insufficient, and Al ingots are added to continue the reduction. The amount added can be determined based on the oxygen content of the molten steel, typically 5~15 kg / t of steel. Reduction continues until (FeO+MnO) in the slag ≤ 1.0 wt% and [O] in the molten steel ≤ 30 ppm, at which point the molten steel is considered well deoxidized, and then the slag is removed.

[0095] (4) Secondary reduction: Add 4~6 kg / t of Al ingots and 5~8 kg / t of fluorite to the steel for secondary reduction, which takes 3~5 min. After the secondary reduction, measure the temperature and take samples for full analysis. The secondary reduction is considered qualified when the Al content of the molten steel is 0.20~0.80 wt%, N is 0.15~0.40 wt%, [O] ≤30 ppm, S ≤0.005 wt%, P ≤0.015 wt%, and the temperature is ≥1500℃. Then, nitrogen blowing is used for alloying to a temperature of 1500~1530℃.

[0096] The endpoint criteria for secondary reduction are determined by a combination of steel composition, oxygen content, and temperature. After secondary reduction, a full analysis is performed on a sample. The secondary reduction is considered complete when the following conditions are met: Al content in the steel is 0.20~0.80wt%, preferably 0.30~0.60wt%; N content is 0.15~0.40wt%, preferably ≥0.30wt%; Oxygen content [O] ≤30ppm, preferably ≤20ppm; S ≤0.005wt%, preferably ≤0.003wt%; P ≤0.015wt%, preferably ≤0.010wt%; and temperature ≥1500℃, preferably 1500~1530℃. If any of the above indicators are not met, adjustments are made: if the Al content is too low, add Al ingots (usually 5~15kg / t of steel); if the N content is too low, continue nitrogen alloying; if the oxygen content is too high, add Al ingots to continue deoxidation; if S or P is too high, continue processing in the LF furnace. Once all indicators have reached the internal control range, the secondary reduction is considered qualified and the material can proceed to the LF furnace for refining.

[0097] B3, LF Refining: Entering the LF refining process, feed aluminum wire and adjust Al to 0.20~0.80wt%; add 5~10kg / t steel of active lime or 6~12kg / t steel of lime powder, 3~6kg / t steel of 80 refining slag (pre-melted refining slag), and 1~3kg / t steel of fluorite. Then, perform electrolytic slag treatment for deep deoxidation and desulfurization at a temperature ≥1500℃. Temperature measurement and full analysis of samples were performed. The chemical composition was found to be acceptable: C≤0.04wt%, Si≤1.0wt%, Mn 8.0~10.0wt%, Cr 19.0~23.0wt%, Mo≤0.05wt%, Ni 5.5~7.5wt%, N 0.15~0.40wt%, Al 0.20~0.80wt%, P≤0.015wt%, S≤0.001wt%, [O]≤30ppm, with the balance being Fe and unavoidable impurities. The temperature was also acceptable: molten steel temperature ≥1500℃, preferably 1500~1530℃. After passing these tests, electrode rods with a diameter of φ400~φ600mm were cast. The pre-melted refining slag could be of specification 80JLZ-YR, with the main components being: Al2O3 78~84%, CaO 4~10%, MgO 5~10%.

[0098] B4. Electroslag Remelting: The electrode rod is subjected to secondary electroslag remelting, with the melting rate controlled at 3~8 kg / min. The electroslag composition is 50±10wt%CaF2-25±5wt%CaO-25±5wt%Al2O3 (total 100%). The protective atmosphere is an Ar+N2 mixture, and an electroslag steel ingot with a diameter of φ500~φ800mm is prepared.

[0099] C. Hot forming (solution and deformation): Homogenization treatment + forging and rolling processes are adopted.

[0100] C1. Homogenization treatment: Heat the φ500~φ800mm electroslag steel ingot to 1150~1250℃ and hold for 24~30h to ensure that the core of the steel ingot is heated fully and evenly and to eliminate dendrite segregation.

[0101] C2. Forging and Billet Opening: A high-speed forging mill is used for billet opening at a temperature of 1150~1250℃. A longitudinal-transverse rolling strategy is adopted, with 3~4 longitudinal rolling passes, followed by 3~5 transverse rolling passes after a 90° turn, for a total of approximately 7~10 passes. The reduction per pass is not less than 40mm (ensuring large reduction rolling throughout the process to fully fragment the ingot core structure). The thickness of the billet from opening to intermediate billet is 100~200mm. The final rolling temperature after opening is ≥950℃ to suppress the precipitation of carbides and Cr2N phases. After opening, the billets are stacked and slowly cooled at a temperature ≥400℃ for 48~72 hours. Due to the slow cooling method used in this invention, Cr2N phase precipitation is unavoidable on the outer surface. Therefore, after unstacking, the billet surface is mechanically ground to remove surface iron oxide scale and Cr2N phase. If the billet temperature is below 1000℃ during the forging process, it should be reheated to 1150~1200℃ and held for 25~35 minutes before rolling.

[0102] C3. Rolling Stage: The intermediate billet is reheated to 1150~1200℃ for 6~8 hours, with a soaking time of 2.5~7.0 hours (holding time is approximately 1.5~2 min / mm to ensure sufficient solid solution of alloying elements and effectively inhibit the growth of original austenite grains). A reciprocating medium-thick plate mill is used for rolling. The roughing rolling start temperature is ≥1150℃, with a reduction rate ≥20% in the first two passes (utilizing high temperature and high reduction to fragment the structure, achieving dynamic recrystallization and obtaining uniform recrystallized austenite grains), and a reduction rate ≤15% in subsequent passes (to prevent edge cracking), roughing to 20~30 mm; reheating to 1150~1200℃, the finishing rolling start temperature is ≥1050℃, the finishing rolling temperature is ≥950℃, and the reduction rate in the finishing rolling passes is ≤20% (to prevent edge cracking), rolling to a plate thickness of 3.5±10 mm. The total number of roughing and finishing rolling passes is approximately 10~14. Water cooling immediately after rolling.

[0103] D. Intermediate annealing: Before cold rolling, the 3.5±10%mm plate is subjected to intermediate annealing at 1050~1100℃ in a continuous annealing furnace, with a holding time of 2~4min, under full argon protection, and a cooling rate ≥10℃ / s.

[0104] E. Cold deformation: Cold deformation can generate a large number of dislocations in austenite grains, inducing nano-AlN to precipitate on dislocation lines and form a nanoscale dispersed distribution.

[0105] E1. Cold rolling to 0.20±25%mm: The 3.5±10%mm sheet after intermediate annealing is cold rolled in 4-6 passes, each pass containing 5-7 passes. The first and second passes use a large deformation with a deformation rate of 12%-15% per pass, and the cumulative reduction rate of each pass is 60%-70%. The third and fourth passes use a small deformation with a deformation rate of 5%-10% per pass, and the cumulative reduction rate of each pass is 35%-45%. The fifth and sixth passes use a leveling process with a deformation rate of ≤0.5% per pass, and the cumulative reduction rate of each pass is ≤2.0%. After each pass, intermediate annealing is performed in a continuous bright annealing furnace at a temperature of 1050-1100℃, a holding time of 2-5 minutes, under a full argon protective atmosphere, and a cooling rate ≥10℃ / s. It is cold rolled through multiple rolling passes to a thickness of 0.15~0.25mm (preferably 0.20mm).

[0106] E2. Rolling to 0.01±25%mm: Take 4~8 sheets of 0.20±25%mm sheet and roll them together for the first round of rolling. The first round of rolling is 15~22 passes, with an average deformation rate of 5%~10% per pass. After rolling to a single sheet thickness of approximately 0.04~0.06mm, anneal at 1050~1100℃ for 2~5 minutes and separate. Take 4~8 sheets of 0.04~0.06mm sheet and roll them together for the second round of rolling. The second round of rolling is 15~22 passes. After rolling to a single sheet thickness of approximately 0.018~0.022mm, anneal at 1050~1100℃ for 2~5 minutes and separate. Take 2 to 4 sheets of 0.018 to 0.022 mm thick plates and stack them together for the third round of stacking. The third round of stacking is 15 to 22 passes, and the foil is rolled to a single sheet thickness of 0.01 ± 25 mm (preferably 0.01 mm).

[0107] E3. Solution Heat Treatment: 0.01±25% mm foil is solution treated in a continuous annealing furnace at a temperature of 1050~1100℃ (preferably 1080℃) for 1~3 minutes under full argon protection, with a cooling rate ≥30℃ / s. Prolonged holding above 1100℃ may lead to grain coarsening, and AlN will partially dissolve at high temperatures, affecting subsequent pore formation. Short-term solution treatment at 1050~1100℃ ensures sufficient recrystallization of the austenite matrix while retaining enough dislocations as AlN nucleation sites.

[0108] In step E, cold rolling from 3.5±10%mm to 0.20±25%mm: This stage involves conventional multi-pass cold rolling followed by intermediate annealing. The purpose is to introduce a large number of dislocations into the austenite grains through cold deformation, providing nucleation sites for the precipitation of nano-AlN along dislocation lines during subsequent aging treatment. Intermediate annealing is performed after each rolling pass (multiple passes) to restore plasticity before continuing to the next rolling pass. Subsequently, this invention further rolls 0.20±25%mm to 0.01±25%mm. This stage employs a multi-sheet stacking process because 0.01±25%mm falls into the category of extremely thin strip / foil materials. During single-sheet rolling, the rolls experience severe elastic flattening, making it difficult to control the sheet shape. Multi-sheet segmented stacking is used to reduce the single-sheet rolling pressure and improve production efficiency. In the final solution treatment, the 0.01±25%mm foil is short-term solution treated at high temperature, which preserves the dislocations generated by cold deformation (as nucleation sites for AlN precipitation) and restores the austenitic structure of the steel matrix.

[0109] F. Aging Treatment: The 0.01±25%mm foil after heat treatment is aged at 650~700℃ for 1~2h in an inert atmosphere furnace, followed by air cooling to room temperature. The presence of Mn can increase the diffusion rate of N in steel, promote the uniform nucleation of AlN at the nanoscale, avoid local coarsening, and further remove the internal stress of the foil. High-temperature evaporation of the surface oil film is beneficial for pore formation. Slight high-temperature oxidation of the surface can destroy the passivation film of stainless steel, which is beneficial for pore formation. It also allows a small amount of fine precipitates to form, which is beneficial for pore formation.

[0110] G. Self-limiting pore formation: Immerse the aged foil (0.01±25 mm) in a dilute sulfuric acid aqueous solution at a temperature of 20~50℃ without an external power supply. Static immersion or gentle stirring can be used to ensure uniform solution concentration and temperature. After immersion, remove the foil, rinse with deionized water, and dry with nitrogen to obtain self-limiting nanoporous austenitic stainless steel. Electrolyte: dilute sulfuric acid solution, concentration 5%~15% (preferably 8%~12%); temperature: 20~50℃ (preferably 25~40℃); time: 5~30 min (preferably 10~20 min).

[0111] This invention's pore-forming process does not require an external power source; strictly speaking, it is not "electrolysis," but rather a spontaneous micro-battery selective anodic dissolution. The principle is as follows: When stainless steel containing nano-AlN phase is immersed in dilute sulfuric acid, a natural electrode potential difference exists between the AlN phase and the stainless steel substrate. The AlN phase, acting as the micro-anode, preferentially dissolves, while the stainless steel substrate / passivation film acts as the micro-cathode, forming an internal short-circuit galvanic cell. Therefore, no electricity is required, there are no external anodes or cathodes, and no current or voltage range. Anode: Stainless steel AlN precipitated phase (micro-anode); Cathode: Stainless steel substrate and surface Cr2O3 passivation film (micro-cathode). The specific mechanism is: The AlN phase and the stainless steel substrate form a micro-battery; the AlN phase, acting as the micro-anode, preferentially dissolves, and the stainless steel substrate / passivation film acts as the micro-cathode. The reaction formula is: Micro-anode (AlN dissolution): Microcathode (substrate hydrogen evolution): Overall reaction of the micro battery: Because 21Cr-6Ni-9Mn contains a high Cr content (approximately 21%), it readily forms a dense Cr2O3 passivation film in dilute sulfuric acid. When the surface AlN dissolves, the exposed Cr2O3 passivation film forms, preventing the reaction from penetrating deeper into the substrate. This ensures the nanoporous layer remains only on the surface (100-800 nm depth), achieving pore formation with "zero energy consumption and no external power supply required," without compromising the mechanical properties of the substrate. Therefore, the self-limiting nanoporous austenitic stainless steel obtained by this invention maintains the high strength and non-magnetic characteristics of the 21Cr-6Ni-9Mn substrate while also possessing a highly active nanoporous layer on the surface.

[0112] The present invention will be explained below with reference to embodiments. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they shall be performed in accordance with the techniques or conditions described in the literature in the art or in accordance with the product manual.

[0113] Example 1

[0114] A. Batching: Batching is performed according to the chemical composition of 21Cr-6Ni-9Mn high-strength austenitic stainless steel before self-limiting pore formation. The alloy material consists of recycled scrap steel, high-carbon ferrochrome (GB / T 5683, FeCr55C10.0), low-carbon ferrochrome (GB / T 5683, FeCr55C0.25), high-nitrogen ferrochrome (YB / T 4135, FeCrN8), metallic manganese, ferrosilicon, electrolytic nickel, pure iron, and Al ingots. The designed composition (mass percentage) is: C 0.04%, Si 0.5%, Mn 9.5%, Cr 20%, Mo 0.01%, Ni 6.8%, N 0.35%, Al 0.5%, P≤0.015%, S≤0.001%, with the remainder being Fe and unavoidable impurities.

[0115] B. Smelting: The process involves electric furnace melting + AOD reduction + LF refining + electroslag remelting.

[0116] B1. Electric furnace melting: Add the above ingredients to the electric furnace, turn on the power to melt, and control the melting temperature at 1520~1545℃. After melting, remove the slag and tap the steel into the AOD furnace.

[0117] B2. AOD Reduction:

[0118] (1) AOD oxidation decarburization: oxygen is blown into the AOD furnace to decarburize to C≤0.05wt%, and the temperature is controlled at 1500~1530℃;

[0119] (2) Nitrogen blowing alloying during the AOD reduction period: During the AOD reduction period, nitrogen blowing alloying begins until the N content is ≥0.30wt%;

[0120] (3) Primary reduction: Add 20 kg / t of Si-Fe (i.e., ferrosilicon) and 10 kg / t of Al ingots to the furnace for primary reduction, with a reduction time of 6 min. After primary reduction, measure the temperature and take samples for full analysis. When (FeO+MnO) in the slag is ≤1.0 wt% and [O] in the molten steel is ≤30 ppm, the primary reduction is considered sufficient. After the molten steel is well deoxidized, remove the slag, and control the amount of residual slag in the furnace to ≤40 kg / t of steel;

[0121] (4) Secondary reduction: Add 6 kg / t of Al ingots and 5 kg / t of fluorite to the steel for secondary reduction, which takes 4 min. After the secondary reduction, measure the temperature and take samples for full analysis. The secondary reduction is considered qualified when the Al content of the molten steel is 0.20~0.80 wt%, N is 0.15~0.40 wt%, [O] ≤30 ppm, S ≤0.005 wt%, P ≤0.015 wt%, and the temperature is ≥1500℃. Then, nitrogen blowing is used for alloying to a temperature of 1500~1530℃.

[0122] B3, LF Refining: Entering the LF refining process, aluminum wire is fed, and the Al content is adjusted to 0.50 wt%. 8 kg / t of active lime, 5 kg / t of 80 refining slag, and 1.5 kg / t of fluorite are added. Electrolytic slag is then introduced for deep deoxidation and desulfurization at 1580℃. Temperature measurement and full analysis of samples are performed. The acceptable standards are: C 0.04%, Si 0.5%, Mn 9.5%, Cr 20%, Mo 0.01%, Ni 6.8%, N 0.35%, Al 0.50%, P≤0.015%, S≤0.001%, [O]≤20ppm, and temperature≥1500℃. After passing the standards, the product is cast into φ400mm electrode rods.

[0123] B4. Electroslag remelting: The electrode rod is subjected to secondary electroslag remelting and smelting. The melting rate is controlled at 5 kg / min. The electroslag composition is 50 wt% CaF2-25 wt% CaO-25 wt% Al2O3. The protective atmosphere is a mixture of Ar (70%) and N2 (30%). φ500 electroslag steel ingot is prepared.

[0124] C. Hot forming (solution and deformation): using homogenization treatment + forging and rolling processes.

[0125] C1. Homogenization treatment: Heat the φ500 electroslag steel ingot to 1200℃ and hold for 25 hours to ensure that the core of the steel ingot is heated fully and evenly, and to eliminate dendrite segregation.

[0126] C2. Forging and Billet Opening: A high-speed forging mill is used for billet opening at a temperature of 1200±30℃. A longitudinal-transverse rolling strategy is employed, with 4 longitudinal rolling passes, followed by 4 transverse rolling passes after a 90° turn, for a total of 8 passes. The reduction per pass is no less than 40mm, ensuring high reduction throughout the rolling process to fully fragment the core structure of the ingot, forging the billet to a 150mm thick intermediate square billet. The final rolling temperature after billet opening is ≥950℃ to suppress the precipitation of carbides and Cr2N phases. After billet opening, the billets are removed from the line and stacked for slow cooling.

[0127] C3. Rolling Stage: The 150mm intermediate square billet is reheated to 1180±20℃ for 7 hours, followed by a 6-hour soaking time to ensure complete dissolution of alloying elements and effectively inhibit the growth of original austenite grains. A reciprocating medium-thick plate rolling mill is used for rolling. The roughing rolling temperature is ≥1150℃ (the billet cools down considerably from the furnace to the mill, typically by 20℃ on the outer surface). The reduction rate in the first two passes is ≥20%, utilizing high temperature and high reduction to fragment the microstructure and achieve dynamic recrystallization, resulting in uniform recrystallized austenite grains. The reduction rate in subsequent passes is ≤15% to prevent edge cracking. The roughing is rolled to 25±10% mm. The billet is then reheated to 1180±20℃. The finishing rolling temperature is 1080±20℃ (due to the thinner billet, it cools down rapidly after exiting the furnace, typically by 100℃ on the outer surface). The final rolling temperature is 960±10℃, with a reduction rate of ≤20% in the finishing passes to prevent edge cracking, rolling to a 3.5mm thick plate. The total number of roughing and finishing passes is 12. The billet is immediately water-cooled after rolling.

[0128] D. Intermediate annealing: Before cold rolling, the 3.5mm plate is subjected to intermediate annealing at 1080℃ in a continuous annealing furnace, with a holding time of 3min, full argon protection, and a cooling rate ≥10℃ / s.

[0129] E. Cold deformation: Cold deformation can generate a large number of dislocations in austenite grains, inducing nano-AlN to precipitate on dislocation lines and form a nanoscale dispersed distribution.

[0130] E1. Cold rolling to 0.20mm: The 3.5mm sheet after intermediate annealing is cold rolled in 5 passes, each pass containing 6 passes. In the first two passes, the deformation rate is approximately 14.2% per pass, and the cumulative reduction is approximately 60.0% per pass. In the third and fourth passes, the deformation rate is approximately 8.2% per pass, and the cumulative reduction is approximately 40.2% per pass. In the fifth leveling pass, the deformation rate is approximately 0.34% per pass, and the cumulative reduction is approximately 2.0% per pass. After each pass, intermediate annealing is performed in a continuous bright annealing furnace at 1080℃ for 3 minutes, using a full argon protective atmosphere, with a cooling rate ≥10℃ / s. The sheet is then cold rolled in multiple passes to a thickness of 0.20mm.

[0131] E2. Rolling to 0.01mm: Take 6 sheets of 0.20mm sheet and roll them together for the first round of rolling, including 20 passes with an average deformation rate of approximately 6.7% per pass, until the thickness of a single sheet is approximately 0.05mm. Then anneal at 1050℃ for 3 minutes and separate. Take 6 sheets of 0.05mm sheet and roll them together for the second round of rolling, including 20 passes, until the thickness of a single sheet is approximately 0.02mm. Then anneal at 1050℃ for 3 minutes and separate. Take 3 sheets of 0.02mm sheet and roll them together for the third round of rolling, including 20 passes, until the thickness of a single sheet of foil is 0.01mm.

[0132] E3. Solution heat treatment of finished product: The 0.01mm foil is solution treated in a continuous annealing furnace at a temperature of 1080℃ for 2 minutes under full argon protection and a cooling rate of ≥30℃ / s.

[0133] F. Aging treatment: The 0.01mm foil after the heat treatment is aged at 677℃ for 1.5h in an inert atmosphere furnace and then air-cooled to room temperature to promote uniform nucleation of AlN at the nanoscale and avoid local coarsening. Figure 1 The image shows a metallographic image of the AlN non-metallic inclusions before self-limiting pore formation in Example 1. Figure 2 The image shown is an electron microscope image of the AlN non-metallic inclusions before the self-limiting pore formation in Example 1. It can be seen that the AlN non-metallic inclusions appear as tiny black dots.

[0134] G. Self-limiting pore formation: A 0.01 mm thick foil after aging treatment is immersed in a 10 wt% dilute sulfuric acid aqueous solution at 30°C for 15 minutes, without the need for an external power source. The AlN phase and the stainless steel substrate form a micro-battery, with the AlN phase acting as the micro-anode and preferentially dissolving, while the stainless steel substrate / Cr2O3 passivation film acts as the micro-cathode. After immersion, the foil is removed, rinsed with deionized water, and dried with nitrogen to obtain self-limiting nanoporous austenitic stainless steel. Micro-anode (AlN dissolution): Microcathode (substrate hydrogen evolution): Overall reaction of the micro battery: Because 21Cr-6Ni-9Mn contains a high amount of Cr, it readily forms a dense Cr2O3 passivation film in dilute sulfuric acid. When the surface AlN dissolves, the exposed Cr2O3 passivation film forms, preventing the reaction from penetrating deeper into the substrate and ensuring that the nanoporous layer remains only on the surface without impairing the mechanical properties of the substrate.

[0135] Upon examination, the electron microscope images of the stainless steel after self-limiting pore formation in Example 1 are as follows: Figure 3 As shown in Table 1, the pore structure parameters of the obtained nanoporous austenitic stainless steel are shown in Table 1.

[0136] Table 1. Pore structure parameters of the nanoporous austenitic stainless steel obtained in Example 1

[0137]

[0138] The "self-limiting" effect, with a pore depth of only about 450 nm, indicates that the reaction automatically terminates after the surface AlN dissolves, without penetrating deep into the matrix. The matrix maintains good mechanical properties, with a tensile strength of 713 MPa, a yield strength of 396 MPa, and an elongation of 55.5%. Compared with the unporous matrix, the decrease is very small, proving that the self-limiting effect effectively protects the mechanical properties of the matrix.

[0139] The nanoporous austenitic stainless steel obtained in this embodiment was used as a catalyst support, loaded with 0.5% Pt, for the catalytic oxidation of toluene. At a space velocity of 10000 h⁻¹, the reaction was carried out. -1 Under conditions of 1000 ppm toluene concentration and 180℃ reaction temperature, the conversion rate reached 98%, the selectivity was 99%, and the system operated stably for 700 hours.

[0140] Compared with products manufactured by additive manufacturing, the product of this embodiment has an 8% higher conversion rate and a 60mV lower overpotential; compared with products manufactured by filter media, the product of this embodiment has a more uniform pore distribution, no interface peeling, and a 40% longer stable operating time.

Claims

1. A method for preparing self-limiting nanoporous austenitic stainless steel, characterized in that: Includes the following steps: A. Ingredients: Ingredients are prepared according to the chemical composition of austenitic stainless steel; B. Smelting: The process involves electric furnace melting + AOD reduction + LF refining + electroslag remelting. B1. Electric furnace melting: The raw materials are melted by passing electricity through them. After melting, the slag is removed, and the steel is tapped into the AOD furnace. B2. AOD Reduction: The process involves AOD oxidation and decarburization, AOD reduction period nitrogen blowing alloying, primary reduction, and secondary reduction. B2.1, AOD oxidation and decarbonization; B2.2, Nitrogen blowing alloying during AOD reduction period; B2.3, Primary reduction: Add 15~25kg / t steel of ferrosilicon and 5~15kg / t steel of Al ingot for primary reduction. After primary reduction, measure the temperature and take samples for full analysis. When (FeO+MnO) in the slag is ≤1.0wt% and [O] in the molten steel is ≤30ppm, the primary reduction is considered sufficient. B2.4 Secondary Reduction: Add 4~6 kg / t of Al ingots and 5~8 kg / t of fluorite to the steel for secondary reduction. After the secondary reduction is completed, measure the temperature and take samples for full analysis. When the Al content of the molten steel is 0.20~0.80 wt%, N is 0.15~0.40 wt%, [O] ≤30 ppm, S ≤0.005 wt%, P ≤0.015 wt%, and the temperature is ≥1500℃, the secondary reduction is deemed qualified. B3, LF Refining: Enter the LF refining process, feed aluminum wire, adjust Al to 0.20~0.80wt%, add active lime or lime powder, add pre-melted refining slag and fluorite, send electrolytic slag, deep deoxidation and desulfurization, temperature ≥1500℃, temperature measurement and sampling full analysis, the qualified standard is: C≤0.04wt%, Si≤1.0wt%, Mn 8.0~10.0wt%, Cr 19.0~23.0wt%, Mo≤0.05wt%, Ni5.5~7.5wt%, N 0.15~0.40wt%, Al 0.20~0.80wt%, P≤0.015wt%, S≤0.001wt%, [O]≤30ppm, temperature ≥1500℃; after passing the test, cast into φ400~φ600mm electrode rods; B4. Electroslag remelting: Electroslag remelting of φ400~φ600mm electrode rods is carried out to obtain φ500~φ800mm electroslag steel ingots. C. Hot forming: Homogenization treatment + forging and rolling processes are adopted; C1. Homogenization treatment; C2. Forging blanking: The thickness of the forging blank to the intermediate blank is 100~200mm; C3. Rolling: After rough rolling and finish rolling, the plate is rolled to a thickness of 3.5±10% mm; D. Intermediate annealing; E. Cold deformation: 3.5±10%mm sheet is cold rolled to 0.20±25%mm, lap rolled to 0.01±25%mm and then subjected to solution heat treatment. E1, Cold rolled to 0.20±25%mm: The 3.5±10%mm sheet after intermediate annealing is cold rolled to a thickness of 0.20±25%mm. E2. Rolling to 0.01±25%mm: Take 4~8 sheets of 0.20±25%mm sheet and roll them together for the first round of rolling, 15~22 passes, with an average deformation rate of 5%~10% per pass, until the single sheet thickness is 0.04~0.06mm, then anneal and separate; Take 4~8 sheets of 0.04~0.06mm sheet and roll them together for the second round of rolling, 15~22 passes, until the single sheet thickness is 0.018~0.022mm, then anneal and separate; Take 2~4 sheets of 0.018~0.022mm sheet and roll them together for the third round of rolling, 15~22 passes, until the single sheet thickness is 0.01±25%mm foil. E3, solution heat treatment; F. Time-sensitive processing; G. Self-limiting pore formation: Immerse the aged 0.01±25%mm foil in a 5~15wt% dilute sulfuric acid aqueous solution at a temperature of 20~50℃. After immersion, remove, rinse, and dry to obtain self-limiting nanoporous austenitic stainless steel.

2. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step A, the austenitic stainless steel is 21Cr-6Ni-9Mn, and its composition by mass percentage is: C≤0.04%, Si≤1.0%, Mn: 8.0~10.0%, Cr: 19.0~23.0%, Mo≤0.05%, Ni: 5.5~7.5%, N: 0.15~0.40%, Al: 0.20~0.80%, P≤0.015%, S≤0.001%, with the remainder being Fe and unavoidable impurities; In step A, the ingredients consist of recycled scrap steel, high-carbon ferrochrome, low-carbon ferrochrome, high-nitrogen ferrochrome, metallic manganese, ferrosilicon, electrolytic nickel, pure iron, and Al ingots.

3. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step B1, the melting temperature is controlled at 1520~1545℃; In step B2.1, oxygen is blown into the AOD furnace to decarburize until C ≤ 0.05 wt%, and the temperature is controlled at 1500~1530℃; In step B2.2, the AOD reduction period begins, during which nitrogen alloying is initiated until the N content is ≥0.30 wt%. In step B2.3, the time for one restoration is 5-8 minutes; In step B2.3, after determining that the reduction is sufficient, the slag is removed, and the amount of residual slag in the furnace is controlled to be ≤40kg / t steel; In step B2.4, the secondary reduction time is 3-5 minutes; In step B2.4, after the secondary reduction is deemed successful, nitrogen alloying is carried out to a temperature of 1500~1530℃; In step B3, the amount of active lime added is 5~10 kg / t steel; In step B3, the amount of lime powder added is 6~12 kg / t steel; In step B3, the amount of pre-melted refining slag added is 3~6 kg / t steel; In step B3, the amount of fluorite added is 1~3 kg / t steel; In step B3, the pre-melted refining slag is 80 refining slag; In step B4, the melting rate is controlled at 3~8 kg / min; In step B4, the electroslag composition is 50±10wt%CaF2-25±5wt%CaO-25±5wt%Al2O3, totaling 100%; In step B4, the protective atmosphere is a mixture of Ar and N2.

4. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step C1, the φ500~φ800mm electroslag steel ingot is heated to 1150~1250℃ and held for 24~30h; In step C2, the billet temperature is 1150~1250℃; In step C2, a longitudinal-transverse rolling strategy is adopted, with 3-4 longitudinal rolling passes, 90° rotation of the steel, and 3-5 transverse rolling passes, for a total of about 7-10 passes, and the reduction per pass is not less than 40mm. In step C2, the final rolling temperature after billet preparation is ≥950℃; In step C2, after the billet is cut off, it is stacked and cooled slowly. The slow cooling temperature is ≥400℃ and the slow cooling time is 48~72h. In step C2, if the billet temperature is below 1000℃ during the forging process, it should be reheated to 1150~1200℃ and held for 25~35 minutes before rolling. In step C3, the 100~200mm intermediate billet is reheated to 1150~1200℃ for 6~8 hours, and the soaking time is 2.5~7.0 hours. In step C3, the roughing rolling temperature is ≥1150℃, the reduction rate of the first two passes is ≥20%, the reduction rate of subsequent passes is ≤15%, and the roughing is rolled to 20~30mm. In step C3, after rough rolling, the temperature is reheated to 1150~1200℃, the starting rolling temperature of finish rolling is ≥1050℃, the finishing rolling temperature is ≥950℃, the reduction rate of each finish rolling pass is ≤20%, and the plate is rolled to 3.5±10%mm. In step C3, the total number of roughing and finishing passes is 10 to 14. In step C3, the material is immediately water-cooled after rolling.

5. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step D, the 3.5±10%mm sheet is subjected to intermediate annealing at 1050~1100℃; In step D, the annealing holding time is 2-4 minutes; In step D, during annealing, the entire process is protected by argon gas, and the cooling rate is ≥10℃ / s.

6. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step E1, the 3.5±10%mm sheet after intermediate annealing is cold rolled in 4-6 passes, each pass containing 5-7 passes. The first and second passes use a large deformation with a deformation rate of 12%-15% per pass, and the cumulative reduction rate of each pass is 60%-70%. The third and fourth passes use a small deformation with a deformation rate of 5%-10% per pass, and the cumulative reduction rate of each pass is 35%-45%. The fifth and sixth passes use a leveling process with a deformation rate of ≤0.5% per pass, and the cumulative reduction rate of each pass is ≤2.0%. In step E1, intermediate annealing is performed after each rolling pass, with an annealing temperature of 1050~1100℃ and a holding time of 2~5min; In step E1, during intermediate annealing after each rolling pass, a full argon protective atmosphere is used, and the cooling rate is ≥10℃ / s; In step E2, the annealing temperature is 1050~1100℃; In step E2, the annealing time is 2-5 minutes; In step E3, the solution heat treatment temperature is 1050~1100℃; In step E3, the holding time for solution heat treatment is 1~3 min; In step E3, the entire gas is protected by argon gas, and the cooling rate is ≥30℃ / s.

7. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step F, the aging treatment temperature is 650~700℃; In step F, the time for aging processing is 1 to 2 hours.

8. The preparation method according to claim 1, characterized in that: At least one of the following must be met: In step G, the concentration of the dilute sulfuric acid aqueous solution is 8~12wt%; In step G, the soaking temperature is 25~40℃; In step G, the soaking time is 5~30 minutes; In step G, during the soaking process, static soaking or gentle stirring is used to ensure uniform solution concentration and temperature; In step G, the obtained self-limiting nanoporous austenitic stainless steel has a tensile strength ≥680MPa, a yield strength ≥340MPa, and an elongation ≥40%. Its pore structure is as follows: average pore size 50~300nm, pore size distribution 50~300nm, pore density 30~60 pores / μm. 2 Pore ​​depth 100~800nm, specific surface area 10~30m² 2 / g, pore volume 0.03~0.06cm 3 / g.

9. The self-limiting nanoporous austenitic stainless steel prepared by the preparation method according to any one of claims 1 to 8.

10. The application of the self-limiting nanoporous austenitic stainless steel according to claim 9 in catalyst supports, microfiltration membranes or ultrafiltration membranes.

Citation Information

Patent Citations

  • A nanoporous array thin film on a stainless steel surface and its preparation method

    CN102268713A

  • A kind of nanoscale porous metal filter medium and preparation method thereof

    CN105268247B

  • Method for preparing nano-porous structure on surfaces of stainless steel and cobalt alloy

    CN106521604A

  • A method for additive manufacturing of porous metal materials by selective laser melting of a solution of micro / nano-mixed metal particles in an air environment.

    CN106825547B