A metal nitriding composite material and its preparation method
By forming a composite structure of a nitrided layer and alternating CrN and CrAlN layers on a metal substrate, the problems of insufficient nitriding depth and surface defects in conventional nitriding processes are solved, achieving high hardness and wear resistance metal surface modification and improving the overall performance of the metal substrate.
Patent Information
- Application Number
- CN202611409928.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Conventional metal nitriding processes suffer from limited nitriding depth, loose surface structure, and hard, brittle, white, and shiny layer defects, leading to decreased corrosion resistance and potential adhesion problems. Furthermore, thin nitrided layers cannot provide sufficient mechanical support, making the coating prone to peeling or wear through.
A composite structure consisting of a nitrided layer and alternating CrN and CrAlN layers is adopted. A nitrided layer with a thickness of 90~500μm and a metal nitride layer with a thickness of 2~10μm are formed by plasma nitriding and deposition processes. Combined with plasma etching and gradient diffusion treatment, a dense nitride layer is formed.
It significantly improves the Vickers hardness of metal substrates, enhances surface wear resistance and adhesion, solves the problems of insufficient penetration depth and surface defects, and improves the overall service performance of metal substrates.
Smart Images

Figure CN123108471A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials and relates to metal surface modification, specifically to a metal nitriding composite material and its preparation method. Background Technology
[0002] Metal components, with their excellent plasticity, toughness, machinability, and structural adaptability, are widely used in many harsh working conditions such as precision machinery, chemical equipment, marine equipment, medical devices, and automotive parts, serving as indispensable basic structural and functional components in industrial production. However, commonly used metal substrates such as conventional carbon steel, alloy steel, and ordinary alloys generally have inherent performance limitations. Their surface hardness is relatively low, and their wear resistance, scratch resistance, and fatigue resistance are poor. Under complex service environments such as high-frequency friction, heavy-load contact, acid and alkali corrosion, and humid heat and salt spray, they are prone to surface wear, scratches, pitting corrosion, and fatigue failure, significantly shortening the service life of components and restricting the stability and service cycle of high-end equipment. This fails to meet the comprehensive performance requirements of high-end industrial fields for metal components, which demand high strength, high wear resistance, long life, and high corrosion resistance. Therefore, surface modification and strengthening of metal substrates is a core technical approach to improve their overall service performance and expand their application scenarios in high-end industries.
[0003] Nitriding modification is a mainstream and efficient technology for surface hardening of metal substrates. Through the diffusion and penetration of nitrogen atoms into the metal surface, a dense nitride reinforcement layer and a modified transition layer can be formed, significantly improving the surface hardness, wear resistance, and surface stability of the metal substrate, effectively compensating for the deficiencies in the surface mechanical properties of conventional metal substrates. However, conventional nitriding processes for metal materials are generally limited by the surface oxide film and process parameters, resulting in a limited nitriding depth. Conventional processes typically produce nitrided layers with thicknesses concentrated between 20 and 60 μm. Thin nitrided layers are easily worn through under heavy loads and high-frequency wear conditions, leading to rapid substrate failure and poor durability of the strengthening effect. Furthermore, even when attempting to extend the nitriding time in conventional low-temperature nitriding (500–600°C), excessive growth of a loose, white compound layer (ε phase) and the formation of penetrating microcracks often occur, leading to decreased corrosion resistance and potential bonding problems. Additionally, stainless steel is prone to surface chromium depletion after nitriding.
[0004] To overcome the aforementioned defects of a single nitriding layer, the industry has gradually developed a composite modification technology combining nitriding and PVD coating. For example, a related patent (CN116770218A) applied for by Changzhou University discloses a three-layer composite reinforcement structure consisting of a nitriding support layer, an oxygen-infiltrating transition layer, and a nanocomposite ceramic functional layer. In this technical approach, the actual thickness of the nitriding layer is often 50-60 μm, and the nitrided surface layer exhibits loose structure and hard, brittle, and bright white defects. To address this, the solution specifically introduces an ion oxygen infiltration process to grow a dense Fe3O4 phase oxygen layer on the surface of the nitriding layer, thereby repairing surface defects and improving the adhesion of the ceramic coating. This type of technical approach, which combines "thin nitriding + surface defect repair + ultra-hard ceramic coating," has inherent limitations such as lengthy processes, altered surface chemical states, and a still limited bearing depth of the nitriding layer.
[0005] To address the issues of insufficient load-bearing depth and complex processes inherent in the aforementioned three-layer structure, another approach employed in the industry is to directly adopt a simplified two-layer model consisting of a thin nitrided layer and a hard coating. However, because conventional thin nitrided layers (20~60μm) cannot provide sufficient mechanical support, and there is a lack of adequate mechanical buffer gradient between the soft substrate and the hard coating, the coating is highly susceptible to interlayer delamination or rapid wear through the substrate under heavy loads.
[0006] In order to solve the above problems, this invention is proposed. Summary of the Invention
[0007] The first objective of this invention is to provide a metal nitriding composite material, and the second objective is to provide a method for preparing the metal nitriding composite material.
[0008] The above-mentioned objective of this invention is achieved through the following technical solution: A metal nitriding composite material includes a nitriding layer directly grown in situ on the surface of a metal substrate and a metal nitride layer deposited on the surface of the nitriding layer; wherein the thickness of the nitriding layer is 90~500μm; the metal nitride layer is formed by alternating cyclic deposition of a CrN underlayer and a CrAlN layer, including a first CrN underlayer deposited on the surface of the nitriding layer, a first CrAlN layer deposited on the surface of the first CrN underlayer, a second CrN underlayer deposited on the surface of the first CrAlN layer, and a second CrAlN layer deposited on the surface of the second CrN underlayer. The CrN and CrAlN layers are repeated twice in the nitriding matrix to finally obtain a composite structure of metal substrate-nitriding layer-CrN+CrAlN layer-CrN+CrAlN layer.
[0009] Furthermore, the surface of the metal nitriding composite material also includes a third CrN underlayer and a third CrAlN layer deposited sequentially. It further includes a third CrN underlayer deposited on the surface of the second CrAlN layer and a third CrAlN layer deposited on the surface of the third CrN underlayer.
[0010] Furthermore, the thickness of the nitrided layer is 90~270μm; the thickness of the metal nitride layer is 2~10μm, for example, it can be 5~7μm.
[0011] Furthermore, the metal substrate is selected from any one of stainless steel, carbon steel, and titanium alloy.
[0012] The preparation method of the above-mentioned metal nitriding composite material of the present invention includes the following steps. Step 1, Metal Substrate Pretreatment and Nitriding Layer: The metal substrate is placed in a plasma metallurgical furnace. After vacuuming, plasma surface cleaning is performed first, followed by plasma nitriding. During plasma nitriding, the hydrogen to nitrogen flow rate ratio is controlled at 1:2 to 1:5, the gas pressure is maintained at 140 to 165 Pa, and the duty cycle is set to 50% to 70%. Step 2, depositing a metal nitride layer on the nitrided layer surface: after nitriding, plasma etching is performed first, and then CrN base layer and CrAlN layer are sequentially deposited on the nitrided layer surface.
[0013] Furthermore, step 1 above includes the following four steps: Step a, nitriding pretreatment: High-energy argon ions bombard the surface of the workpiece, causing the water vapor and organic pollutant molecules adsorbed on the sample surface to desorb and be discharged from the furnace chamber with the vacuum unit; Step b, furnace heating and pre-diffusion treatment: The furnace temperature is controlled to rise to 500℃ at a constant rate and maintained for 80~100 min. Nitrogen atoms are initially diffused into the surface layer of the workpiece substrate through constant temperature pre-diffusion, eliminating the nitrogen concentration gradient on the workpiece surface, laying the foundation for subsequent deep diffusion, and ensuring the stability of the diffusion layer. Step c, medium-temperature gradient diffusion treatment: The furnace temperature is finely adjusted to 520℃ and maintained for 160 min to carry out gradient diffusion process treatment, which promotes the continuous diffusion of nitrogen atoms into the deep layer of the workpiece substrate, effectively increases the thickness of the nitriding diffusion layer, and improves the uniformity of the transition between the workpiece substrate and the hardened layer. Step d, constant temperature surface hardening treatment: Adjust the furnace temperature to 510℃ and maintain it for 150 min. Perform surface hardening modification at a constant temperature to enrich nitrogen atoms on the surface of the workpiece and generate a dense nitrided hard phase, forming a functional hardened layer with high hardness and high wear resistance, giving the workpiece excellent surface mechanical properties.
[0014] Furthermore, the plasma etching process described in step 2 above includes: introducing argon gas at 100 sccm, maintaining a gas pressure of 0.3 Pa, applying a bias voltage of 50 V, turning on the Ti target and setting the target current to 100 A, and using Ti ions to bombard and remove the white bright layer on the surface of the nitrided sample.
[0015] Furthermore, in step 2 above, Cr targets are used to sputter and deposit each CrN underlayer, and CrAl targets are used to sputter and deposit each CrAlN layer. In each cycle, the CrN underlayer and CrAlN layer are transferred by co-sputtering with Cr and CrAl targets.
[0016] Further, in step 2, nitrogen gas is introduced at 700 sccm, maintaining a pressure of 0.9 Pa. The Cr target is turned on and the current is set to 100 A to deposit the first CrN underlayer. Then, while maintaining the nitrogen flow rate and pressure, the CrAl target is turned on and the target current is set to 150 A to perform co-sputtering of the Cr and CrAl targets. After that, the Cr target is turned off, leaving only the CrAl target. The nitrogen flow rate is increased to 1200 sccm, the pressure is increased to 3 Pa, the bias voltage is set to 100 V, and the target current remains at 150 A to deposit the first CrAlN underlayer. The above cycle is repeated to deposit the second CrN underlayer and the second CrAlN layer.
[0017] Furthermore, the average atomic masses of Cr, Al, and N in the second CrAlN layer are 18.34, 25.48, and 50.04, respectively. The second CrAlN layer is denoted as Cr 18.34 Al 25.48 N 50.04 .
[0018] Compared with the prior art, the present invention has the following advantages: The metal nitriding composite material of the present invention comprises a nitriding layer directly grown in situ on the surface of a metal substrate and a metal nitride layer (CrN underlayer + CrAlN layer + CrN underlayer + CrAlN layer) deposited on the surface of the nitriding layer. The nitriding layer and the metal nitride layer deposited on its surface can synergistically enhance the Vickers hardness of the metal substrate. In a specific embodiment and comparative example, taking a stainless steel metal substrate as an example: compared with a stainless steel substrate, the Vickers hardness of the product obtained by adding only the nitriding layer can be increased by 110.97%; compared with a stainless steel substrate, the Vickers hardness of the product obtained by adding only the metal nitride layer can be increased by 126.45%; compared with a stainless steel substrate, the Vickers hardness of the product obtained by simultaneously adding both the nitriding layer and the metal nitride layer can be increased by 260.65%, significantly higher than the sum of 110.97% and 126.45%, indicating that the nitriding layer and the metal nitride layer deposited on its surface have a synergistic effect in enhancing the Vickers hardness of the product.
[0019] The preparation method of this invention, by controlling parameters such as the hydrogen and nitrogen flow rate ratio during plasma nitriding, can obtain a nitrided layer with excellent Vickers hardness and a smooth surface. In a specific embodiment and its comparative examples, single-factor comparisons demonstrate that parameters such as the hydrogen and nitrogen flow rate ratio during plasma nitriding can significantly improve the Vickers hardness of the nitrided metal substrate. Attached Figure Description
[0020] Figure 1 The XRD pattern of the nitrided layer composition of the sample in Example 5 shows that the main component is Fe4N.
[0021] Figure 2 The samples of Example 6 (A), Comparative Example 4 (B), and Comparative Example 5 (C) were compared by applying a 60N load to create scratches. Among them, the sample of Example 6 showed almost no exposure of the substrate, indicating that the bonding force was very good. The samples of Comparative Example 4 and Comparative Example 5 both showed obvious exposure of the substrate, indicating that the bonding force was not as good as that of Example 6. Detailed Implementation
[0022] The substantive content of the present invention will be described in detail below with reference to specific embodiments. However, those skilled in the art should know that the scope of protection of the present invention should not be limited to these specific embodiments.
[0023] Part 1: Coating Structures and Preparation Examples of Metal Nitriding Composite Materials Examples 1, 2, 3, and 4 aim to introduce the structure and preparation process of the metal nitriding composite material coating of the present invention. Within the test range, all process parameters yielded a composite coating with an ultra-thick, uniform, and dense nitriding layer plus a metal nitride layer structure of 90-500 μm. The Vickers hardness of the composite coating was significantly higher than that of the substrate. All examples used stainless steel sheets of the same batch, specifications, and performance parameters for experiments. The key instrument used was a plasma metallurgical furnace, model DH-1180, manufactured by Shenyang Keyou Vacuum Technology Co., Ltd. Example 1
[0024] Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen gas, control the hydrogen to nitrogen flow ratio to be 1:2, and maintain the gas pressure at 140 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off hydrogen and nitrogen, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; after the duty cycle and voltage are reduced to zero, immediately begin alternating deposition of CrN and CrAlN layers.
[0025] The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Co-sputtering of the target (70% Cr atoms, 30% Al atoms, the same below): Then, maintaining the nitrogen flow rate and pressure constant, while simultaneously turning on the Cr... 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0026] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0027] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN. Example 2
[0028] Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:5, and maintain the gas pressure at 165 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off hydrogen and nitrogen, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; after the duty cycle and voltage are reduced to zero, immediately begin alternating deposition of CrN and CrAlN layers.
[0029] The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0030] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0031] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN. Example 3
[0032] Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off hydrogen and nitrogen, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; after the duty cycle and voltage are reduced to zero, immediately begin alternating deposition of CrN and CrAlN layers.
[0033] The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0034] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0035] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN. Example 4
[0036] A mold steel block measuring 210mm (length) × 120mm (width) × 60mm (height) is placed inside the plasma metallurgy furnace. Stainless steel sheets (6×4×3mm) are placed on the surface of the mold steel. The nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen gas, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 100 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off hydrogen and nitrogen, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; after the duty cycle and voltage are reduced to zero, immediately begin alternating deposition of CrN and CrAlN layers.
[0037] The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0038] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0039] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN.
[0040] Measurement of appearance, thickness, and hardness of samples in Examples 1, 2, 3, and 4: 1. Appearance Examples 1, 2, 3, and 4 all yielded a smooth nitrided layer after nitriding treatment. Alternating deposition of CrN and CrAlN layers also yielded a smooth metal nitride layer, forming a composite structure of nitrided layer and metal nitride layer on the substrate – a metal nitriding composite material.
[0041] 2. Thickness Measurement After the nitrided and metal nitride layer treatment, the sample was cut to a suitable size, embedded and fixed with an insert, and then subjected to coarse grinding, fine grinding and polishing in sequence on a grinding and polishing machine to obtain a bright and scratch-free cross section. Then, the thickness of the nitrided layer and the metal nitride layer was measured under an optical microscope.
[0042] In Examples 1, 2, 3, and 4, the thicknesses of the nitrided layers were 95 μm, 102 μm, 106 μm, and 263 μm, respectively; and the thicknesses of the metal nitride layers were 6.4 μm, 6.5 μm, 6.3 μm, and 6.4 μm, respectively.
[0043] 3. Vickers hardness test The surface hardness of the samples was measured using a Vickers hardness tester with a 10 gf load cell and a holding time of 10 s. Multiple tests were performed on each group of samples, and the average value was taken. After nitriding treatment in Examples 1, 2, 3, and 4, the Vickers hardness was 710 HV0. .01 670HV 0.01 981HV 0.01 954HV 0.01 After depositing CrN and CrAlN layers, the Vickers hardness was 1211 HV. 0.01 1357HV 0.01 1677HV 0.01 1474HV 0.01 Whether it's a single nitriding treatment or further alternating deposition of CrN and CrAlN layers, the Vickers hardness (465 HV) of the substrate is higher than that of the stainless steel sheet. 0.01 () significantly improved.
[0044] 4. Measurement of friction coefficient and wear rate The surface friction coefficient and wear rate of the sample obtained in Example 3 were measured using a friction and wear testing machine under the conditions of a load of 5 N, a rotation speed of 500 r / min, and 12 h of rotational friction. The measured friction coefficient was 0.5, and the wear rate was 7.84 × 10⁻⁶. -8 mm 3 / (N∙m).
[0045] 5. Surface elemental composition determination The surface elemental composition of Example 3 was determined using scanning electron microscopy, as shown in Table 1. The composition of the sample surface at three points (second CrAlN layer) is as follows: Cr: 16.44-19.35 wt%, Al: 21.74-27.36%, N: 48.79-51.96%. The average atomic masses of Cr, Al, and N are 18.34, 25.48, and 50.04, respectively. The second CrAlN layer is represented as Cr 18.34 Al 25.48 N 50.04 The atomic ratio of Cr 18.34 Al 25.48 N 50.04 The layer has high hardness and excellent wear resistance.
[0046] Table 1
[0047] Part Two: Examples of the Influence of Nitriding Layer Preparation Method Parameters on the Appearance and Properties of Nitriding Layers Examples 5, 1, 2, and 3 aim to demonstrate the influence of certain key preparation process parameters on the appearance and properties of the nitrided layer. All examples and comparative examples used stainless steel sheets of the same batch, specifications, and performance parameters. The key instrument used was a plasma metallurgical furnace, model DH-1180, manufactured by Shenyang Keyou Vacuum Technology Co., Ltd.
[0048] Example 5 (Nitriding process is the same as in Example 3) (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, and then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min.
[0049] Comparative Example 1 (compared to Example 5, only the hydrogen and nitrogen flow rate ratio was changed) Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 3:1, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, and then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min.
[0050] Comparative Example 2 (compared to Example 5, only the time was changed) Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen gas, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 40 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min and increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min. Continue to increase the temperature to 520 ℃ and maintain it for 80 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min and decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min. Simultaneously decrease the temperature to 510 ℃ and maintain it for 75 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, and then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min.
[0051] Comparative Example 3 (compared to Example 5, only the air pressure was changed) Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen gas, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 135 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment. (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, and then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min.
[0052] Example 5: Determination of appearance, thickness, and hardness of samples from Comparative Examples 1, 2, and 3: 1. Appearance Example 5 shows that after nitriding treatment, a smooth nitrided layer is obtained, while the sample of Comparative Example 1 has a white edge around the edge, and the color of the edge and the center is inconsistent; the surface of the sample of Comparative Example 2 is rough; the sample of Comparative Example 3 also has a white edge at the edge, and there is blackening in some local areas.
[0053] XRD was measured on the sample from Example 5 (e.g.) Figure 1 Studies have found that the main component of the nitriding layer is Fe4N.
[0054] 2. Thickness measurement (measurement method as before) Example 5: The nitriding layer thickness was 106 μm. Comparative Example 1: The nitriding layer thickness was 86 μm; Comparative Example 2: The nitriding layer thickness was 67 μm; Comparative Example 3: The nitriding layer thickness was 79 μm. All of these thicknesses were lower than those of Example 5.
[0055] 3. Vickers hardness test (testing method as before) Example 5: Nitrided layer Vickers hardness 981 HV 0.01 Comparative Example 1: Nitrided layer Vickers hardness 643 HV 0.01 Comparative Example 2: Nitrided layer with a Vickers hardness of 578 HV 0.01 Comparative Example 3: Nitrided layer Vickers hardness 497 HV 0.01 The Vickers hardness of these samples is far lower than that of Example 5.
[0056] The comparison of Examples 5, 1, 2 and 3 shows that the hydrogen to nitrogen flow ratio, time and pressure parameters play an important role in the appearance, thickness and hardness of the nitrided layer.
[0057] Part Three: Examples of the Synergistic Effect of Nitriding Layers and Metal Nitride Layers Examples 6, 4, and 5 aim to demonstrate a synergistic effect between the nitrided layer and the metal nitride layer in increasing hardness. All examples and comparative examples used stainless steel sheets from the same batch, with the same specifications and performance parameters. The key instrument used was a plasma metallurgical furnace, model DH-1180, manufactured by Shenyang Keyou Vacuum Technology Co., Ltd.
[0058] Example 6 (nitrided layer + metal nitride layer, process same as Example 3) (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment.
[0059] (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; once both the duty cycle and voltage have reached zero, immediately begin alternating deposition of CrN and CrAlN layers. The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0060] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0061] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN.
[0062] Comparative Example 4 (without a metal nitride layer compared to Example 6) Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace, and the nitriding process is as follows: (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment.
[0063] (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, and then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min.
[0064] Comparative Example 5 (without the nitriding layer compared to Example 6) Stainless steel sheets (6×4×3mm) are placed in a plasma metallurgical furnace to deposit CrN and CrAlN. The process is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0065] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0066] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN. Scratch test on samples from Example 6, Comparative Example 4, and Comparative Example 5:
[0067] Figure 2 In the diagram, A, B, and C represent samples from Example 6, Comparative Example 4, and Comparative Example 5, respectively, scratched under a 60N load. Sample 6 showed almost no substrate exposure, indicating excellent adhesion. Comparative Example 4 and Comparative Example 5 both showed significant substrate exposure (red box area), indicating weaker adhesion than Sample 6.
[0068] Hardness determination of stainless steel sheet substrate, Example 6, Comparative Example 4, and Comparative Example 5 samples: The Vickers hardness of the stainless steel sheet substrate, the samples of Example 6, Comparative Example 4, and Comparative Example 5 were measured using a Vickers hardness tester (the measurement method was the same as before), and the results are shown in Table 2.
[0069] Table 2
[0070] Table 1 shows that compared with stainless steel sheet substrate, the Vickers hardness of the product obtained by adding only the nitriding layer can be increased by 110.97%; compared with stainless steel sheet substrate, the Vickers hardness of the product obtained by adding only the metal nitride layer can be increased by 126.45%; compared with stainless steel sheet substrate, the Vickers hardness of the product obtained by adding both the nitriding layer and the metal nitride layer can be increased by 260.65%, which is significantly higher than the sum of 110.97% and 126.45%, indicating that the nitriding layer and the metal nitride layer deposited on its surface have a synergistic effect in enhancing the Vickers hardness of the product.
[0071] Part 4: Examples of monolayer deposition of CrN+CrAlN and alternating deposition of CrN+CrAlN-CrN+CrAlN Example 7 (nitrided layer + metal nitride layer, process same as Example 3) (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment.
[0072] (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; once both the duty cycle and voltage have reached zero, immediately begin alternating deposition of CrN and CrAlN layers. The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30 Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0073] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0074] (5) Repeat steps (2), (3) and (4) to form a metal nitriding layer in the form of CrN+CrAlN-CrN+CrAlN.
[0075] Comparative Example 6 (compared to Example 7, only a single layer of CrN+CrAlN) (1) Turn on the mechanical pump and molecular pump, and evacuate to 5×10⁻⁶. -3 The experiment begins when the pressure is below 1. (2) Pass argon gas at 100 sccm and pressure at 0.3 Pa. Adjust the duty cycle and voltage of the pulse power supply. Gradually increase the duty cycle from 0 to 50% and the voltage from 0 to 300 V. Clean the sample surface for 60 min. The cleaning process temperature is 260℃. (3) After cleaning, first adjust the duty cycle and voltage to zero and turn off the argon gas. Then, reintroduce hydrogen and nitrogen, control the hydrogen to nitrogen flow ratio to be 1:3, and maintain the gas pressure at 150 Pa. Next, set the duty cycle to 50%, the voltage to 300V, and gradually increase the temperature. At the same time, increase the duty cycle at a gradient of 10% / 5 min and increase the voltage at a rate of 50 V / 5 min. After the temperature reaches 500 ℃, maintain it for 80 min. Then, increase the duty cycle from 50% to 70% at a rate of 10% / 5 min, increase the voltage from 300 V to 450 V at a rate of 50 V / 5 min, and continue to increase the temperature to 520 ℃ and maintain it for 160 min. Finally, decrease the duty cycle from 70% to 60% at a rate of 10% / 5 min, decrease the voltage from 450 V to 400 V at a rate of 50 V / 5 min, and simultaneously decrease the temperature to 510 ℃ and maintain it for 150 min. The sample temperature was monitored in real time using an infrared thermometer throughout the experiment.
[0076] (4) After nitriding is completed, turn off the hydrogen and nitrogen gas, then reduce the duty cycle to 0 at a gradient of 10% / 5 min, and reduce the voltage to 0 at a rate of 80 V / 5 min; once both the duty cycle and voltage have reached zero, immediately begin alternating deposition of CrN and CrAlN layers. The deposition process for CrN and CrAlN layers is as follows: (1) Etching: Introduce 100 sccm of argon gas, maintain the gas pressure at 0.3 Pa, apply a bias voltage of 50 V, turn on the Ti target and set the target current to 100 A, and maintain for 30 min; (2) Deposit CrN layer: Introduce nitrogen gas at 700 sccm, maintain gas pressure at 0.9 Pa, turn on Cr target and set current to 100 A, deposit CrN layer for 5 min, CrN layer is about 300 nm; (3) Cr and Cr 70 Al 30Target co-sputtering: Subsequently, while maintaining the nitrogen flow rate and pressure constant, Cr was turned on. 70 Al 30 Target (target current set to 150 A), Cr target and Cr 70 Al 30 The target was sputtered for a total of 10 minutes.
[0077] (4) Deposition of CrAlN layer: Turn off Cr target and retain only Cr 70 Al 30 The target was prepared, and the nitrogen flow rate was increased to 1200 sccm, the gas pressure was increased to 3 Pa, the bias voltage was set to 100 V, the target current remained at 150 A, and deposition was carried out for 120 min.
[0078] Hardness determination of samples from Example 7 and Comparative Example 6: The Vickers hardness of the samples in Example 7 and Comparative Example 6 was measured using a Vickers hardness tester (measurement method as before). The Vickers hardness of Example 7 was 1677 HV. 0.025 Comparative Example 6: Vickers hardness 1246 HV 0.025 .
[0079] The purpose of the above embodiments is to specifically illustrate the substantive content of the present invention, but those skilled in the art should know that the scope of protection of the present invention should not be limited to the specific embodiments.
Claims
1. A metal nitriding composite material, characterized in that: It includes a nitriding layer grown directly in situ on the surface of a metal substrate and a metal nitride layer deposited on the surface of the nitriding layer; wherein the thickness of the nitriding layer is 90~500μm; the metal nitride layer is formed by alternating cyclic deposition of a CrN underlayer and a CrAlN layer, including a first CrN underlayer deposited on the surface of the nitriding layer, a first CrAlN layer deposited on the surface of the first CrN underlayer, a second CrN underlayer deposited on the surface of the first CrAlN layer, and a second CrAlN layer deposited on the surface of the second CrN underlayer.
2. The metal nitriding composite material according to claim 1, characterized in that: The surface of the metal nitriding composite material also includes a third CrN underlayer and a third CrAlN layer deposited sequentially.
3. The metal nitriding composite material according to claim 1, characterized in that: The thickness of the nitrided layer is 90~270μm; the thickness of the metal nitride layer is 2~10μm.
4. The metal nitriding composite material according to claim 1, characterized in that: The metal substrate is selected from any one of stainless steel, carbon steel, and titanium alloy.
5. A method for preparing the metal nitriding composite material according to any one of claims 1 to 4, characterized in that, Includes the following steps: Step 1, Metal Substrate Pretreatment and Nitriding Layer: The metal substrate is placed in a plasma metallurgical furnace. After vacuuming, plasma surface cleaning is performed first, followed by plasma nitriding. During plasma nitriding, the hydrogen to nitrogen flow rate ratio is controlled at 1:2 to 1:5, the gas pressure is maintained at 140 to 165 Pa, and the duty cycle is set to 50% to 70%. Step 2, depositing a metal nitride layer on the nitrided layer surface: after nitriding, plasma etching is performed first, and then CrN base layer and CrAlN layer are sequentially deposited on the nitrided layer surface.
6. The preparation method according to claim 5, characterized in that, Step 1 includes the following four steps: Step a, nitriding pretreatment: High-energy argon ions bombard the surface of the workpiece, causing the water vapor and organic pollutant molecules adsorbed on the sample surface to desorb and be discharged from the furnace chamber with the vacuum unit; Step b, furnace heating and pre-diffusion treatment: The furnace temperature is controlled to rise to 500℃ at a constant rate and maintained for 80~100 min. Nitrogen atoms are initially diffused into the surface layer of the workpiece substrate through constant temperature pre-diffusion, eliminating the nitrogen concentration gradient on the workpiece surface, laying the foundation for subsequent deep diffusion, and ensuring the stability of the diffusion layer. Step c, medium-temperature gradient diffusion treatment: The furnace temperature is finely adjusted to 520℃ and maintained for 160 min to carry out gradient diffusion process treatment, which promotes the continuous diffusion of nitrogen atoms into the deep layer of the workpiece substrate, effectively increases the thickness of the nitriding diffusion layer, and improves the uniformity of the transition between the workpiece substrate and the hardened layer. Step d, constant temperature surface hardening treatment: Adjust the furnace temperature to 510℃ and maintain it for 150 min. Perform surface hardening modification at a constant temperature to enrich nitrogen atoms on the surface of the workpiece and generate a dense nitrided hard phase, forming a functional hardened layer with high hardness and high wear resistance, giving the workpiece excellent surface mechanical properties.
7. The preparation method according to claim 5, characterized in that, The plasma etching process described in step 2 includes: introducing argon gas at 100 sccm, maintaining a gas pressure of 0.3 Pa, applying a bias voltage of 50 V, turning on the Ti target and setting the target current to 100 A, and using Ti ions to bombard and remove the white bright layer on the surface of the nitrided sample.
8. The preparation method according to claim 5, characterized in that, In step 2, CrN layers are deposited by sputtering using a Cr target, and CrAlN layers are deposited by sputtering using a Cr target. The CrN layers and CrAlN layers are transitioned by co-sputtering using Cr and CrAl targets in each cycle.
9. The preparation method according to claim 8, characterized in that, In step 2: Nitrogen gas is introduced at 700 sccm, maintaining a pressure of 0.9 Pa. The Cr target is turned on and the current is set to 100 A to deposit the first CrN underlayer. Then, while maintaining the nitrogen flow rate and pressure, the CrAl target is turned on and the target current is set to 150 A to perform co-sputtering of the Cr and CrAl targets. After that, the Cr target is turned off, leaving only the CrAl target. The nitrogen flow rate is increased to 1200 sccm, the pressure is increased to 3 Pa, the bias voltage is set to 100 V, and the target current remains at 150 A to deposit the first CrAlN underlayer. The above cycle is repeated to deposit the second CrN underlayer and the second CrAlN layer.
10. The preparation method according to claim 9, characterized in that, The average atomic masses of Cr, Al, and N in the second CrAlN layer are 18.34, 25.48, and 50.04, respectively. The second CrAlN layer is represented as... .
Citation Information
Patent Citations
High-wear-resistance and corrosion-resistance composite reinforced layer on metal surface and preparation method thereof
CN116770218A