A FeCrW-based ODS~F / M steel containing Al and Ti and its preparation method

By preparing FeCrW-based ODS-F/M steel containing Al and Ti, the problem of insufficient high-temperature strength and corrosion resistance of existing F/M steel in lead-cooled fast reactors has been solved. The material has achieved improved high strength and corrosion resistance under high-temperature conditions and is suitable for cladding materials of lead-cooled fast reactors.

CN123108433APending Publication Date: 2026-11-17NUCLEAR POWER INSTITUTE OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611041487.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-14
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing F/M steels cannot meet the requirements of lead-cooled fast reactors for high-temperature strength, creep performance, and corrosion resistance of cladding materials under high temperature and high-neutron irradiation, especially exhibiting poor performance in liquid Pb-Bi corrosive environments.

Method used

Using FeCrW-based ODS-F/M steel containing Al and Ti, and by adding finely dispersed Y2O3 particles and a reasonable element ratio, ODS-F/M steel with excellent high-temperature mechanical properties is prepared. The process includes steps such as pre-alloyed powder mixing, ball milling, spark plasma sintering, hot rolling, and heat treatment.

Benefits of technology

It significantly improves the high-temperature strength and corrosion resistance of the material, especially the tensile strength and yield strength at 550℃ and 600℃, making it suitable for cladding materials of lead-cooled fast reactors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of nuclear materials, and more particularly to an Al and Ti-containing FeCrW-based ODS~F / M steel and its preparation method. The FeCrW-based ODS~F / M steel is produced by sintering, hot rolling, and heat treatment of pre-alloyed powder and Y₂O₃ with a particle size ≤20nm. The amount of Y₂O₃ added is 0.3~0.4wt% of the mass of the pre-alloyed powder. The pre-alloyed powder consists of the following components by weight: 9~12.2wt% Cr powder, 1~2wt% W powder, 0.3~0.6wt% Mn powder, 0.2~0.5wt% Ta and V powder, 0.01~0.1wt% Zr and La powder, 0.15~0.25wt% C powder, 0.1~5.0wt% Al powder, 0.3~0.5wt% Ti powder, and the balance being iron powder. This invention is applicable to cladding materials for lead-based reactors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of nuclear materials, and more particularly to an Al and Ti-containing FeCrW-based ODS~F / M steel and its preparation method. Background Technology

[0002] The Generation IV Nuclear Energy Systems International Forum (GIF) has proposed six advanced reactor types: gas-cooled fast reactors, lead-cooled fast reactors, molten salt reactors, nano-cooled fast reactors, ultra-high-temperature gas-cooled reactors, and supercritical water-cooled reactors. These aim to systematically address the economic, safety, waste management, and protection issues in the development of nuclear power. Among these six pre-selected reactor types, lead-cooled fast reactors have attracted significant attention due to their unique advantages in neutron economy, thermal-hydraulic characteristics, chemical stability, and safety. They are a key focus of advanced nuclear energy system research and are expected to be the first to achieve industrial demonstration applications within the Generation IV nuclear energy system.

[0003] Among them, the reliability of reactor cladding materials is one of the main bottlenecks restricting the sustainable use of advanced nuclear energy in the future, which determines the feasibility, safety and economy of nuclear energy systems. For lead-cooled fast reactors, the irradiation and corrosion environment faced by their cladding materials is more severe than that of current commercial pressurized water reactors, which puts forward higher requirements for the high temperature strength, creep performance, radiation resistance and corrosion resistance of the cladding materials. For example, compared with the relatively low operating temperature (≤350℃) and neutron irradiation dose of most current commercial nuclear power plants, the service environment faced by the cladding components of lead-cooled fast reactors will be more severe: (1) higher operating temperature (500℃~650℃); (2) corrosive environment of liquid Pb~Bi metal solution; (3) high neutron irradiation dose: between 50~150 dpa, up to 200 dpa. Existing cladding materials for nuclear power water reactors, such as zirconium alloys and austenitic stainless steel, suffer from severe radiation swelling, radiation hardening, and Pb-Bi metal corrosion under high-temperature, high-neutron irradiation. Therefore, they cannot fully meet the requirements for cladding materials in fast neutron reactors such as lead-cooled fast reactors. Ferritic / martensitic (F / M) steel is considered one of the most promising candidate cladding materials for lead-cooled fast reactors due to its superior high-temperature mechanical properties and resistance to radiation swelling. However, traditional commercial and re-developed F / M steels are not specifically designed for lead-cooled fast reactor cladding materials and still have considerable limitations in terms of high-temperature strength, creep resistance, and resistance to lead-bismuth corrosion.

[0004] In fourth-generation advanced nuclear energy systems, liquid lead or lead-bismuth eutectic (LBE) is used as a coolant. Corrosion of the liquid metal can alter the microstructure, composition, and surface morphology of the material, thus affecting its mechanical and physical properties. Therefore, the resistance of the cladding material to liquid LBE corrosion must be carefully considered when designing cladding materials for lead-based reactors. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide an Al and Ti-containing FeCrW-based ODS~F / M steel and its preparation method, which has finer and more dispersed precipitates and better high-temperature mechanical properties, and is suitable for cladding materials for lead-based reactors.

[0006] This invention provides a FeCrW-based ODS~F / M steel containing Al and Ti, which is made by sintering, hot rolling, and heat treatment of pre-alloyed powder and Y2O3 with a particle size ≤20nm. The amount of Y2O3 added is 0.3wt%~0.4wt% of the mass of the pre-alloyed powder. The pre-alloyed powder is composed of the following components in parts by weight: 9wt%~12.2wt%Cr, 1wt%~2wt%W, 0.3wt%~0.6wt%Mn, 0.2wt%~0.5wt% Ta and V, 0.01wt%~0.1wt% Zr and La, 0.15wt%~0.25wt%C, 0.1wt%~5.0wt% Al, 0.3wt%~0.5wt%Ti, The balance is Fe.

[0007] As a further technical solution, the amount of Y2O3 added is 0.35wt%~4wt% of the mass of the pre-alloyed powder.

[0008] As a further technical solution, 1wt%~3wt% Al is added to the pre-alloyed powder.

[0009] As a further technical solution, the pre-alloyed powder is composed of the following components in parts by weight: 11.8wt%~12.2wt% Cr, 1.4wt%~1.6wt% W, 0.3wt%~0.6wt% Mn, 0.2wt%~0.5wt% Ta and V, 0.01wt%~0.1wt% Zr and La, 0.18wt%~0.22wt% C, 1~2wt% Al, 0.3wt%~0.4wt% Ti, and the balance being Fe.

[0010] This invention provides a method for preparing FeCrW-based ODS~F / M steel containing Al and Ti, comprising the following steps: Step 1: Mix 9wt%~12.2wt% Cr powder, 1wt%~2wt% W powder, 0.3wt%~0.6wt% Mn powder, 0.2wt%~0.5wt% Ta and V powder, 0.01wt%~0.1wt% Zr and La powder, 0.15wt%~0.25wt% C powder, 0.1wt%~5.0wt% Al powder, 0.3wt%~0.5wt% Ti powder and iron powder to obtain pre-alloyed powder; Step 2: The pre-alloyed powder and Y2O3 with a particle size ≤20nm are ball-milled under inert gas protection to obtain alloyed powder; the amount of Y2O3 added is 0.1wt%~0.5wt% of the mass of the pre-alloyed powder. Step 3: Sift the powder through a 200-300 mesh sieve and a 500-600 mesh sieve in sequence, and then perform spark plasma sintering in a high-purity argon atmosphere. Step 4: Hot rolling the sintered material; Step 5: Perform final heat treatment on the material.

[0011] As a further technical solution, step 1 specifically involves mixing 11.8wt%~12.2wt% of Cr powder, 1.4wt%~1.6wt% of W powder, 0.3wt%~0.6wt% of Mn powder, 0.2wt%~0.5wt% of Ta and V powder, 0.01wt%~0.1wt% of Zr and La powder, 0.18wt%~0.22wt% of C powder, 1~2wt% of Al powder, 0.3wt%~0.4wt% of Ti powder, and iron powder to obtain a pre-alloyed powder.

[0012] As a further technical solution, in step 2, the ball-to-material ratio is 10~20:1, preferably 11~15:1; the filling coefficient is 0.4~0.6; the ball milling speed is 350~500 rpm; and the alloyed powder is obtained after ball milling for 50 h~80 h.

[0013] As a further technical solution, in step 3, during sintering, the temperature is heated to 1050℃~1150℃ at a rate of 100℃ / min~120℃ / min, the sintering pressure is 50 MPa~60 MPa, and the sintering time is 5 min~10 min.

[0014] As a further technical solution, in step 4, the hot rolling is a sheathed hot rolling, the hot rolling temperature is 1000℃~1200℃, the holding time is 30min~40min, the reduction is about 80%, the interval between each pass is 5min~10min, and the sheath is removed after hot rolling.

[0015] As a further technical solution, step 5 specifically includes: Step 5-1: Perform austenitizing treatment and normalizing: hold at 950℃~1150℃ for 60~120 minutes, quench, and water cool; Step 5-2: Perform stress relief and carbide precipitation tempering: hold at 700℃~750℃ for 90~100 minutes, then air cool.

[0016] Compared with the prior art, the Al and Ti-containing FeCrW-based ODS~F / M steel and its preparation method of the present invention have the following beneficial effects: (1) Materials in which ultrafine Y2O3 particles with extremely high thermal and chemical stability are dispersed in the alloy matrix. The added trace amount of nano Y2O3 particles not only hinders dislocation movement and improves the high temperature strength and high temperature creep performance of the material, but also the dispersed nano particles can effectively annihilate the defects caused by irradiation and enhance the radiation resistance of the material. (2) The addition of Al can not only improve the toughness and machinability of ODS alloy, but also form a dense Al2O3 film on the alloy surface, thereby effectively enhancing its resistance to LBE dissolution and corrosion; by adding a small amount of Ti, the oxide particles can be refined, thereby improving the high temperature strength of the material. (3) Based on ODS-F / M steel, aluminum is added to it. Through the synergistic effect of the elements, the prepared ODS-F / M steel exhibits higher mechanical properties and resistance to lead and bismuth corrosion. The reinforcing phase is finer and more uniform, and the tensile strength and yield strength at 550℃ and 600℃ are significantly improved. Attached Figure Description

[0017] Figure 1 The test curves show the mechanical properties of materials with different compositions at 550℃. Figure 2 This represents the mechanical property test curves of materials with different compositions at 600℃. Detailed Implementation

[0018] To further understand the present invention, embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, and not for limiting the present invention.

[0019] An embodiment of the present invention discloses a method for preparing FeCrW-based ODS~F / M steel containing Al and Ti, comprising the following steps: Step 1: Mix 9wt%~12.2wt% Cr powder, 1wt%~2wt% W powder, 0.3wt%~0.6wt% Mn powder, 0.2wt%~0.5wt% Ta and V powder, 0.01wt%~0.1wt% Zr and La powder, 0.15wt%~0.25wt% C powder, 0.1wt%~5.0wt% Al powder, 0.3wt%~0.5wt% Ti powder and iron powder to obtain pre-alloyed powder; Preferably, 11.8wt%~12.2wt% of Cr powder, 1.4wt%~1.6wt% of W powder, 0.3wt%~0.6wt% of Mn powder, 0.2wt%~0.5wt% of Ta and V powder, 0.01wt%~0.1wt% of Zr and La powder, 0.18wt%~0.22wt% of C powder, 1wt%~2wt% of Al powder, 0.3wt%~0.4wt% of Ti powder and iron powder are mixed to obtain pre-alloyed powder; Step 2: The pre-alloyed powder and Y2O3 with a particle size ≤20nm are ball-milled under inert gas protection to obtain alloyed powder; The amount of Y2O3 added is 0.1wt%~0.5wt% of the pre-alloyed powder mass, preferably 0.3wt%~0.4wt%, and more preferably 0.35wt%. Specifically, the ball-to-material ratio is 10~20:1, preferably 11~15:1; the filling coefficient is 0.4~0.6, preferably 0.45~0.5; the ball milling speed is 350~500 rpm, and the alloyed powder is obtained after ball milling for 50 h~80 h; Step 3: Sift the powder through a 200-300 mesh sieve and a 500-600 mesh sieve in sequence, and then perform spark plasma sintering in a high-purity argon atmosphere. Specifically, the powder is sieved through a 200-mesh sieve and a 500-mesh sieve in sequence. The sieved powder is then placed into a 20 mm diameter graphite mold in a vacuum glove box and sintered by spark plasma in a high-purity argon atmosphere. During sintering, the temperature is raised to 1050-1150℃ at a rate of 100℃ / min-120℃ / min, the sintering pressure is 50MPa-60MPa, and the sintering time is 5 min-10 min. Step 4: Hot rolling the sintered material; Hot rolling is enclosed hot rolling, with a hot rolling temperature of 1000℃~1200℃, preferably 1050℃~1100℃, a holding time of 30min~40min, a reduction of 78%~82%, and a holding interval of 5~10min between each pass. The enclosed sleeve is removed after hot rolling. Step 5: Perform final heat treatment on the material; Specifically, it includes: Step 5-1: Perform austenitizing treatment and normalizing: hold at 950℃~1150℃ for 60~120 minutes, quench, and water cool; Step 5-2: Perform stress relief and carbide precipitation tempering: hold at 700℃~750℃ for 90~100 minutes, then air cool.

[0020] An embodiment of the present invention discloses a FeCrW-based ODS~F / M steel containing Al and Ti, which is made by sintering, hot rolling and heat treatment of pre-alloyed powder and Y2O3 with a particle size ≤20nm. The amount of Y2O3 added is 0.3~0.4wt% of the mass of the pre-alloyed powder, preferably 0.35wt%. The pre-alloyed powder is composed of the following components in parts by weight: 9wt%~12.2wt%Cr, 1wt%~2wt%W, 0.3wt%~0.6wt%Mn, 0.2wt%~0.5wt% Ta and V, 0.01wt%~0.1wt% Zr and La, 0.15wt%~0.25wt%C, 0.1wt%~5.0wt% Al, 0.3wt%~0.5wt%Ti, The balance is Fe.

[0021] The pre-alloyed powder is preferably composed of 11.8wt%~12.2wt% Cr powder, 1.4wt%~1.6wt% W powder, 0.3wt%~0.6wt% Mn powder, 0.2wt%~0.5wt% Ta and V powder, 0.01wt%~0.1wt% Zr and La powder, 0.18wt%~0.22wt% C powder, 1wt%~2wt% Al powder, and 0.3wt%~0.4wt% Ti powder.

[0022] In the FeCrW-based ODS~F / M steel containing Al and Ti, the content of impurities such as P, S, and O is <0.003%, and the N content is <0.02%.

[0023] The Al and Ti-containing FeCrW-based ODS~F / M steel of this invention not only exhibits good resistance to lead-bismuth corrosion, but also features finer reinforcing phases and significantly improved high-temperature mechanical properties at 550℃ and 600℃. It can be used as a core structural material for fuel element cladding, lattice, etc., in lead-cooled fast reactors and other Generation IV reactors, providing theoretical guidance and technical foundation for the continuous improvement of cladding materials for lead-cooled fast reactors in advanced nuclear energy systems. This has positive exploratory significance for improving the safety and economy of fuel elements in advanced nuclear reactors.

[0024] To further understand the present invention, the FeCrW-based ODS~F / M steel and its preparation method provided by the present invention will be described in detail below with reference to the embodiments. The scope of protection of the present invention is not limited by the following embodiments.

[0025] Example 1: (1) Mix 11.8wt%Cr, 0.2wt%C, 1.5wt%W, 0.5wt%Mn, 0.4wt%(Ta+V), 0.06wt%(Zr+La), 1.0wt%Al, and 0.3wt%Ti alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.35 wt% Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity 99.99%) was passed through for protection. The ball-to-powder ratio was 10:1 and the filling coefficient was 0.4. The ball milling speed was 350 rpm, and the alloyed powder was obtained after 50 h of ball milling. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1050℃ at a rate of 100℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1100℃, the holding time is 30 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1100℃ for 60 minutes, quench, and water cool; (6) Then stress relief and carbide precipitation tempering are performed on the material: hold at 750℃ for 90 minutes and air cool.

[0026] (7) The tensile strength of the 1Al+0.3Ti-FeCrW-based ODS-F / M steel obtained at 550℃ was 762.09 MPa, and the tensile strength at 600℃ was 569.62 MPa.

[0027] Comparative Example 1 (1) Mix 11.8wt%Cr, 0.2wt%C, 1.5wt%W, 0.5wt%Mn, 0.4wt%(Ta+V), and 0.06wt%(Zr+La) alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder was placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity 99.99%) was passed through for protection. The ball-to-powder ratio was 10:1 and the filling coefficient was 0.4. The ball milling speed was 350 rpm, and the alloyed powder was obtained after 50 h of ball milling. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1050℃ at a rate of 100℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1100℃, the holding time is 30 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1100℃ for 60 minutes, quench, and water cool; (6) Then stress relief and carbide precipitation tempering are performed on the material: hold at 750℃ for 90 minutes and air cool.

[0028] The final FeCrW-based F / M steel has a tensile strength of 540.41 MPa at 550℃ and a tensile strength of 436.86 MPa at 600℃.

[0029] Comparative Example 2 (1) Mix 11.8wt%Cr, 0.2wt%C, 1.5wt%W, 0.5wt%Mn, 0.4wt%(Ta+V), and 0.06wt%(Zr+La) alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.35% by mass of Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity of 99.99%) was passed through for protection. The ball-to-powder ratio was 10:1 and the filling coefficient was 0.4. The ball milling speed was 350 rpm, and the alloyed powder was obtained after 50 h of ball milling. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1050℃ at a rate of 100℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1100℃, the holding time is 30 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1100℃ for 60 minutes, quench, and water cool; (6) Then stress relief and carbide precipitation tempering are performed on the material: hold at 750℃ for 90 minutes and air cool.

[0030] The final FeCrW-based ODS-F / M steel has a tensile strength of 590.72 MPa at 550℃ and a tensile strength of 430.735 MPa at 600℃.

[0031] Comparative Example 3: (1) Mix 11.8wt%Cr, 0.2wt%C, 1.5wt%W, 0.5wt%Mn, 0.4wt%(Ta+V), 0.06wt%(Zr+La), and 1.0wt%Al alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.35% by mass of Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity of 99.99%) was passed through for protection. The ball-to-powder ratio was 10:1 and the filling coefficient was 0.4. The ball milling speed was 350 rpm, and the alloyed powder was obtained after 50 h of ball milling. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1050℃ at a rate of 100℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1100℃, the holding time is 30 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1100℃ for 60 minutes, quench, and water cool; (6) Then stress relief and carbide precipitation tempering are performed on the material: hold at 750℃ for 90 minutes and air cool.

[0032] The final 1Al-FeCrW-based ODS-F / M steel has a tensile strength of 598.785 MPa at 550℃ and a tensile strength of 483.945 MPa at 600℃.

[0033] Table 1 Chemical composition (mass fraction) of F / M steels with different compositions / % Table 2. High-Temperature Mechanical Properties Test Results of F / M Steels with Different Compositions like Figures 1-2 As shown, the material prepared in Example 1 of the present invention has excellent tensile strength and yield strength at 550°C and 600°C.

[0034] The material prepared in Example 1 showed a 35% increase in high-temperature yield strength at 550°C compared to the material prepared in Comparative Example 3; and a 38% increase in high-temperature yield strength at 550°C compared to the material prepared in Comparative Example 2. The material prepared in Example 1 showed a 25.59% increase in high-temperature yield strength at 600°C compared to the material prepared in Comparative Example 3; and a 33% increase in high-temperature yield strength at 550°C compared to the material prepared in Comparative Example 2.

[0035] Example 2 (1) Mix 12wt%Cr, 0.21wt%C, 1.4wt%W, 0.52wt%Mn, 0.3wt%(Ta+V), 0.05wt%(Zr+La), 1.1wt%Al, and 0.3wt%Ti alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.35wt% Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity 99.99%) was passed through for protection. The ball-to-powder ratio was 9:1 and the filling coefficient was 0.5. The ball milling speed was 400 rpm, and the alloyed powder was obtained after ball milling for 50 h. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1100℃ at a rate of 105℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1080℃, the holding time is 40 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1000℃ for 100 minutes, quench, and water cool; (6) Then stress relief and carbide precipitation tempering of the material: hold at 730℃ for 100 minutes and air cool.

[0036] The final FeCrW-based ODS-F / M steel has a tensile strength of 761.25 MPa and a yield strength of 683.2 MPa at 550℃; and a tensile strength of 562.96 MPa and a yield strength of 505.9 MPa at 600℃.

[0037] Example 3 (1) Mix 10.9wt%Cr, 0.18wt%C, 2wt%W, 0.3wt%Mn, 0.2wt%(Ta+V), 0.1wt%(Zr+La), 1.2wt%Al, and 0.4wt%Ti alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.4 wt% Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity 99.99%) was passed through for protection. The ball-to-powder ratio was 11:1 and the filling coefficient was 0.4. The ball milling speed was 400 rpm, and the alloyed powder was obtained after ball milling for 50 h. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1120℃ at a rate of 101℃ / min, sintering pressure of 50 MPa, and sintering time of 6 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1120℃, the holding time is 30 min, the reduction is about 80%, and the interval between each pass is 6 min. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 950℃ for 120 minutes, quench, and water cool; (6) Then the material is subjected to stress relief and carbide precipitation tempering: hold at 700℃ for 100 minutes and air cool.

[0038] The final FeCrW-based ODS-F / M steel has a tensile strength of 761 MPa and a yield strength of 686 MPa at 550℃; and a tensile strength of 566.36 MPa and a yield strength of 510 MPa at 600℃.

[0039] Example 4 (1) Mix 12.2wt%Cr, 0.23wt%C, 2wt%W, 0.6wt%Mn, 0.5wt%(Ta+V), 0.1wt%(Zr+La), 5wt%Al, and 0.5wt%Ti alloy powders in proportion, with the remainder being Fe. All of the above are mass percentages. (2) The pre-alloyed powder and 0.4 wt% Y2O3 (i.e., oxide dispersion strengthening phase) were placed in a ball mill jar in a vacuum glove box. Before ball milling, pure argon gas (purity 99.99%) was passed through for protection. The ball-to-powder ratio was 10:1 and the filling coefficient was 0.5. The ball milling speed was 400 rpm, and the alloyed powder was obtained after ball milling for 50 h. (3) Use 200 mesh and 500 mesh screens to sieve, put the sieved powder into a graphite mold with a diameter of 20 mm in a vacuum glove box, and perform spark plasma (SPS) sintering in a high-purity argon environment. Heat to 1150℃ at a rate of 110℃ / min, sintering pressure of 50 MPa, and sintering time of 5 min. (4) After sintering, the material is hot rolled. The hot rolling is a cladding hot rolling. The hot rolling temperature is 1100℃, the holding time is 30 min, the reduction is about 80%, and the holding time is 5 min between each pass. After hot rolling, the cladding is removed. (5) After rolling, perform austenitizing treatment and normalizing: hold at 1150℃ for 65 minutes, quench, and water cool; (6) Then the material is subjected to stress relief and carbide precipitation tempering: 750℃ for 90 minutes, followed by air cooling.

[0040] The final FeCrW-based ODS-F / M steel has a tensile strength of 758 MPa and a yield strength of 640 MPa at 550℃; and a tensile strength of 550 MPa and a yield strength of 500 MPa at 600℃.

[0041] The above description of the embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

[0042] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A FeCrW-based ODS~F / M steel containing Al and Ti, characterized in that, It is made by sintering, hot rolling and heat treatment of pre-alloyed powder and Y2O3 with a particle size ≤20nm. The amount of Y2O3 added is 0.3wt%~0.4wt% of the mass of the pre-alloyed powder. The pre-alloyed powder is composed of the following components in parts by weight: 9wt%~12.2wt%Cr, 1wt%~2wt%W, 0.3wt%~0.6wt%Mn, 0.2wt%~0.5wt% Ta and V, 0.01wt%~0.1wt% Zr and La, 0.15wt%~0.25wt%C, 0.1wt%~5.0wt% Al, 0.3wt%~0.5wt%Ti, The balance is Fe.

2. The FeCrW-based ODS~F / M steel containing Al and Ti according to claim 1, characterized in that, The amount of Y2O3 added is 0.35wt% to 4wt% of the mass of the pre-alloyed powder.

3. The FeCrW-based ODS~F / M steel containing Al and Ti according to claim 1, characterized in that, The pre-alloyed powder contains 1wt%~3wt% Al.

4. The FeCrW-based ODS~F / M steel containing Al and Ti according to claim 1, characterized in that, The pre-alloyed powder is composed of the following components in parts by weight: 11.8wt%~12.2wt% Cr, 1.4wt%~1.6wt% W, 0.3wt%~0.6wt% Mn, 0.2wt%~0.5wt% Ta and V, 0.01wt%~0.1wt% Zr and La, 0.18wt%~0.22wt% C, 1~2wt% Al, 0.3wt%~0.4wt% Ti, and the balance being Fe.

5. A method for preparing FeCrW-based ODS~F / M steel containing Al and Ti, characterized in that, Includes the following steps: Step 1: Mix 9wt%~12.2wt% Cr powder, 1wt%~2wt% W powder, 0.3wt%~0.6wt% Mn powder, 0.2wt%~0.5wt% Ta and V powder, 0.01wt%~0.1wt% Zr and La powder, 0.15wt%~0.25wt% C powder, 0.1wt%~5.0wt% Al powder, 0.3wt%~0.5wt% Ti powder and iron powder to obtain pre-alloyed powder; Step 2: The pre-alloyed powder and Y2O3 with a particle size ≤20nm are ball-milled under inert gas protection to obtain alloyed powder; the amount of Y2O3 added is 0.1wt%~0.5wt% of the mass of the pre-alloyed powder. Step 3: Sift the powder through a 200-300 mesh sieve and a 500-600 mesh sieve in sequence, and then perform spark plasma sintering in a high-purity argon atmosphere. Step 4: Hot rolling the sintered material; Step 5: Perform final heat treatment on the material.

6. The method for preparing FeCrW-based ODS~F / M steel containing Al and Ti according to claim 5, characterized in that, Step 1 specifically involves mixing 11.8wt%~12.2wt% of Cr powder, 1.4wt%~1.6wt% of W powder, 0.3wt%~0.6wt% of Mn powder, 0.2wt%~0.5wt% of Ta and V powder, 0.01wt%~0.1wt% of Zr and La powder, 0.18wt%~0.22wt% of C powder, 1~2wt% of Al powder, 0.3wt%~0.4wt% of Ti powder, and iron powder to obtain a pre-alloyed powder.

7. The method for preparing FeCrW-based ODS~F / M steel containing Al and Ti according to claim 5, characterized in that, In step 2, the ball-to-material ratio is 10~20:1, preferably 11~15:1; the filling coefficient is 0.4~0.6; the ball milling speed is 350~500 rpm; and the alloyed powder is obtained after ball milling for 50 h~80 h.

8. The method for preparing FeCrW-based ODS~F / M steel containing Al and Ti according to claim 5, characterized in that, In step 3, during sintering, the temperature is raised to 1050℃~1150℃ at a rate of 100℃ / min~120℃ / min, the sintering pressure is 50MPa~60MPa, and the sintering time is 5 min~10 min.

9. The method for preparing FeCrW-based ODS~F / M steel containing Al and Ti according to claim 5, characterized in that, In step 4, the hot rolling is a sheathed hot rolling, the hot rolling temperature is 1000℃~1200℃, the holding time is 30min~40min, the reduction is 80%, the interval between each pass is 5min~10min, and the sheath is removed after hot rolling.

10. The method for preparing FeCrW-based ODS~F / M steel containing Al and Ti according to claim 5, characterized in that, Step 5 specifically includes: Step 5-1: Perform austenitizing treatment and normalizing: hold at 950℃~1150℃ for 60~120 minutes, quench, and water cool; Step 5-2: Perform stress relief and carbide precipitation tempering: hold at 700℃~750℃ for 90~100 minutes, then air cool.