A high-strength, high-toughness, wear-resistant, and corrosion-resistant steel for chains, its manufacturing method, and heat treatment process.

Through composition design and process optimization, ultrafine-grained high-strength, tough, wear-resistant, and corrosion-resistant chain steel was prepared, solving the problems of strength, toughness, wear resistance, and corrosion resistance of existing mooring chain steel in deep-sea environments, and realizing high-performance chain materials.

CN123108435APending Publication Date: 2026-11-17МААНЬШАНЬ АЙРОН ЭНД СТИЛ КО ЛТД
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202611269197.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing mooring chain steel lacks sufficient strength and toughness in deep-sea environments, making it difficult to withstand extreme loads. Furthermore, it suffers from high corrosion rates and significant wear due to seawater corrosion, microbial adhesion, and silt abrasion, which limits the service life and safety of the chain.

Method used

Through composition design and process optimization, using φ600mm large round billets, controlled smelting, casting, high rolling ratio, controlled rolling and controlled cooling processes, combined with graded quenching and tempering heat treatment, ultra-fine grain high strength, toughness, wear resistance and corrosion resistance chain steel is prepared. The precipitation coefficient, wear resistance factor and corrosion resistance factor are controlled to ensure the steel's microstructure is refined and its performance is stable.

Benefits of technology

It achieves a yield strength ≥1150MPa, tensile strength ≥1300MPa, yield-to-tensile ratio ≤0.92, KV2 ≥130J at -20℃, wear rate ≤0.023/mm/thousand working hours, and average corrosion rate ≤0.145g/(m2·h), meeting the stringent requirements of deep-sea mooring and coal mining environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108435A_ABST
    Figure CN123108435A_ABST
Patent Text Reader

Abstract

This invention provides an ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel, its manufacturing method, and heat treatment process. The composition meets the following requirements: Q = 80 × (2.5 × %N - 0.8 × %Al - 1.3 × %Ti) / 13 ≥ 0.060; A = (2.4 × %Cr + 1.6 × %Mo + 3.7 × %Si × %Mn) × (1 + 1.3 × %V × %Cr × %Mo) ≥ 18; X = (12.6 × %Ni + 5.2 × %Cr - 2.1 × %Si - 0.9 × %Cu × %Ni - 1.2 × %Mn) × (1 + 0.7% × Cu) ≥ 68. Compared with existing technologies, this invention combines ultrafine-grained strengthening, nanoprecipitation toughening, and weather-resistant alloy design. By controlling the heating temperature and time during quenching and controlling the cooling through staged quenching, the microstructure is further refined, thus meeting the requirements of harsh marine mooring and coal mining environments.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of alloy steel, and in particular relates to an ultrafine-grained high-strength, high-toughness, wear-resistant and corrosion-resistant chain steel, its manufacturing method and heat treatment process, and the product can meet the more stringent requirements of marine mooring. Background Technology

[0002] As global marine resource development accelerates into deeper waters, marine facilities such as deep-sea oil and gas platforms and floating wind power units are placing increasingly stringent demands on mooring chain performance. Traditional mooring chain steel suffers from insufficient strength and toughness, making it difficult to withstand extreme loads in the deep sea. Existing materials, under the combined effects of seawater corrosion, microbial adhesion, and sediment abrasion, exhibit an average annual corrosion rate exceeding 0.5 mm / year, with wear rates three times that of conventional marine anchor chain steel. These factors significantly limit the service life and operational safety of the chains.

[0003] Patent CN106521356A, published on March 22, 2017, discloses a high-strength, high-toughness, corrosion-resistant steel for chains and its heat treatment method. The chemical composition, by weight percentage (wt.%), is: C: 0.06-0.11 wt.%, Si: 0.15-0.35 wt.%, Mn: 0.30-0.50 wt.%, Cr: 1.00-3.00 wt.%, Ni: 2.00-4.00 wt.%, Mo: 0.30-0.60 wt.%, Nb: 0.02-0.06 wt.%, V: 0.03-0.09 wt.%, P < 0.015 wt.%, S < 0.015 wt.%, with the balance being Fe and unavoidable impurities. This patent employs an ultra-low carbon design, primarily using a vertical continuous heat treatment furnace and a process of two quenching heat treatments and one tempering heat treatment. However, its steel strength and toughness are generally low, so it can only be used for lower-grade chain steel.

[0004] Therefore, it is essential to provide a high-strength and high-toughness chain steel to meet the requirements of marine mooring applications. Summary of the Invention

[0005] The purpose of this invention is to provide an ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel and its manufacturing method. Through composition design, using φ600mm large round billets, controlled smelting, casting, high rolling ratio, controlled rolling and controlled cooling processes, low segregation, high homogeneity ultrafine-grained round steel (φ20-100mm) material is obtained.

[0006] Another objective of this invention is to provide a heat treatment process for ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel. Using the steel produced above, a matching heat treatment process is designed. By controlling the heating temperature and time during round steel quenching and controlling the cooling through staged quenching, the microstructure is further refined to meet the performance requirements of the round steel design.

[0007] The specific technical solution of this invention is as follows:

[0008] A type of ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel comprises the following components by weight percentage:

[0009] C 0.20%-0.25%, Si 0.50%-0.60%, Mn 1.55%-1.75%, Cr 2.30%-2.60%, Mo 1.10%-1.25%, Ni 3.80%-4.20%, Al≤0.015%, V 0.15-0.25%, Cu 0.15-0.25%, Ti≤0.0050%, P≤0.015%, S≤0.005%, N 0.0080-0.012%, with the remainder being Fe and other unavoidable impurities.

[0010] The composition of the steel used in the ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain also meets the following requirements:

[0011] The precipitation coefficient Q ≥ 0.060; Q = 80 × (2.5 × %N - 0.8 × %Al - 1.3 × %Ti) / 13;

[0012] Wear resistance factor A≥18; A=(2.4×%Cr+1.6×%Mo+3.7×%Si×%Mn)×(1+1.3×%V×%Cr×%Mo)

[0013] Corrosion resistance factor X≥68; X=(12.6×%Ni+5.2×%Cr-2.1×%Si-0.9×%Cu×%Ni-1.2×%Mn)×(1+0.7%Cu).

[0014] When calculating using the above formula, each element represents its mass content × 100. Simply substitute the data before the % sign into the formula to calculate.

[0015] This invention provides a method for manufacturing ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel. Through controlled smelting and casting of φ600mm large round billets and high rolling ratios combined with controlled rolling and cooling, low-segregation, high-homogeneity ultrafine-grained round steel (φ20-100mm) material is obtained. Based on 100t of molten steel per heat, the specific process includes the following steps:

[0016] Smelting → LF furnace refining → RH vacuum degassing → continuous casting → 250 cubic meter intermediate billet rolling → hot delivery heating → round steel rolling → finishing → packaging and warehousing.

[0017] The smelting process employs an electric furnace or converter, with the final P content controlled to be ≤0.006%.

[0018] The LF furnace refining process requires the white slag to be held for ≥20 minutes.

[0019] The RH vacuum degassing process involves an RH vacuum time of ≥25 min, a calcium feeding line of 25-35 meters, and a soft blowing time of 15-25 min.

[0020] In the above process, the control of the final P content ensures the residual P requirement of the finished product; the white slag retention time is mainly considered based on the desulfurization and deoxidation effect of this steel grade; parameters such as vacuum degassing are limited according to the steel quality requirements such as residual H, inclusion level purity requirements, etc., and the degassing time, calcium line, soft blowing parameters are limited, together with the composition design to ensure service life and other performance.

[0021] The continuous casting process yields φ600 round billets. The casting employs induction heating in the tundish with narrow-range low superheat control (15-25℃), and the crystallizer level fluctuation is controlled within ±5mm. Simultaneously, low casting speed control is implemented (0.29-0.31 m / min). The electric stirring parameters are configured as follows: crystallizer stirring: 1.5Hz / 400A; casting stream stirring: 6.0Hz / 180A; end stirring: 5.0Hz / 500A. The continuously cast billets are promptly placed into the cooling pit for slow cooling, with a pit temperature ≥200℃, billet temperature upon entry ≥600℃, slow cooling time ≥72h, and exit temperature ≤200℃. Rolling is performed immediately after exiting the pit. The low-magnification quality of the cast billets is controlled according to YB / T 153 standard, meeting the requirements of central porosity, general porosity, segregation ≤1.0, and the proportion of equiaxed crystal zones in the core being 20-25%. Continuous casting significantly impacts the purity, density, and homogeneity of this steel grade. This is achieved by limiting billet size and the continuous casting process. The combination of superheat, casting speed range, and matching electric stirring parameters greatly influences the control of core quality and liquid core solidification. Slow cooling parameters for this steel grade ensure core quality and reduce stress. Furthermore, specific time and temperature controls are needed for hydrogen removal from the center of this large-section round billet.

[0022] The 250mm square intermediate billet rolling refers to heating a φ600mm continuous casting billet, controlling the temperature of the preheating section to ≤750℃, and holding it at 1250±10℃ in the soaking section for 8-10 hours for high-temperature diffusion, and rolling it into an intermediate billet with a size of 250mm×250mm.

[0023] The hot-feeding heating process involves directly hot-feeding intermediate billets to roll round steel with a diameter of φ20-100mm. The temperature of the billets entering the furnace is controlled at ≥600℃, and the total heating time is ≥180min before being rolled out of the furnace.

[0024] The round steel rolling process employs controlled rolling and cooling, controlling the initial rolling temperature at 1080±10℃, the final rolling temperature at 800-840℃, and the final rolling deformation at 25-30%. High-temperature diffusion during rolling ensures high homogeneity, while a high rolling ratio ≥40, combined with the controlled rolling process, guarantees a round steel grain size ≥11.0, increasing interfacial energy to promote dispersed carbide precipitation and enhance toughness. Final rolling at 800-840℃ within the non-recrystallization range, coupled with a 25%-30% final rolling deformation and a high rolling ratio of not less than 40, fully flattens and elongates the austenite grains, generating high-density dislocations and numerous deformation substructures, significantly increasing grain boundary interfacial energy. The high-density interface can provide sufficient nucleation sites for V (C,N) nano-precipitates, promoting fine and dispersed precipitation of carbides. It can also refine the original grains through dislocation segmentation and, together with the precipitates pinning grain boundaries, inhibit grain growth, ultimately resulting in a stable ultrafine grain structure of grade 11 or higher.

[0025] To ensure sufficient hydrogen diffusion and removal at the center of the round steel, the round steel is immediately placed in a pit for slow cooling after coming off the production line. The pit temperature is ≥650℃. The cooling rate is controlled as follows: when the round steel temperature is between 500℃ and 350℃, the cooling rate is ≤15℃ / h; when the round steel temperature is between 150℃ and 350℃, the cooling rate is ≤10℃ / h; the steel is removed from the pit when the temperature is ≤150℃. Due to the hydrogen sensitivity of this steel grade, the core of the round steel is thoroughly dehydrogenated.

[0026] This invention provides a heat treatment process for ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel. Utilizing the steel produced above, the microstructure is further refined through controlled quenching temperature and time, combined with staged quenching and controlled cooling, to meet the performance requirements of the round steel design. The heat treatment includes staged quenching and tempering.

[0027] The graded quenching process is as follows: heating at ≤80℃ / min to 860±5℃ and holding at that temperature for (1.25-1.30)×d min, where d is the diameter of the round steel in mm. The value before mm is substituted into the formula for calculation. Then, cooling is performed. When the round steel temperature is >450℃, the cooling rate is controlled at 50±5℃ / s. When the temperature is 200℃ < ≤450℃, the cooling rate is 25±5℃ / s. When the temperature drops below 200℃, deep cryogenic treatment is performed at -120℃ for 2 hours. After sufficient austenitization, the high-temperature section ensures a high cooling rate to promote phase transformation, while the low-temperature section reduces quenching stress. Deep cryogenic treatment promotes sufficient phase transformation and improves the comprehensive mechanical properties of the material.

[0028] The tempering process involves immediately removing the steel after graded quenching and then performing high-temperature tempering. The specific tempering process is as follows: heat the steel to 580±5℃ at a rate of ≤80℃ / min, hold for (1.55-1.60)×d min, and then cool it at a cooling rate of 20-30℃ / s. d is the diameter of the round steel in mm. The value before mm is substituted into the formula for calculation.

[0029] After heat treatment, the product's steel microstructure has a grain size ≥11.0, yield strength ≥1150MPa, tensile strength ≥1300MPa, yield-to-tensile ratio ≤0.92, KV2 ≥130J at -20℃, elongation A ≥15%, reduction of area ≥56%, wear rate ≤0.023 g / mm / thousand working hours, and average corrosion rate ≤0.145 g / (m²). 2 ·h);

[0030] After heat treatment, the microstructure of the round steel 1 / 6D is 100% tempered sorbite with carbide size ≤90nm.

[0031] This heat treatment process is highly compatible with the composition of the Cr-Mo-Ni-V-Cu-N alloy system of this invention. Precise austenitization at 860±5℃ ensures complete solid solution of Cr, Mo, and V alloy carbides. Utilizing a high hardenability alloy system, combined with segmented gradient rapid cooling, it quickly avoids the bainitic phase transformation range, preventing the formation of abnormally brittle structures. Deep cryogenic treatment at -120℃ after quenching promotes the full transformation of residual austenite, and the pinning effect of V (C,N) precipitates stabilizes the ultrafine grain structure. High-temperature tempering at 580±5℃ eliminates residual quenching stress and precipitates dispersed hard Cr, Mo, and V carbides, improving low-temperature toughness and wear resistance while ensuring high strength. Finally, a 1 / 6D cross-section yields 100% uniform fine tempered sorbite with a stable grain size ≥11, achieving a synergistic match of high strength, high toughness, wear resistance, and corrosion resistance, effectively reducing performance dispersion caused by process fluctuations.

[0032] The design concept of this invention is as follows:

[0033] Carbon (C): Carbon is the cheapest strengthening element in steel. Each 0.1% increase in dissolved C can increase strength by 400-450 MPa. C forms precipitates with alloying elements in steel, resulting in precipitation strengthening. C significantly improves hardenability, making it easier to obtain martensitic structure in the core during oil well tubing preparation. However, as its content increases, plasticity and toughness decrease, and high C content makes welding chain links difficult. Therefore, the C content is controlled at 0.20%-0.25%.

[0034] Si: Si is an effective solid solution strengthening element in steel, increasing its strength and hardness. Si also acts as a deoxidizer during steelmaking. However, Si tends to segregate at austenite grain boundaries, reducing grain boundary bonding and causing brittleness. Furthermore, Si easily causes elemental segregation in steel. Therefore, the Si content should be controlled between 0.50% and 0.60%.

[0035] Mn: As a major strengthening element and austenite stabilizing element, Mn can significantly improve the hardenability of steel and reduce decarburization. However, excessive Mn will increase the risk of temper brittleness. Therefore, the Mn content should be controlled between 1.55% and 1.75%.

[0036] Cr: Cr is a carbide-forming element. Cr can improve the hardenability and strength of steel, but it easily causes temper brittleness. However, excessive Cr content will increase crack susceptibility. The Cr content should be controlled between 2.30% and 2.60%.

[0037] Mo: Mo greatly improves the hardenability of steel. Mo dissolved in the matrix enables the steel microstructure to maintain high stability during tempering and effectively reduces the segregation of impurity elements such as P, S, and As at grain boundaries, thereby improving the toughness of the steel and reducing temper brittleness. This invention appropriately increases the Mo content to improve the temper brittleness caused by Cr and Ni, the main alloying and toughening elements, and reduces heat treatment sensitivity. Therefore, the Mo content is controlled at 1.10%-1.25%.

[0038] Ni: Ni can form an infinitely miscible solid solution with Fe. It is an austenite stabilizing element, expanding the phase region, increasing the stability of supercooled austenite, shifting the C-curve to the right, and improving the hardenability of steel. Ni can refine the width of martensite laths, increasing strength. Ni significantly lowers the ductile-brittle transition temperature of steel and improves low-temperature toughness. The Ni content should be controlled between 3.80% and 4.20%.

[0039] Cu: Cu significantly improves the corrosion resistance of steel; adding 0.1% Cu to steel can significantly enhance its corrosion resistance. However, excessive Cu content can easily cause hot brittleness during hot rolling or forging. Considering all factors, the Cu content should be controlled within the range of 0.15-0.25%.

[0040] With an Al content of ≤0.015%, the Al content is controlled to ensure that the N element is not excessively consumed and to guarantee the precipitation effect. On the other hand, the lower Al content is beneficial to prevent weld oxidation during the subsequent welding process of the chain, thus ensuring the weld quality of the high alloy finished chain.

[0041] Vanadium (V) primarily functions to refine grain size, reduce overheating sensitivity, and increase tempering stability and toughness, thereby extending service life. Furthermore, due to its strong affinity for nitrogen, vanadium can fix nitrogen in steel, forming VN and promoting the formation of fine eutectic carbides. This invention controls the V content to be 0.15%-0.25%.

[0042] [N]: Trace amounts of nitrogen can promote the precipitation of V(C,N), increase the quantity and stability of undissolved carbides in quenched steel, and act as a nucleation core to reduce the size of eutectic carbides such as Cr23C6. This enhances the overall performance of steel by increasing grain refinement and precipitation strengthening, thereby improving the material's thermal strength and toughness. In this invention, [N] is controlled at 80-120 ppm.

[0043] This invention precisely controls the amount of trace nitrogen (0.0080%-0.012%) to fully activate the precipitation strengthening effect of vanadium (V). Nitrogen combines with vanadium to generate a large number of dispersed and stable nano-V (C,N) precipitates, which can both pin austenite grain boundaries at high temperatures, inhibit grain coarsening, and achieve ultrafine grain strengthening; and also act as heterogeneous nucleation sites, guiding Cr during tempering. 23 The uniform precipitation of C6-type carbides prevents their aggregation along grain boundaries, thus avoiding the formation of a coarse, brittle network structure. The carbide size is controlled to within 90 nm, with spherical particles dispersed throughout the matrix. These fine precipitates not only hinder dislocation slip during friction, improving wear resistance, but also suppress crack propagation, thus improving low-temperature toughness. Since Al and Ti preferentially bind to nitrogen, consuming the effective nitrogen source, this invention sets a precipitation coefficient Q ≥ 0.060 to constrain the composition ratio, ensuring sufficient effective nitrogen within the steel and stably achieving the designed precipitation strengthening effect.

[0044] Q=80×(2.5×%N-0.8×%Al-1.3×%Ti) / 13;

[0045] To ensure the wear resistance of steel, certain constraints need to be placed on the main active elements in the steel. The wear resistance factor is defined as A, where A = (2.4 × %Cr + 1.6 × %Mo + 3.7 × %Si × %Mn) × (1 + 1.3 × %V × %Cr × %Mo), and A ≥ 18. Existing mooring chain steels rely solely on Cr and Mo to improve wear resistance, neglecting the coupling effect of matrix solid solution strengthening and multi-alloy synergistic precipitation strengthening. Under the conditions of repeated scouring and alternating friction of deep-sea sediment, abrasive wear and fatigue spalling failure are easily caused by local plastic rheology and intergranular coarsening and aggregation of hard carbides. At the same time, conventional single-element range constraints cannot take into account the microstructure evolution during austenitization and high-temperature tempering. Small fluctuations in heat treatment processes can cause differences in carbide morphology and size, ultimately resulting in large dispersion in the wear resistance performance of batches. Based on the aforementioned industry pain points, this invention innovatively constructs a quantitative evaluation formula for wear resistance factor A. It fits the contribution weights of each element from three dimensions: matrix solid solution wear resistance, alloy carbide precipitation wear resistance, and multi-element synergistic gain, achieving precise pre-constraints on wear resistance performance. The first part of the formula is the matrix solid solution wear resistance contribution term: 2.4×%Cr+1.6×%Mo+3.7×%Si×%Mn. Cr and Mo, as strong carbide-forming elements, can be fully dissolved into the austenitic matrix during the austenitization stage at 860±5℃. After high-temperature tempering at 580±5℃, they precipitate dispersed hard alloy carbides, effectively hindering dislocation slip under frictional loads and resisting abrasive indentation and plastic deformation. Based on extensive isothermal quenching and tempering friction and wear test data, it is found that Cr contributes the most to hardness improvement and wear resistance, therefore it is assigned a weight of 2.4, followed by Mo at 1.6. The addition of Si and Mn composites can significantly improve the work hardening ability of the matrix. A high-hardness work hardened layer can be quickly formed in the friction contact area to resist repeated shear wear. The synergistic strengthening effect of the two is far greater than that of a single element. Therefore, the cross term Si×Mn is used and given the highest weight of 3.7 to accurately characterize the synergistic solid solution wear resistance gain effect of Si-Mn. The second part of the formula is the multi-element synergistic precipitation correction term 1+1.3×%V×%Cr×%Mo. This invention relies on the VN microalloying system. During tempering, V (C,N) nano-precipitates and Cr and Mo carbides mutually adhere to each other and nucleate, which greatly improves the quantity and dispersion uniformity of hard precipitates and avoids Cr 23C6 coarsens along the grain network, reducing the risk of brittle spalling and further amplifying wear resistance. 1.3 is the experimental fitting correction coefficient for the synergistic wear resistance of the three elements, used to quantify the gain in wear resistance under the combined effect of V, Cr, and Mo. Combining multiple sets of gradient composition samples for friction and wear verification, a threshold A≥18 was set to ensure that the steel simultaneously possesses a dual wear resistance mechanism of high solid solution matrix hardness and dispersed hard multi-component precipitates. Even with reasonable fluctuations in heat treatment holding and cooling parameters, the size and distribution of carbides can remain stable, ultimately controlling the wear rate to within 0.023 mm / thousand working hours. This addresses the shortcomings of traditional chain steel in terms of unstable wear resistance and easy wear failure in deep-sea conditions from the composition design perspective.

[0046] To ensure good corrosion resistance, the proportions of elements such as Si, Mn, Cu, Ni, and Cr need to be optimized, requiring the corrosion resistance factor X to satisfy X≥68; X = (12.6×%Ni + 5.2×%Cr - 2.1×%Si - 0.9×%Cu×%Ni - 1.2×%Mn) × (1 + 0.7%Cu). Traditional corrosion-resistant chain steels often limit the upper and lower limits of Cr, Ni, and Cu elements individually, without considering the interaction between elements and the risk of galvanic corrosion caused by microsegregation. On the one hand, Si and Mn are prone to microsegregation during casting, rolling, and heat treatment, forming compositional micro-regions in the matrix and inducing localized electrochemical pitting corrosion in seawater. On the other hand, when the Cu and Ni proportions are unbalanced, Cu-rich precipitates are easily formed at grain boundaries, creating a potential difference with the matrix and accelerating corrosion. Constraining the range of a single element cannot avoid the corrosion resistance degradation caused by the interaction of these elements. To address the highly corrosive service environment of deep-sea high-salt and microbial adhesion, this invention constructs a corrosion resistance factor X quantitative model. Based on the passivation film formation mechanism and electrochemical corrosion potential law, it fits the positive and negative weights of each element, balancing the ratio of beneficial corrosion-resistant elements to harmful elements prone to segregation, thus achieving precise and controllable corrosion resistance performance. In the main formula 12.6×%Ni+5.2×%Cr-2.1×%Si-0.9×%Cu×%Ni-1.2×%Mn, Ni can increase the substrate electrode potential, while optimizing the density and self-healing ability of the surface passivation film, inhibiting pitting corrosion caused by chloride ion penetration. It has the highest contribution to corrosion resistance among all alloying elements and is assigned the highest weight of 12.6 based on electrochemical corrosion test fitting. Cr can form a stable and dense Cr2O3 passivation barrier layer on the steel surface, effectively blocking corrosive media, and its weight is set to 5.2. Si and Mn are elements prone to microsegregation, and their uneven composition can lead to the formation of micro-cells that accelerate localized corrosion. Therefore, negative weights of -2.1 and -1.2 are set to constrain their content limits, respectively. The Cu×Ni cross-negative term is used to avoid intergranular galvanic corrosion caused by Cu and Ni imbalance. -0.9 is the fitting coefficient for the elemental cross-corrosion effect, preventing a sharp decline in corrosion resistance caused by the local enrichment of Cu-rich phases. The correction term 1+0.7×%Cu is used to quantify the synergistic gain effect of Cu on corrosion resistance. An appropriate amount of Cu can be doped into the passivation film structure, further improving the passivation film's resistance to chloride ion erosion. 0.7 is the gain fitting coefficient of Cu on the stability of the passivation film. By combining gradient composition salt spray and electrochemical corrosion verification, a threshold X≥68 was set to ensure that the Cr-Ni-Cu synergistic construction of a stable passivation film is achieved, while the negative weight constraint weakens the harm of Si and Mn segregation. Even if the heat treatment causes slight differences in the microstructure, the overall corrosion potential of the steel can still remain stable, and the average corrosion rate can be controlled within 0.145 g / (m²・h).

[0047] Compared with existing technologies, this invention addresses the performance shortcomings of existing mooring chain steel in deep-sea environments. It innovatively relies on ultra-high rolling ratio controlled rolling technology to achieve ultra-fine grain strengthening, combined with VN nanoprecipitation toughening mechanism and corrosion-resistant and wear-resistant multi-component alloy system design. The steel has a grain size ≥11.0 grade, yield strength ≥1150MPa, tensile strength ≥1300MPa, yield ratio ≤0.92, and KV2 ≥130J at -20℃. It also has excellent wear and corrosion resistance, thus meeting the requirements of harsh marine mooring and coal mining environments. Attached Figure Description

[0048] Figure 1 The microstructure of the round steel at position 1 / 6D is shown in Example 1;

[0049] Figure 2 The microstructure of the round steel at position 1 / 6D is shown in Comparative Example 1. Detailed Implementation

[0050] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0051] Examples 1-3

[0052] A high-strength, high-toughness, wear-resistant, and corrosion-resistant chain steel with ultrafine grains comprises the following composition by mass percentage as shown in Tables 1-1 and 1-2. The balance not shown in Tables 1-1 and 1-2 is Fe and unavoidable impurities.

[0053] Comparative Examples 1-5

[0054] A chain steel comprises the following composition by weight percentage as shown in Tables 1-1 and 1-2, wherein the balance not shown in Tables 1-1 and 1-2 is Fe and unavoidable impurities.

[0055] Table 1-1 Chemical composition (wt%) of embodiments and comparative examples of the present invention

[0056]

[0057] Table 1-2 Chemical composition (wt%) of the embodiments and comparative examples of the present invention

[0058]

[0059] The steel used in each embodiment and comparative example was processed using controlled smelting and casting of a φ600mm large round billet, along with high rolling ratios and controlled rolling and cooling, to obtain low-segregation, high-homogeneity, ultrafine wafer steel (φ20~100mm) material. The specific process flow includes the following:

[0060] Smelting → LF furnace refining → RH vacuum degassing → continuous casting → 250 cubic meter intermediate billet rolling → hot delivery heating → round steel rolling → finishing → packaging and warehousing.

[0061] The smelting process is carried out using an electric furnace or converter (based on 100t of molten steel per furnace), and the final P content is controlled to be ≤0.006%.

[0062] The LF furnace refining process requires the white slag to be held for ≥20 minutes.

[0063] The RH vacuum degassing process involves an RH vacuum time of ≥25 min, a calcium feeding line of 25-35 meters, and a soft blowing time of 15-25 min.

[0064] The continuous casting process yields φ600 round billets. The casting employs induction heating in the tundish with narrow-range low superheat control (15-25℃), and the crystallizer level fluctuation is controlled within ±5mm. Simultaneously, low casting speed control is implemented (0.29-0.31 m / min). The electric stirring parameters are configured as follows: crystallizer stirring: 1.5Hz / 400A; casting stream stirring: 6.0Hz / 180A; end stirring: 5.0Hz / 500A. The continuously cast billets are promptly placed into the cooling pit for slow cooling, with a pit temperature ≥200℃, billet temperature upon entry ≥600℃, slow cooling time ≥72h, and exit temperature ≤200℃. Rolling is performed immediately after exiting the pit. The low-magnification quality of the cast billets is controlled according to YB / T 153 standard, meeting the requirements of central porosity, general porosity, segregation ≤1.0, and the proportion of equiaxed crystal zones in the core being 20-25%.

[0065] The 250mm square intermediate billet rolling refers to heating a φ600mm continuous casting billet, controlling the temperature of the preheating section to ≤750℃, and holding it at 1250±10℃ in the soaking section for 8-10 hours for high-temperature diffusion, and rolling it into an intermediate billet with a size of 250mm×250mm.

[0066] The hot-feeding heating process involves directly hot-feeding intermediate billets to roll round steel with a diameter of φ20-100mm. The temperature of the billets entering the furnace is controlled at ≥600℃, and the total heating time is ≥180min before being rolled out of the furnace.

[0067] The round steel rolling process employs controlled rolling and controlled cooling, controlling the initial rolling temperature at 1080±10℃, the final rolling temperature at 800-840℃, and the final rolling deformation at 25-30%. High-temperature diffusion during rolling ensures high homogeneity, and a high rolling ratio ≥40, combined with the controlled rolling process, ensures a round steel grain size ≥11.0, increasing interfacial energy to promote dispersed carbide precipitation and enhancing toughness.

[0068] To ensure sufficient hydrogen diffusion and removal at the center of the round steel, the round steel is immediately placed in a pit for slow cooling after coming off the production line. The pit temperature is ≥650℃. The cooling rate is controlled as follows: when the round steel temperature is between 500℃ and 350℃, the cooling rate is ≤15℃ / h; when the round steel temperature is between 150℃ and 350℃, the cooling rate is ≤10℃ / h; the steel is removed from the pit when the temperature is ≤150℃. Due to the hydrogen sensitivity of this steel grade, the core of the round steel is thoroughly dehydrogenated.

[0069] The main production process parameters for each embodiment and comparative example are shown in Table 2-1 and Table 2-2.

[0070] Table 2-1 Main production process parameters for steel smelting and continuous casting in each embodiment and comparative example

[0071]

[0072] Table 2-2 Main production process parameters for heating, controlled rolling and controlled cooling of steel in each embodiment and comparative example

[0073]

[0074] The heat treatment process for the round steel produced in each embodiment and comparative example includes: graded quenching and tempering.

[0075] The graded quenching process is as follows: heating at ≤80℃ / min to 860±5℃ and holding for (1.25-1.30) × d min, followed by cooling: when the round steel temperature is >450℃, the cooling rate is controlled at 50±5℃ / s; when the temperature is 200-450℃, the cooling rate is 25±5℃ / s; and when the temperature drops below 200℃, deep cryogenic treatment is performed at -120℃ for 2 hours. The tempering process involves immediately removing the steel after graded quenching and performing high-temperature tempering. The tempering process specifically involves heating at ≤80℃ / min to 580±5℃ and holding for (1.55-1.60) × d min, followed by cooling at a rate of 20-30℃ / s. Specific heat treatment parameters for each embodiment and comparative example are shown in Table 3.

[0076] Table 3 Main heat treatment parameters for each embodiment and comparative example

[0077]

[0078] Performance testing methods: After heat treatment, samples of round steel were taken at 1 / 6D of the diameter and subjected to mechanical property tests according to ISO 6892 and ISO 148 standards; the steel was evaluated according to GB / T 13298, GB / T 13320, and ASTM E112; ring-block friction tests were conducted according to GB / T 12444 to determine the wear thickness per unit working time and evaluate the steel's resistance to abrasive wear; and corrosion resistance was evaluated according to GB / T 10125. The performance results are shown in Table 4.

[0079] Table 4. List of mechanical property test results for embodiments and comparative examples of the present invention.

[0080]

[0081] Figure 1 Example 1 shows the microstructure at a position 1 / 6D in diameter of the chain link, which is 100% tempered sorbite. Figure 2 In Comparative Example 1, the chain link at a diameter of 1 / 6D contains 84% ​​tempered sorbite + 13% tempered bainite + 3% retained austenite. Unlike the comparative example, the microstructure of this example is fine and uniform, exhibiting a better microstructure ratio.

[0082] The chemical composition and production methods of the steels in Examples 1-3 were appropriately controlled, resulting in good strength, toughness, grain size, and wear and corrosion resistance. Comparative Example 1 had a reasonable composition design, but the staged quenching cooling rate was too low during heat treatment, and deep cryogenic treatment and immediate tempering were not performed, leading to insufficient tempering and an excessively high proportion of residual bainite and martensite, as well as coarse carbides, ultimately resulting in insufficient strength and toughness. Comparative Examples 2 and 3 had unsuitable chemical compositions; specifically, the Q and X values ​​of Comparative Example 2 and the A and X values ​​of Comparative Example 3 did not meet the requirements. After heat treatment, the materials failed to obtain a sufficient proportion of tempered sorbite, and the carbides were coarse, resulting in insufficient chain strength and toughness, and poor wear and corrosion resistance. Comparative Example 4 met the composition requirements, but improper production process control and heat treatment led to unsatisfactory overall performance. Comparative Example 5 had improperly controlled production process parameters, a low rolling ratio, uneven microstructure, and unqualified performance.

[0083] The above description of the embodiments is intended to enable those skilled in the art to understand and use the invention. It will be apparent to those skilled in the art that various modifications can be made to these embodiments, and the general principles described herein can be applied to other embodiments without inventive effort. Therefore, the present invention is not limited to the above embodiments, and any improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the invention should be within the protection scope of the present invention.

Claims

1. A steel for ultra-fine grained high-strength high-toughness wear and corrosion resistant chain, characterized in that, The ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain steel comprises the following components by weight percentage: C 0.20%-0.25%, Si 0.50%-0.60%, Mn 1.55%-1.75%, Cr 2.30%-2.60%, Mo 1.10%-1.25%, Ni 3.80%-4.20%, Al≤0.015%, V 0.15-0.25%, Cu 0.15-0.25%, Ti≤0.0050%, P≤0.015%, S≤0.005%, N 0.0080-0.012%, with the remainder being Fe and other unavoidable impurities.

2. The ultra-fine grained high strength-to-toughness wear and corrosion resistant steel chain according to claim 1, characterized in that, The composition of the steel used in the ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain also meets the following requirements: The precipitation coefficient Q ≥ 0.060; Q = 80 × (2.5 × %N - 0.8 × %Al - 1.3 × %Ti) / 13.

3. The ultrafine-grained high-strength and high-toughness steel for wear and corrosion resistant chains according to claim 1, characterized in that, The composition of the steel used in the ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain also meets the following requirements: Wear resistance factor A≥18; A=(2.4×%Cr+1.6×%Mo+3.7×%Si×%Mn)×(1+1.3×%V×%Cr×%Mo).

4. The ultra-fine grained high strength-to-toughness wear and corrosion resistant steel chain according to claim 1, characterized in that, The composition of the steel used in the ultrafine-grained, high-strength, tough, wear-resistant, and corrosion-resistant chain also meets the following requirements: Corrosion resistance factor X≥68; X=(12.6×%Ni+5.2×%Cr-2.1×%Si-0.9×%Cu×%Ni-1.2×%Mn)×(1+0.7%Cu).

5. A method of manufacturing a steel for a high-strength and high-toughness wear and corrosion resistant ultrafine-grained chain, characterized by, The manufacturing method includes the following process flow: Smelting → LF furnace refining → RH vacuum degassing → continuous casting → 250 cubic meter intermediate billet rolling → hot delivery heating → round steel rolling → finishing → packaging and warehousing.

6. The production method according to claim 5, wherein The continuous casting process yields φ600 round billets. The continuous casting employs tundish induction heating with narrow-range low superheat control (15-25℃), and the crystallizer liquid level fluctuation is controlled within ±5mm. Simultaneously, low casting speed control is implemented, with parameters of 0.29-0.31m / min. The electric stirring parameters are configured as follows: crystallizer electric stirring: 1.5Hz / 400A; casting stream electric stirring: 6.0Hz / 180A; end electric stirring: 5.0Hz / 500A. The continuously cast billets are promptly placed into the cooling pit for slow cooling, with a pit temperature ≥200℃, a billet temperature ≥600℃ upon entry, a slow cooling time ≥72h, and an exit temperature ≤200℃. The billets are then rolled immediately after exiting the pit.

7. The production method according to claim 5, wherein The round steel rolling process controls the initial rolling temperature at 1080±10℃, the final rolling temperature at 800-840℃, the final rolling deformation at 25-30%, and the rolling ratio at ≥40.

8. The production method according to claim 5, wherein After the round steel is rolled, it is immediately placed in a pit for slow cooling to remove hydrogen after it comes off the production line. The temperature in the pit is ≥650℃. The cooling rate is controlled in each stage of the slow cooling process as follows: when the temperature of the round steel is ≥500℃ and >350℃, the cooling rate is ≤15℃ / h; when the temperature of the round steel is <150℃ and ≤350℃, the cooling rate is ≤10℃ / h; when the temperature is ≤150℃, the steel is removed from the pit.

9. A heat treatment process of the ultra-fine grained high strength and toughness wear and corrosion resistant steel chain steel according to any one of claims 1 to 4, characterized in that, The heat treatment includes graded quenching and tempering.

10. The heat treatment process of claim 9, wherein, The graded quenching process is as follows: heating at ≤80℃ / min to 860±5℃ and holding at that temperature for (1.25-1.30)×d min, where d is the diameter of the round steel in mm; then cooling, wherein when the round steel temperature is >450℃, the cooling rate is controlled at 50±5℃ / s; when the temperature is 200-450℃, the cooling rate is 25±5℃ / s; and when the temperature drops below 200℃, deep cryogenic treatment is performed by holding at -120℃ for 2 hours.

11. The heat treatment process of claim 9, wherein, The tempering process involves immediately removing the product after graded quenching and then performing high-temperature tempering. The specific tempering process is as follows: heating to 580±5℃ at a rate of ≤80℃ / min, holding at that temperature for (1.55-1.60)×d min, and then cooling at a rate of 20-30℃ / s.

12. Heat treatment process according to any one of claims 9-11, characterized in that, After heat treatment, the microstructure of the round steel 1 / 6D is 100% tempered sorbite with carbide size ≤90nm.

13. Heat treatment process according to any one of claims 9-11, characterized in that, After heat treatment, the product steel has a grain size of ≥ 11.0, a yield strength of ≥ 1150 MPa, a tensile strength of ≥ 1300 MPa, a yield ratio of ≤ 0.92, a KV2 of ≥ 130 J at -20°C, an elongation A of ≥ 15%, a reduction of area of ≥ 56%, a wear rate of ≤ 0.023 mm per 1000 operating hours, and an average corrosion rate of ≤ 0.145 g / (m 2 ·h).

Citation Information

Patent Citations

  • High-strength high-toughness corrosion-resistant chain steel and heat treatment method thereof

    CN106521356A