A method for controlling the multi-scale heterogeneous microstructure of aluminum alloys to resist ultra-low temperature fatigue
By constructing a multi-scale heterogeneous structure of aluminum alloy through a time-sequential mechanical-thermal matching process, the problem of insufficient fatigue performance of aluminum alloy components in ultra-low temperature environments was solved, thereby improving fatigue life and service reliability.
Patent Information
- Application Number
- CN202611210333.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing aluminum alloy components have insufficient fatigue performance in ultra-low temperature environments. Traditional heat treatment processes lack multi-scale heterogeneous microstructure design, leading to dislocation pile-up and stress concentration, which easily results in fatigue cracks.
By employing a time-sequential thermo-mechanical matching process, and through the synergistic control of point-local continuous loading forming, cryogenic-assisted surface strengthening, solution treatment, and artificial aging, a multi-scale heterogeneous structure with grain and precipitate scales is constructed, which is adapted to the deformation mechanism of aluminum alloys at ultra-low temperatures.
It significantly improves the fatigue life and service reliability of aluminum alloy components in ultra-low temperature environments by inhibiting the initiation and propagation of fatigue cracks through deformation coordination and back stress strengthening at the interface of heterogeneous structures.
Smart Images

Figure CN123108443A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of metal plastic forming technology, specifically to a method for controlling the multi-scale heterogeneous structure of aluminum alloys to resist ultra-low temperature fatigue. Background Technology
[0002] With the rapid development of deep space exploration and reusable launch vehicle technologies, thin-walled aluminum alloy load-bearing components, such as rocket propellant tanks, have been operating in cryogenic environments such as liquid oxygen and liquid hydrogen for extended periods. During service, they repeatedly endure cyclic loads including pressurization-depressurization and vibration, thus facing severe fatigue damage problems. The cryogenic fatigue performance of aluminum alloy components is not only related to the static strength of the material but also closely related to microstructural characteristics such as grain size, grain boundary features, and the morphology and distribution of precipitated phases. Under cryogenic cyclic loading, the dislocation movement, pile-up, cross-slip, and recovery behaviors within the aluminum alloy material all undergo significant changes. When a local area of the material enters the cyclic plastic deformation stage, plastic strain accumulates continuously, and dislocations pile up near grain boundaries and second phase regions, leading to local stress concentration. With the continued action of cyclic loading, local stress concentration gradually evolves into fatigue crack initiation sites, further causing crack propagation and component failure. Therefore, the key to improving the fatigue performance of aluminum alloy components in ultra-low temperature environments lies in improving the material's plastic coordination ability and resistance to crack initiation and propagation during cyclic deformation through reasonable microstructure control.
[0003] Currently, the common methods for improving the fatigue performance of aluminum alloys mainly rely on traditional heat treatment processes, such as T6 and T8 tempers. The T6 process typically involves artificial peak aging directly after solution treatment to improve material strength by obtaining a higher density of strengthening precipitates. The T8 process, on the other hand, introduces a certain amount of plastic deformation after solution treatment followed by artificial aging to further promote precipitation strengthening and dislocation strengthening. These processes are relatively mature in engineering applications and can improve the strength and conventional service performance of aluminum alloys to a certain extent.
[0004] However, from the perspective of microstructure control, traditional heat treatment processes such as T6 and T8 typically aim to achieve a uniform grain structure and uniformly dispersed precipitates. Their microstructure design primarily serves to improve strength at room temperature or under normal conditions, lacking multi-scale heterogeneous microstructure design for ultra-low temperature fatigue service environments. Specifically, under traditional T6 or T8 conditions, the grain size, precipitate size and distribution, dislocation density, and deformation energy storage within the material tend to be uniform, making it prone to forming a relatively singular deformation response mode under cyclic loading. When cyclic plastic deformation continues, dislocations continuously move along the slip plane and accumulate at grain boundaries and second-phase particle locations, leading to localized stress concentrations that are difficult to release in a timely manner.
[0005] Especially in ultra-low temperature environments such as liquid oxygen and liquid hydrogen, the deformation coordination mechanisms of dislocation cross-slip, climb, and dynamic recovery within aluminum alloys are significantly suppressed, making it difficult for dislocations generated during cycling to rearrange and annihilate in a timely manner. In such cases, if the material still possesses a traditional homogeneous structure, the lack of microstructural gradients or heterogeneous interfaces between different regions to disperse strain, coordinate plastic deformation, and impede crack propagation leads to a greater concentration of cyclic plastic strain in localized areas. As the number of cycles increases, dislocation pile-up and stress concentration near grain boundaries continuously intensify, ultimately inducing fatigue crack initiation, which then propagates along grain boundaries, precipitate-rich regions, or other locally weak areas.
[0006] Therefore, there is an urgent need to develop a method for controlling the fatigue microstructure of aluminum alloys suitable for cryogenic service environments. This method actively constructs a multi-scale heterogeneous microstructure with synergistic interaction between the grain scale and the precipitate scale within the aluminum alloy component. This results in differentiated microstructures in the surface and inner layers of the component, thereby improving the coordination of cyclic plastic deformation, reducing local dislocation pile-up and stress concentration, inhibiting fatigue crack initiation and delaying crack propagation, and ultimately significantly improving the fatigue life and service reliability of aluminum alloy components in cryogenic environments. Summary of the Invention
[0007] To address the insufficient fatigue resistance of aluminum alloys under ultra-low temperature conditions, this invention provides a method for controlling the multi-scale heterogeneous microstructure of aluminum alloys to resist ultra-low temperature fatigue. This method is based on the intrinsic correlation between deformation energy storage, recovery recrystallization kinetics, and precipitation kinetics in aluminum alloys, constructing a time-sequential thermo-mechanical matching process. This process uses a multi-point local continuous loading forming method as the means of constructing a gradient deformation energy storage field. Through the synergistic control of recovery and recrystallization kinetics in the solid solution stage and precipitation kinetics in the artificial aging stage, a multi-scale heterogeneous microstructure with both grain and precipitate scales is actively constructed within the aluminum alloy. The constructed heterogeneous microstructure can highly adapt to the ultra-low temperature deformation mechanism of aluminum alloys, inducing geometrically necessary dislocation accumulation and back stress strengthening under cyclic loading, promoting cyclic strain redistribution and local plastic coordination, reducing dislocation pile-up near grain boundaries and local stress concentration, thereby effectively inhibiting fatigue crack initiation and delaying crack propagation, ultimately improving the fatigue performance and service reliability of aluminum alloys under ultra-low temperature conditions.
[0008] To achieve the above objectives, the present invention provides a method for controlling the multi-scale heterogeneous structure of aluminum alloys to resist ultra-low temperature fatigue, which includes the following steps: S1, Select the semi-cone angle as A conical mandrel with a frustum structure is coaxially fixed to the spinneret mandrel via its large end plane. An aluminum alloy slab with a solution-aging strengthening response is fixed to the small end plane of the conical mandrel via its tail end. The value range is 40-60°; S2. Start the spinning machine and use a point-local continuous loading forming method to feed along the outer conical surface contour line of the conical core mold to perform the first thinning forming of the aluminum alloy blank with a thickness of t in S1 into a conical part; The thickness of the cone wall after forming, the initial thickness of the aluminum alloy slab, and the semi-cone angle satisfy the following formula: t is the thickness after forming. The initial thickness of the billet. It is a semi-cone angle; S3. Cool the conical part formed in S2 to a cryogenic state of -196~-160℃, start the spinning machine, and apply T-times of local continuous loading to the surface of the conical part with cryogenic assistance, so that the surface material thickness within a depth of 0.5mm from the surface is reduced by 20%. The total reduction is evenly distributed through T passes, 2≤T≤6. S4. Place the tapered part after the cryogenic assisted surface spinning treatment in S3 into a heat treatment furnace, heat it to 510~540℃ at a heating rate of 5~20℃ / min, and hold it for 40~90min; after the holding period, cool it to room temperature by water quenching. S5. Quickly transfer the conical part quenched in S4 to an aging furnace that has been heated and stabilized at 160~180℃, with a transfer time not exceeding 15s; after the conical part is placed in the aging furnace, keep it at that temperature for 5~12h; after the holding time is over, remove the part from the aging furnace and air cool it to room temperature.
[0009] Preferably, the semi-cone angle The value range is 45-55°.
[0010] Preferably, the aluminum alloy slab is a 2-series aluminum alloy, such as 2219 or 2195 aluminum alloy. The principle of regulating multi-scale heterogeneous structure of the present invention is applicable to all aluminum alloys with age-hardening response, including not only 2-series aluminum alloys, but also 6-series Al-Mg-Si aluminum alloys and 7-series Al-Zn-Mg-Cu aluminum alloys (such as 7075 and 7050 aluminum alloys) widely used in aerospace.
[0011] Preferably, the point local continuous loading uses a spinning wheel, roller, or local rolling head for surface loading to satisfy the requirement that the processing process is a continuous spatiotemporal movement and the contact surface is locally loaded at points / lines, which can introduce a non-uniform thickness direction strain field and dislocation gradient.
[0012] Preferably, the process further includes a pretreatment step before forming the aluminum alloy slab, specifically: cutting and cleaning the surface of the aluminum alloy slab to obtain the aluminum alloy slab to be formed. Furthermore, before the slab is installed into the conical mandrel, lubricating oil is applied to the surface of the conical mandrel; and before spinning begins, lubricating oil is applied to the outer surface of the slab. According to a second aspect of the present invention, the present invention also provides an aluminum alloy component resistant to ultra-low temperature fatigue obtained by the method of the first aspect.
[0013] By adopting the above technical solution, the beneficial effects achieved by the present invention compared with the prior art are as follows: This invention does not simply superimpose forming, surface strengthening, solution treatment, and artificial aging, but rather uses a time-series thermo-mechanical matching process to create a continuous microstructure evolution relationship between each step. Specifically, this invention first introduces a gradient deformation energy storage field into the aluminum alloy component through point-local continuous loading forming, resulting in different deformation energy storage levels on the surface and inside of the component. Subsequently, through cryogenic-assisted point-local continuous loading strengthening of the surface, the dislocation density and deformation energy storage of the surface are further increased while suppressing dynamic recovery and dislocation annihilation, thereby forming a composite gradient deformation energy storage field. During the solution treatment process, by controlling the heating rate, solution temperature, and time, the recovery and recrystallization behaviors of different regions are differentiated. The high deformation energy storage region on the surface has a larger recrystallization driving force and easily forms a fine-grained structure; the low deformation energy storage region inside has a smaller recrystallization driving force and can form a relatively coarse-grained structure. This achieves the active construction of a grain-scale heterogeneous structure. During artificial aging, different regions exhibit varying nucleation and growth behaviors of precipitated phases due to differences in grain size, dislocation density, and defect structure. The fine-grained and high-defect-density surface regions provide more nucleation sites, resulting in small, dispersed precipitates with a high number density. Conversely, the relatively coarse-grained and low-defect-density interior regions form slightly larger and more stably distributed precipitates. This leads to the active construction of heterogeneous structures at the precipitate scale.
[0014] The multi-scale heterogeneous microstructure constructed in this invention can adapt to the deformation mechanism of aluminum alloys under ultra-low temperature environments. Under ultra-low temperature cyclic loading, the deformation incoordination at the interface of the heterogeneous microstructure can induce the accumulation of geometrically necessary dislocations and generate back stress strengthening, promote the redistribution of cyclic strain and local plastic coordination, and reduce the continuous accumulation of dislocations and local stress concentration near grain boundaries.
[0015] Therefore, by combining and coordinating the temporal and thermal matching between forming, ultra-low temperature surface strengthening, solution treatment and aging, this invention can simultaneously improve the fatigue crack initiation resistance and crack propagation resistance of aluminum alloy components, and significantly improve the fatigue life and service reliability of aluminum alloy components under ultra-low temperature cyclic loading environment. Attached Figure Description
[0016] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.
[0017] Figure 1 Microstructure of aluminum alloy components in thick sections: (a) Comparative Example 2; (b) Example 1; Figure 2 Schematic diagram of the ultra-low temperature fatigue resistance mechanism: (a) conventional homogeneous structure; (b) multi-scale heterogeneous structure; Figure 3 This is a comparison of the low-cycle fatigue life of components from Example 1 and Comparative Examples 1-5 at ultra-low temperatures.
[0018] The objectives, features, and advantages of this invention will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation
[0019] The present invention will be further described below with reference to the accompanying drawings and specific embodiments. Terms such as "upper," "lower," "left," "right," "middle," and "one" used in the preferred embodiments are merely for clarity of description and are not intended to limit the scope of the invention. Changes or adjustments to their relative relationships, without substantially altering the technical content, should also be considered within the scope of the invention.
[0020] Example 1 This embodiment provides a method for controlling the multi-scale heterogeneous structure of aluminum alloys to resist ultra-low temperature fatigue, comprising the following steps: Step S1, Blank preparation and assembly: A 3mm thick 2195-O state aluminum alloy rolled sheet was selected as the initial billet. Before processing, the aluminum alloy rolled sheet was subjected to conventional surface cleaning to remove the oxide film and other impurities on the surface of the sheet.
[0021] A conical core mold with a truncated cone structure (diameter Ф330mm, height 150mm, half cone angle 50°) is selected and coaxially fixed to the spindle of the spinning machine through its large end plane. The initial blank is fixed on the small end plane (referring to the cone top plane) of the shearing conical core mold through the tail-top mechanism, and the axes of the conical core mold, the circular sheet and the tail-top mechanism are aligned.
[0022] Before the slab is installed into the conical mandrel, apply lubricating oil to the surface of the conical mandrel; before spinning begins, apply lubricating oil to the outer surface of the slab.
[0023] Step S2, conventional point local continuous loading shaping: A circular arc spinning wheel with a corner radius of 10mm is selected, mounted on the outer spinning wheel frame, and adjusted to the starting position with a 30° installation angle. The spinning machine is started to rotate the conical mandrel, and the circular arc spinning wheel is controlled to follow the spinning trajectory set according to the outer contour of the conical mandrel, so that the spinning wheel performs high-pressure spinning forming on the aluminum alloy blank with a thinning rate of 23.4%. The spindle speed is 120 r / min, and the feed ratio is 1 mm / r. This processing is carried out at room temperature.
[0024] Step S3: Local continuous loading and forming of surface points with cryogenic assistance: The formed component obtained in step 2 is cooled by liquid nitrogen spray to maintain the surface temperature at approximately -196℃. Under this cryogenic treatment, surface spinning is performed. The spindle speed is 240 r / min, the feed ratio of the spinning wheel is 3 mm / r, and a circular arc spinning wheel with a radius of 1 mm is used. Under this cryogenic assistance, four point local continuous loadings are applied to the surface of the conical part, reducing the surface material thickness by 20% within a depth of 0.5 mm from the surface. The amount of pressing down each time is evenly distributed through four passes. The spinning wheel performs multiple continuous loadings along the outer contour of the component, resulting in local plastic deformation of the surface of the component. Step S4: Constructing a grain-scale heterogeneous structure: The component, after undergoing the ultra-low temperature surface spinning treatment in step S3, is placed in a heat treatment furnace, and the furnace door is closed. A heating program is set to raise the furnace temperature to 510°C at a rate of 10°C / min, and the temperature is held at 510°C for 40 minutes. After the holding period, the spun component is quenched in water within 5 seconds to rapidly cool it to room temperature.
[0025] Step 5: Constructing precipitate-scale heterogeneous structures: The component quenched in step S4 is quickly transferred to the aging furnace, with the transfer time not exceeding 15 seconds. Before the component enters the furnace, the temperature of the aging furnace has been raised and stabilized at 165℃. After the component is placed in the aging furnace, it is held at 165℃ for 8 hours. After the holding period, the component is removed from the aging furnace and air-cooled to room temperature to complete the processing.
[0026] Comparative Example 1 As a comparative experiment of Example 1, the only difference is that steps 2 and 3 are omitted, while the rest of the process remains the same as in Example 1.
[0027] Comparative Example 2: As a comparative experiment of Example 1, the only difference is that step 3 is omitted, while the rest of the process remains the same as in Example 1.
[0028] Comparative Example 3: As a comparative experiment of Example 1, the only difference is that the cryogenic environment in step 3 is adjusted to room temperature, while the rest of the process remains the same as in Example 1.
[0029] Comparative Example 4: (Standard T6) As a comparative experiment of Example 1, the only difference is that in step 4, before the component is placed in, the temperature of the heat treatment furnace has been raised and stabilized at 510°C, and the heat preservation time in step 5 is adjusted to 36 hours. The rest of the process is consistent with Example 1.
[0030] Comparative Example 5: (Standard T8) As a comparative experiment of Example 1, the only difference is that the solution-treated plate obtained by solution treatment of 2195-O state slab at 510℃ for 1.5h is used as the initial material, and then steps 2 and 3 are performed, the solution treatment process of step 4 is omitted, and finally step 5 is performed. The heat preservation time of step 5 is adjusted to 36h, and the rest of the process is consistent with Example 1.
[0031] Structural characterization and performance testing are detailed below: The microstructure of the aluminum alloy components obtained in Example 1 and Comparative Example 2 was characterized by thickness sections, and the results are as follows: Figure 1 As shown, there are significant differences in the microstructure morphology of the two. The microstructure of Comparative Example 2 is mainly composed of relatively coarse equiaxed or near-equiaxed polygonal grains with clear grain boundaries and relatively uniform grain distribution. In contrast, Example 1 exhibits obvious gradient heterogeneous microstructure characteristics: the grains in the surface region are significantly refined, forming a relatively fine equiaxed grain structure; along the thickness direction from the surface to the interior, a structure of alternating fine and coarse grains is formed, while the interior exhibits a relatively coarse grain structure. This microstructure characteristic indicates that the point-local continuous loading forming, cryogenic-assisted surface strengthening, and subsequent solution aging treatment used in Example 1 achieved control over the microstructure of the component. Figure 2 This study investigates the fatigue damage and deformation mechanisms of homogeneous and heterogeneous microstructures under cyclic loading in a cryogenic environment. In conventional homogeneous microstructures, dislocations generated under cyclic loading tend to accumulate near grain boundaries and precipitates, leading to local stress concentration and promoting fatigue crack initiation. For the heterogeneous microstructure formed in Example 1, the difference in plastic deformation between the fine-grained and relatively coarse-grained regions creates a strain gradient near the heterogeneous interface, inducing the accumulation of geometrically necessary dislocations and the formation of back stress. The resulting back stress and heterogeneous interface help regulate local plastic deformation and promote the redistribution of cyclic strain among different microstructure regions. Simultaneously, the fine-grained region, precipitates, and heterogeneous interface can also pin, deflect, or impede fatigue cracks, thereby reducing local stress concentration and delaying the initiation and propagation of fatigue cracks.
[0032] For Example 1 and Comparative Examples 1-5 above, after aging, samples were taken circumferentially from the components and subjected to low-cycle fatigue tests in a 77K liquid nitrogen environment, and their fatigue lives were compared. Figure 3 As shown, the low-cycle fatigue test employed stress control with a stress ratio of 0, a frequency of 0.5 Hz, and a stress amplitude of 400 MPa. The results indicate that, under the same test conditions, Example 1 exhibited the highest fatigue life, reaching approximately 1.6 × 10⁻⁶ cycles. 4 The results were significantly higher than those of comparative examples 1-5, indicating that the synergistic regulation between point local continuous loading forming, cryogenic assisted surface strengthening, and subsequent solution aging treatment is beneficial to improving the resistance of aluminum alloy components to ultra-low temperature fatigue.
[0033] In Comparative Example 1, steps 2 and 3 are omitted, and its fatigue life is lower than that of Example 1. This shows that the difference in gradient deformation field and deformation energy storage formed by point local continuous loading is the basis for subsequent construction of heterogeneous structures and improvement of ultra-low temperature fatigue performance.
[0034] Comparative Example 2 retains the point-local continuous loading forming in step two, but omits the deep cryogenic surface strengthening in step three. Its fatigue life is still significantly lower than that of Example 1, indicating that step three can further introduce plastic deformation into the surface of the component, increase the dislocation density and deformation energy storage difference between the surface and the interior, and provide a stronger driving force for the microstructure evolution to form a fine-grained surface structure and gradient transition structure during subsequent solution treatment.
[0035] Comparative Example 3 retained the continuous local loading of the surface layer in step three, but changed its treatment environment from cryogenic to room temperature. Its fatigue life was also lower than that of Example 1. This result indicates that the performance improvement in Example 1 did not solely stem from the increased number of surface mechanical loading passes; the cryogenic environment was also a key condition for achieving the strengthening effect. Under cryogenic conditions, dislocation cross-slip, dynamic recovery, and dislocation annihilation in the aluminum alloy are suppressed, allowing the surface layer to retain a higher density of dislocations and substructures during continuous local loading, thereby forming higher surface deformation energy storage and a more pronounced thickness-direction energy storage gradient. This energy storage gradient further transforms into spatial differences in grain size and precipitate distribution during subsequent solid solution and aging processes, ultimately forming a multi-scale heterogeneous structure that is beneficial for suppressing surface crack initiation and delaying crack propagation.
[0036] Comparative Examples 4 and 5 employed conventional T6 and T8 heat treatment processes, including deformation, solution treatment, and aging. However, their fatigue life under ultra-low temperature cyclic loading was still significantly lower than that of Example 1. This further demonstrates that the technical effect of the present invention does not stem from a simple superposition of forming, solution treatment, and aging processes, but rather from the temporal and thermal synergistic regulation between the gradient deformation field and the solution and aging heat treatment windows.
[0037] While specific embodiments of the present invention have been described above, those skilled in the art should understand that these are merely illustrative examples, and various changes or modifications can be made to these embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is defined only by the appended claims.
Claims
1. A method for controlling the multi-scale heterogeneous structure of aluminum alloys to resist ultra-low temperature fatigue, characterized in that: Includes the following steps: S1, Select the semi-cone angle as A conical mandrel with a frustum structure is coaxially fixed to the spinneret mandrel via its large end plane. An aluminum alloy slab with a solution-aging strengthening response is fixed to the small end plane of the conical mandrel via its tail end. The value range is 40-60°; S2. Start the spinning machine and use a point-local continuous loading forming method to feed along the outer conical surface contour line of the conical core mold to perform the first thinning forming of the aluminum alloy blank with a thickness of t in S1 into a conical part; The thickness of the cone wall after forming, the initial thickness of the aluminum alloy slab, and the semi-cone angle satisfy the following formula: t is the thickness after forming. The initial thickness of the billet. It is a semi-cone angle; S3. Cool the conical part formed in S2 to a cryogenic state of -196~-160℃, start the spinning machine, and apply T points of local continuous loading to the surface of the conical part under the assistance of cryogenic loading, so that the thickness of the surface material within 0.5mm from the surface is reduced by 20%, and the total reduction is evenly distributed through T passes, 2≤T≤6. S4. Place the tapered part after the cryogenic assisted surface spinning treatment in S3 into a heat treatment furnace, heat it to 510~540℃ at a heating rate of 5~20℃ / min, and hold it for 40~90min; after the holding period, cool it to room temperature by water quenching. S5. Quickly transfer the conical part quenched in S4 to an aging furnace that has been heated and stabilized at 160~180℃, with a transfer time not exceeding 15s; after the conical part is placed in the aging furnace, keep it at that temperature for 5~12h; after the holding time is over, remove the part from the aging furnace and air cool it to room temperature.
2. The method for controlling the multi-scale heterogeneous structure of aluminum alloys resistant to ultra-low temperature fatigue according to claim 1, characterized in that, The semi-cone angle The value range is 45-55°.
3. The method for controlling the multi-scale heterogeneous structure of aluminum alloys resistant to ultra-low temperature fatigue according to claim 1, characterized in that, Before the aluminum alloy slab is installed into the conical mandrel, lubricating oil is applied to the surface of the conical mandrel; before spinning begins, lubricating oil is applied to the outer surface of the slab.
4. The method for controlling the multi-scale heterogeneous structure of aluminum alloys resistant to ultra-low temperature fatigue according to claim 1, characterized in that, The aluminum alloy slab is a 2-series aluminum alloy.
5. The method for controlling the multi-scale heterogeneous structure of aluminum alloys resistant to ultra-low temperature fatigue according to claim 1, characterized in that, The point-based local continuous loading is performed using a rotary wheel, roller, or local rolling head for surface loading.
6. The method for controlling the multi-scale heterogeneous structure of aluminum alloys resistant to ultra-low temperature fatigue according to claim 1, characterized in that, It also includes a pretreatment step before processing and forming the aluminum alloy slab, specifically: cutting and cleaning the aluminum alloy blank to obtain the aluminum alloy slab to be formed.
7. An aluminum alloy component resistant to ultra-low temperature fatigue, characterized in that, It is processed using the control method described in any one of claims 1-6.