A powder for plasma spraying and a cladding coating

By using a multi-layer gradient plasma spraying coating, combined with NiCrAlY powder and composite powder, the problem of poor thermal shock resistance of plasma spraying coatings under high-temperature service was solved, and the coating's high toughness and heat resistance were improved.

CN123108464APending Publication Date: 2026-11-17TANGSHAN XIDE SURFACE TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611254683.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing plasma spray coatings have poor thermal shock resistance in high-temperature service scenarios, and are prone to cracking, interface debonding and peeling, which cannot meet the needs of use under extreme conditions.

Method used

The cladding coating, which adopts a multi-layer gradient structure, includes an underlayer, a transition layer, and a top layer. It is composed of NiCrAlY powder and composite powders (ZrO2-Al2O3, SiC, Si3N4) and is formed by plasma spraying and penetration sealing processes. This process alleviates the difference in thermal expansion coefficients and thermal stress, and improves the toughness and heat resistance of the coating.

Benefits of technology

It significantly improves the thermal shock resistance of the coating, delays crack initiation and propagation, and increases the service life and stability of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of powder coating technology, and proposes a powder for plasma spraying and a cladding coating. The cladding coating, from bottom to top, comprises a base layer, a transition layer, and a top layer. The base layer uses NiCrAlY powder as the raw material; the transition layer uses NiCrAlY powder and composite powder A in a mass ratio of 1:1~2; the top layer uses NiCrAlY powder and composite powder B in a mass ratio of 1:9~10. Composite powder A and composite powder B each independently comprise the following components in parts by weight: 50~60 parts ZrO2-Al2O3 composite powder, 30~40 parts SiC powder, and 5~15 parts Si3N4 powder. This invention provides a powder for plasma spraying and a cladding coating, solving the technical problem of insufficient thermal shock resistance in existing plasma spraying coatings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of powder coating technology, specifically to a plasma spraying powder and a cladding coating. Background Technology

[0002] Plasma spraying technology, with its advantages of high heating temperature, fast deposition efficiency, and wide coating adaptability, is widely used in the surface protection of high-temperature critical equipment in aerospace, energy, metallurgy, and chemical industries. It can prepare high-temperature resistant, wear-resistant, and corrosion-resistant protective coatings on metal substrates, effectively improving the service life and operational stability of components under extreme conditions. In high-temperature service scenarios, equipment components frequently undergo rapid heating and cooling thermal cycles, and the coating must continuously withstand severe thermal shock loads. Therefore, thermal shock resistance is a core indicator determining the service reliability and service life of plasma-sprayed cladding coatings.

[0003] For example, the blast furnace mud gun cap is subjected to asymmetrical strong thermal shock with unidirectional rapid heating and slow cooling, while simultaneously being eroded by a strong reducing atmosphere and alkaline slag, resulting in harsh operating conditions. Conventional plasma spraying coatings have simple formulations, numerous internal pores and interlayer gaps, and insufficient deformation tolerance. Under the combined effects of repeated thermal stress accumulation and medium erosion, the coating is prone to the initiation and propagation of cracks, leading to interface debonding, peeling, and loss of protective function, resulting in poor thermal shock resistance.

[0004] Therefore, there is an urgent need to develop a powder and cladding coating for plasma spraying to improve the thermal shock resistance of the coating. Summary of the Invention

[0005] To address the above technical problems, the present invention provides a plasma spraying powder and a cladding coating, which have high thermal shock resistance.

[0006] The specific technical solution of the present invention is as follows: According to one aspect of the present invention, a cladding coating is provided, comprising, from bottom to top, an underlayer, a transition layer and a top layer, wherein the underlayer is made of NiCrAlY powder, the transition layer is made of NiCrAlY powder and composite powder A in a mass ratio of 1:1 to 2, and the top layer is made of NiCrAlY powder and composite powder B in a mass ratio of 1:9 to 10. The composite powder A and composite powder B independently comprise the following components in parts by weight: 50-60 parts ZrO2-Al2O3 composite powder, 30-40 parts SiC powder, and 5-15 parts Si3N4 powder.

[0007] In the above technical solution, the average particle size of the ZrO2-Al2O3 composite powder is 1~5μm; the average particle size of the SiC is 1~5μm; and the average particle size of the Si3N4 powder is 5~15μm.

[0008] In the above technical solution, the average particle size of composite powder A and composite powder B is independently 40~60μm.

[0009] In the above technical solution, the preparation method of the composite powder A includes the following steps: mixing the components of the composite powder A, spray granulation, and sintering to obtain the composite powder A; The sintering temperature is 1300~1350℃, and the sintering time is 2.5~3h.

[0010] According to another aspect of the present invention, the present invention also provides a method for preparing the above-mentioned cladding coating, which includes the following steps: on a substrate, the cladding coating is sequentially formed by plasma spraying of the corresponding raw materials in the order of bottom layer, transition layer and top layer from bottom to top, to form bottom layer, transition layer and top layer, and then annealed and penetrated to seal the pores to obtain the cladding coating.

[0011] In the above technical solution, the thickness of the bottom layer is 100~150μm, the thickness of the transition layer is 100~200μm, and the thickness of the top layer is 200~300μm.

[0012] In the above technical solution, the specific process of the permeation sealing is as follows: aluminum dihydrogen phosphate is sprayed and then cured.

[0013] In the above technical solution, the parameters of plasma spraying are as follows: main gas flow rate 35~45L / min, auxiliary gas flow rate 4~7 L / min, carrier gas flow rate 3~6 L / min, spraying power 30~40kW, working current 550~600A, powder feeding rate 20~50g / min, the powder feeding carrier gas is argon, spraying distance 80~120mm, and spraying angle 90°.

[0014] In the above technical solution, the annealing is performed by heating to 850-900°C at a heating rate of 3-5°C / min, holding at that temperature for 1.5-2 hours, and then cooling.

[0015] According to another aspect of the present invention, the present invention also provides a plasma spraying powder, comprising a base layer spraying material, a transition layer spraying material, and a top layer spraying material; wherein the base layer, transition layer, and top layer materials are spraying materials corresponding to the preparation of the cladding coating.

[0016] Compared with existing technologies, this invention provides a powder for plasma spraying and its cladding coating. The cladding coating employs a gradient composite structure consisting of a base layer, a transition layer, and a top layer. The base layer, NiCrAlY, ensures good adhesion between the coating and the substrate. The transition layer gradually increases the proportion of ceramic phase, smoothing the difference in thermal expansion coefficients between the base layer and the top layer, and alleviating interlayer thermal mismatch stress. The high ceramic content of the top layer meets the requirements for high-temperature resistance and corrosion resistance, while the dispersed NiCrAlY provides toughness and absorbs thermal shock stress. ZrO2-Al2O3 in the composite powder plays a phase transformation toughening role; SiC and Si3N4 can reduce the thermal conductivity of the coating, reduce the internal temperature gradient under thermal shock, and reduce instantaneous thermal stress. By limiting the raw material composition of each layer, the synergistic effect of the multi-layer gradient structure and functional powders can be achieved, effectively delaying crack initiation and propagation, and significantly improving the coating's thermal shock resistance. Detailed Implementation

[0017] To make the objectives, technical solutions, and advantages of this invention more apparent, the invention is described in detail below. It should be understood that the invention is not limited to the description herein.

[0018] The cladding coating of the present invention comprises, from bottom to top, a base layer, a transition layer, and a top layer. The base layer uses NiCrAlY powder as the raw material. The transition layer uses NiCrAlY powder and composite powder A in a mass ratio of 1:1 to 2, for example, any value from 1:1, 1:1.2, 1:1.4, 1:1.5, 1:1.8, 1:2, or any range between any two values. The top layer uses NiCrAlY powder and composite powder B in a mass ratio of 1:9 to 10, for example, any value from 1:9, 1:9.2, 1:9.4, 1:9.5, 1:10, or any range between any two values. Composite powder A and composite powder B each independently include the following components in parts by weight: 50-60 parts ZrO2-Al2O3 composite powder, 30-40 parts SiC powder, and 5-15 parts Si3N4 powder.

[0019] In the cladding coating, the average particle size of the ZrO2-Al2O3 composite powder is 1~5μm, for example, it can be any point value among 1μm, 2μm, 3μm, 4μm, 5μm and any range between any two point values; the average particle size of the SiC powder is 1~5μm, for example, it can be any point value among 1μm, 2μm, 3μm, 4μm, 5μm and any range between any two point values; the average particle size of the Si3N4 powder is 5~15μm, for example, it can be any point value among 5μm, 8μm, 10μm, 14μm, 15μm and any range between any two point values.

[0020] In the cladding coating, the average particle size of composite powder A and composite powder B is independently 40~60μm, for example, it can be any point value among 40μm, 45μm, 50μm, 55μm, 60μm and any range between any two point values.

[0021] The preparation method of composite powder A in cladding coating includes the following steps: mixing the components of composite powder A, spray granulation, and sintering to obtain composite powder A; The sintering temperature is 1300~1350℃, for example, it can be any point value or any range between two points from 1300℃, 1310℃, 1320℃, 1330℃, 1340℃, 1350℃, and the sintering time is 2.5~3h.

[0022] The present invention also provides a method for preparing a cladding coating as described above, comprising the following steps: on a substrate, the cladding coating is sequentially formed by plasma spraying of the corresponding raw materials in the order of bottom layer, transition layer and top layer from bottom to top, to form a bottom layer, transition layer and top layer, followed by annealing and penetration sealing to obtain a cladding coating.

[0023] This invention, by limiting the thickness of the bottom layer, transition layer, and top layer in the cladding coating, can further adjust the gradient distribution of the coefficient of thermal expansion by adjusting the thickness of each coating, under the condition of limiting the raw material composition of each layer. This further alleviates the alternating stress caused by the difference in the coefficient of thermal expansion between adjacent coatings due to the hot and cold cycles, and reduces the internal stress of the coating. During the heating and cooling process of the coating, heat is transferred from the top layer to the substrate. The reasonable thickness ratio of each layer can improve the temperature gradient inside the coating, prevent the coating interface from delamination and peeling, and greatly improve the coating's resistance to thermal shock damage. In the preparation method of the cladding coating, the thickness of the bottom layer is 100~150μm, for example, it can be any point value or any range between any two point values ​​from 100μm, 110μm, 120μm, 130μm, 140μm, 150μm; the thickness of the transition layer is 100~200μm, for example, it can be any point value or any range between any two point values ​​from 100μm, 110μm, 120μm, 130μm, 140μm, 150μm, 200μm; the thickness of the top layer is 200~300μm, for example, it can be any point value or any range between any two point values ​​from 200μm, 210μm, 220μm, 230μm, 240μm, 250μm, 300μm; in a preferred embodiment, the thickness of the bottom layer is 100μm, the thickness of the transition layer is 100μm, and the thickness of the top layer is 300μm.

[0024] In the preparation method of the cladding coating, the specific process of penetration sealing is as follows: aluminum dihydrogen phosphate is sprayed and then cured.

[0025] In the preparation method of the cladding coating, the parameters of plasma spraying are as follows: main gas flow rate 35~45L / min, auxiliary gas flow rate 4~7L / min, carrier gas flow rate 3~6L / min, spraying power 30~40kW, working current 550~600A, powder feeding rate 20~50g / min, the powder feeding carrier gas is argon, spraying distance 80~120mm, and spraying angle 90°.

[0026] In the preparation method of the cladding coating, the annealing is carried out by heating to 850-900℃ at a heating rate of 3-5℃ / min, holding at that temperature for 1.5-2 hours, and then cooling.

[0027] The present invention also provides a plasma spraying powder, comprising a base layer spraying material, a transition layer spraying material, and a top layer spraying material; the base layer, transition layer, and top layer materials are spraying materials corresponding to the cladding coating.

[0028] To further illustrate the present invention, the following examples will provide a detailed description. The raw materials used in the following examples and comparative examples are all commercially available. Specifically, the ZrO2-Al2O3 composite powder is composed of ZrO2 powder and Al2O3 powder in a mass ratio of 4:1; aluminum dihydrogen phosphate: liquid, model PAL-1, with an effective substance (aluminum dihydrogen phosphate) content of 40wt%, manufactured by Guangzhou Fuer Chemical Technology Co., Ltd.; NiCrAlY powder, with an average particle size of 40μm; and a 2mm thick GH4169 substrate, which was cleaned with acetone before spraying, and then sandblasted with 40-mesh corundum abrasive to achieve a surface roughness of Ra=6.5μm.

[0029] Example 1 A method for preparing a cladding coating includes the following steps: Following the order of the cladding coating from bottom to top—comprising a base layer, a transition layer, and a top layer—plasma spraying was performed sequentially on the substrate. The parameters for plasma spraying were: main gas flow rate 35 L / min, auxiliary gas flow rate 4 L / min, carrier gas flow rate 3 L / min, spraying power 30 kW, operating current 550 A, powder feed rate 20 g / min, argon as the carrier gas, spraying distance 80 mm, and spraying angle 90°. After applying the corresponding layer material, a 100 μm thick base layer, a 150 μm thick transition layer, and a 200 μm thick top layer were formed. The temperature was increased to 850 °C at a rate of 3 °C / min, held for 2 hours, cooled, and then sprayed with aluminum dihydrogen phosphate (coating amount 2.5 g / m²). 2 After that, it is cured at 250℃ to obtain the cladding coating; The bottom layer uses NiCrAlY powder as its raw material. The transition layer is made of NiCrAlY powder and composite powder A in a mass ratio of 1:1. The surface layer is made of NiCrAlY powder and composite powder B in a mass ratio of 1:9. The preparation method of composite powder A includes the following steps: 50 parts of ZrO2-Al2O3 composite powder with an average particle size of 5μm, 30 parts of SiC powder with an average particle size of 5μm, 5 parts of Si3N4 powder with an average particle size of 5μm, water, and polyvinyl alcohol (PVA1788) are mixed to form a slurry; wherein, the amount of polyvinyl alcohol added is 3.0% of the total mass of the powder, and the solid content of the slurry is controlled at 45wt%; the slurry is thoroughly wet ball-milled and mixed, and then spray-granulated to obtain spherical agglomerated powder; subsequently, it is sintered at 1300℃ for 3h under a nitrogen protective atmosphere; the sintered product is dispersed by airflow and sieved to obtain composite powder A with an average particle size of 40μm; composite powder B is prepared using the same raw material ratio and preparation process as composite powder A.

[0030] Example 2 A method for preparing a cladding coating includes the following steps: Following the order of the cladding coating from bottom to top—comprising a base layer, a transition layer, and a top layer—plasma spraying was performed sequentially on the substrate. The parameters for plasma spraying were: main gas flow rate 45 L / min, auxiliary gas flow rate 7 L / min, carrier gas flow rate 6 L / min, spraying power 40 kW, operating current 600 A, powder feed rate 50 g / min, argon as the carrier gas, spraying distance 120 mm, and spraying angle 90°. After applying the corresponding layer material, a 150 μm thick base layer, a 150 μm thick transition layer, and a 300 μm thick top layer were formed. The temperature was increased to 900 °C at a rate of 5 °C / min, held for 1.5 h, cooled, and then sprayed with aluminum dihydrogen phosphate (coating amount 2.5 g / m²). 2 After that, it is cured at 250℃ to obtain the cladding coating; The bottom layer uses NiCrAlY powder as its raw material. The transition layer is made of NiCrAlY powder and composite powder A in a mass ratio of 1:1. The surface layer is made of NiCrAlY powder and composite powder B in a mass ratio of 1:9. The preparation method of composite powder A includes the following steps: 60 parts of ZrO2-Al2O3 composite powder with an average particle size of 5μm, 40 parts of SiC powder with an average particle size of 5μm, 15 parts of Si3N4 powder with an average particle size of 15μm, water, and polyvinyl alcohol (PVA1788) are mixed to form a slurry; wherein, the amount of polyvinyl alcohol added is 3.0% of the total mass of the powder, and the solid content of the slurry is controlled at 60wt%; the slurry is thoroughly wet ball-milled and mixed, and then spray-granulated to obtain spherical agglomerated powder; subsequently, it is sintered at 1350℃ for 2.5h under a nitrogen protective atmosphere; the sintered product is dispersed by airflow and sieved to obtain composite powder A with an average particle size of 60μm; composite powder B is prepared using the same raw material ratio and preparation process as composite powder A.

[0031] Example 3 Compared with Example 1, the only difference is that the mass ratio of NiCrAlY powder to composite powder A in the transition layer of this example is 1:1.5.

[0032] Example 4 Compared with Example 1, the only difference is that the mass ratio of NiCrAlY powder to composite powder A in the transition layer of this example is 1:2.

[0033] Example 5 Compared with Example 1, the only difference is that the mass ratio of NiCrAlY powder to composite powder B in the surface layer of this example is 1:9.5.

[0034] Example 6 Compared with Example 1, the only difference is that the mass ratio of NiCrAlY powder to composite powder B in the surface layer of this example is 1:10.

[0035] Example 7 Compared with Example 5, the only difference is that the thickness of the bottom layer is 150 μm, the thickness of the transition layer is 150 μm, and the thickness of the top layer is 200 μm.

[0036] Example 8 Compared with Example 5, the only difference is that the thickness of the bottom layer is 100 μm, the thickness of the transition layer is 100 μm, and the thickness of the top layer is 300 μm.

[0037] Example 9 Compared with Example 5, the only difference is that the thickness of the bottom layer is 100 μm, the thickness of the transition layer is 200 μm, and the thickness of the top layer is 200 μm.

[0038] Comparative Example 1 Compared with Example 1, the only difference is that the surface layer in this example does not contain NiCrAlY powder.

[0039] Comparative Example 2 Compared with Example 1, the only difference is that neither composite powder A nor composite powder B in this example contains Si3N4 powder.

[0040] Comparative Example 3 Compared with Example 1, the only difference is that neither composite powder A nor composite powder B in this example contains SiC powder.

[0041] Performance testing Thermal shock performance: The coatings of Examples 1-9 and Comparative Examples 1-3 were subjected to thermal shock performance tests. The tube furnace was heated to 1250°C, the samples were placed in the furnace, and kept at that temperature for 30 minutes. The samples were then removed and cooled in room temperature water. This was recorded as one cycle. When the area of ​​the surface coating peeling off exceeded 10% of the total area, the coating was considered to have failed. The number of thermal shocks was recorded, and the results are shown in Table 1.

[0042] Table 1. Number of thermal shocks in the cladding coatings of Examples 1-9 and Comparative Examples 1-3

[0043] Compared with Example 1, Comparative Example 1 changed the raw material composition of the surface layer, and Comparative Examples 2 and 3 changed the composition of the composite powder. The results showed that the thermal shock performance of the cladding coating in Comparative Examples 1 and 3 was lower than that in Example 1, indicating that the present invention can improve the thermal shock performance of the cladding coating by limiting the composition of the surface layer and the composite powder.

[0044] Compared with Example 1, Examples 3-6 changed the proportion of raw material components in the transition layer and the top layer. As a result, the thermal shock performance of the cladding coating in Example 5 was higher than that in Examples 3, 4 and 6, indicating that the thermal shock performance of the cladding coating can be further improved by adjusting the proportion of NiCrAlY powder and composite powder in the transition layer and the top layer.

[0045] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A cladding coating, characterized in that, From bottom to top, it includes a bottom layer, a transition layer, and a top layer. The bottom layer uses NiCrAlY powder as the raw material. The transition layer uses NiCrAlY powder and composite powder A in a mass ratio of 1:1 to 2. The top layer uses NiCrAlY powder and composite powder B in a mass ratio of 1:9 to 10. The composite powder A and composite powder B each independently comprise the following components in parts by weight: 50-60 parts ZrO2-Al2O3 composite powder, 30-40 parts SiC powder, and 5-15 parts Si3N4 powder.

2. The cladding coating according to claim 1, characterized in that, The average particle size of the ZrO2-Al2O3 composite powder is 1~5μm; the average particle size of the SiC is 1~5μm; and the average particle size of the Si3N4 powder is 5~15μm.

3. The cladding coating according to claim 1, characterized in that, The average particle size of composite powder A and composite powder B is independently 40~60μm.

4. The cladding coating according to claim 1, characterized in that, The preparation method of the composite powder A includes the following steps: mixing the components of the composite powder A, spray granulation, and sintering to obtain the composite powder A; The sintering temperature is 1300~1350℃, and the sintering time is 2.5~3h.

5. A method for preparing a cladding coating, used to prepare the cladding coating according to any one of claims 1 to 4, characterized in that, Includes the following steps: The cladding coating is formed on the substrate by plasma spraying the corresponding raw materials in the order of bottom layer, transition layer and top layer from bottom to top. After annealing and penetration sealing, the cladding coating is obtained.

6. The method for preparing a cladding coating according to claim 5, characterized in that, The thickness of the bottom layer is 100~150μm, the thickness of the transition layer is 100~200μm, and the thickness of the top layer is 200~300μm.

7. The method for preparing a cladding coating according to claim 5, characterized in that, The specific process for the permeation sealing is as follows: aluminum dihydrogen phosphate is sprayed and then cured.

8. The method for preparing a cladding coating according to claim 5, characterized in that, The parameters for plasma spraying are as follows: main gas flow rate 35~45L / min, auxiliary gas flow rate 4~7L / min, carrier gas flow rate 3~6L / min, spraying power 30~40kW, working current 550~600A, powder feeding rate 20~50g / min, the powder feeding carrier gas is argon, spraying distance 80~120mm, and spraying angle 90°.

9. The method for preparing a cladding coating according to claim 5, characterized in that, The annealing process involves heating the temperature to 850-900°C at a rate of 3-5°C / min, holding it at that temperature for 1.5-2 hours, and then cooling it.

10. A plasma spraying powder, comprising a base layer spraying material, a transition layer spraying material, and a top layer spraying material; wherein the base layer, transition layer, and top layer materials are spraying materials corresponding to the cladding coatings described in any one of claims 1 to 4.