A method for processing PVD coating on the surface of a workpiece

By using a composite target material composed of molybdenum, tungsten, chromium, and silicon, combined with magnetron sputtering and heat treatment technology, the problems of insufficient film adhesion and poor wear resistance in PVD coating technology have been solved, achieving a coating effect with high wear resistance, corrosion resistance, and smoothness. It is suitable for surface strengthening and protection of cutting tools, stamping dies, aerospace parts, and 3C consumer electronics structural components.

CN123108499APending Publication Date: 2026-11-17GUANGDONG TISNAWELL NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611312931.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-27
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing PVD coating technology suffers from problems such as insufficient film adhesion, poor wear resistance, and poor smoothness on the workpiece surface. In particular, the coating is prone to peeling and wear under high temperature and long-term alternating friction load.

Method used

A composite target composed of molybdenum, tungsten, chromium, and silicon is used to form a nanocomposite ceramic structure containing molybdenum, tungsten, chromium, silicon, and carbon through continuous magnetron sputtering and heat treatment. Combined with pretreatment steps of alkaline degreasing and plasma cleaning, a PVD coating with strong adhesion, wear resistance, corrosion resistance, and smoothness is prepared.

Benefits of technology

It significantly improves the adhesion between the film and the substrate, enhances wear resistance and corrosion resistance, improves the smoothness of the coating, meets high surface quality requirements, and achieves diverse decorative effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention belongs to the field of coating technology, specifically relating to a method for processing a PVD coating on a workpiece surface. The processing method includes the following steps: S1. After alkaline degreasing and plasma cleaning of a metal substrate, a pretreated substrate is obtained; S2. The surface of the pretreated substrate is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate; S3. The coated substrate is heat-treated and naturally cooled to room temperature, thus completing the preparation process. The composite target is composed of molybdenum powder, tungsten powder, chromium powder, and silicon powder in a mass ratio of 30~45:20~35:15~20:5~10; the average particle size of the molybdenum powder, tungsten powder, and chromium powder is 6~12 μm, and the average particle size of the silicon powder is 2~5 μm. This invention uses continuous magnetron sputtering with a composite target to form a Mo-W-Cr-Si amorphous nanocomposite ceramic system, significantly improving the nanohardness, abrasion resistance, and high-temperature resistance of the film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of coating technology and relates to a method for processing PVD coating on the surface of a workpiece. Background Technology

[0002] Physical vapor deposition (PVD) is a surface treatment technology that uses physical methods to vaporize a solid target into atoms, molecules, or ionize them into ions under vacuum conditions, and then deposits a thin film with specific functions onto the workpiece surface through a gas-phase transport process. With advantages such as low deposition temperature, high film density, and environmental friendliness, it is widely used for surface strengthening and protection of cutting tools, stamping dies, aerospace components, and 3C consumer electronics structural parts. This technology effectively improves the wear resistance, corrosion resistance, and oxidation resistance of workpieces by depositing a high-density coating on the workpiece surface.

[0003] However, with the increasing demands of modern industry for workpiece surface performance, existing PVD coating technology still has shortcomings in practical applications. Large particle defects and insufficient film-substrate adhesion exist on the film surface, making it difficult to meet high surface quality requirements. Moreover, when subjected to high temperatures and long-term alternating friction loads, failure phenomena such as coating peeling and accelerated wear are prone to occur.

[0004] Currently, the mainstream PVD coating methods include cathodic arc evaporation and magnetron sputtering. For example, patent CN111850482B discloses a vacuum electroplating PVD coating process, with specific steps including: S1, wheel hub degreasing pretreatment; S2, pickling; S3, passivation; S4, base powder coating; S5, polishing; S6, cleaning and drying; S7, dielectric powder coating; S8, coating; S9, painting. While this invention effectively improves the film-substrate adhesion, it does not consider wear resistance and smoothness. Patent CN121320894B discloses a PVD coating process for galvanized sheet stamping dies. This invention involves placing treated glass and modified AF coating material into a spraying device, followed by spraying and baking. This invention solves the problems of poor coating adhesion and insufficient high-temperature resistance in existing technologies by combining high-power pulsed magnetron sputtering and unbalanced magnetron sputtering techniques; however, it does not consider the wear resistance and smoothness of the film.

[0005] Therefore, there is an urgent need for a processing method that can form a PVD coating on the surface of a workpiece that has good adhesion, high wear and corrosion resistance, and excellent smoothness. Summary of the Invention

[0006] To overcome the above-mentioned technical problems, the present invention provides a processing method for PVD coating on the surface of a workpiece, which not only has strong film adhesion, but also has high wear resistance, corrosion resistance and excellent smoothness.

[0007] To achieve the above objectives, the present invention adopts the following technical solution:

[0008] On one hand, the present invention provides a method for processing a PVD coating on the surface of a workpiece, the method comprising the following steps:

[0009] S1. After alkaline degreasing and plasma cleaning, the pretreated substrate is obtained;

[0010] S2. The pretreated substrate surface is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate.

[0011] S3. Heat-treat the coated substrate and allow it to cool naturally to room temperature to complete the preparation.

[0012] The composite target material is composed of molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio of 30~45:20~35:15~20:5~10; the average particle size of the molybdenum powder, tungsten powder and chromium powder is 6~12μm, and the average particle size of the silicon powder is 2~5μm.

[0013] Further, in step S3, the heat treatment operation is as follows: under argon protection, at 600~800℃, medium-temperature annealing for 4~6 hours, air cooling to 450~500℃, low-temperature storage for 0.5~1.5 hours, and then heating to 800~900℃ for high-temperature heat treatment for 2~3 hours.

[0014] Further, in step S2, the composite target material is prepared by mixing molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio, placing them in a ball mill, and ball milling them under an argon atmosphere. The resulting ball-milled mixture is then placed in a graphite mold for vacuum hot pressing treatment to obtain the target material.

[0015] Furthermore, the vacuum hot pressing operation is performed at a vacuum degree of 5×10⁻⁶. -3 Under argon protection, the temperature is raised to 1300~1800℃ and held for 1~3h. At the same time, the uniaxial pressure is increased to 20~45MPa at 800℃ and maintained for 1~3h.

[0016] Furthermore, in step S2, the continuous magnetron sputtering process includes the sequential deposition of an underlayer, a transition layer, a structural layer, and a color layer.

[0017] Furthermore, the base layer is a metal layer containing molybdenum, tungsten, and chromium, with a thickness of 0.1~0.3μm; the transition layer is a buffer layer containing molybdenum, tungsten, chromium, silicon, carbon, and nitrogen, with a thickness of 0.5~1.0μm; the structural layer is a nanocomposite ceramic layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 1.5~2.0μm; and the color layer is a coloring layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 0.3~0.5μm.

[0018] Furthermore, the conditions for preparing the substrate are as follows: argon flow rate of 250 sccm, negative bias voltage of 80~100V, and sputtering power of 5.5kW.

[0019] Furthermore, the preparation conditions for the transition layer are as follows: argon flow rate of 400 sccm, acetylene and nitrogen are introduced to slowly increase the flow rate to 140 sccm, negative bias voltage of 120~180V, and sputtering power of 6.0kW.

[0020] Furthermore, the preparation conditions for the structural layer are as follows: argon flow rate of 200 sccm, acetylene flow rate of 180 sccm, nitrogen flow rate of 100 sccm, negative bias voltage of 120~180V, and sputtering power of 5.0kW.

[0021] Furthermore, the preparation conditions for the color layer are as follows: stop the introduction of acetylene and nitrogen, argon flow rate is 350 sccm, negative bias voltage is 80~100V, and sputtering power is 5.0kW.

[0022] On the other hand, the present invention provides a PVD coating on the surface of a workpiece prepared by the above processing method.

[0023] The beneficial effects of this invention are:

[0024] 1. This invention addresses the problems of poor adhesion and large particles on the film surface of single-layer targets in existing technologies by innovatively designing a composite target. This composite target is composed of molybdenum (Mo), tungsten (W), chromium (Cr), and silicon (Si) in specific mass ratios. The high melting points of molybdenum and tungsten enhance the energy of sputtered particles, while chromium possesses high hardness. Together, they form a "Mo-W-Cr" structure, which strengthens the adhesion between the film and the substrate, improving the film's wear resistance and salt spray resistance. Silicon alleviates stress abrupt changes between the metal film and the substrate, forming a stable "Mo-W-Cr-Si-C" nanocomposite ceramic structure. Simultaneously, silicon inhibits abnormal growth of metal grains, preventing large-sized cells from forming protrusions on the film surface and significantly increasing the smoothness of the coated surface.

[0025] 2. This invention achieves diverse decorative effects, ranging from dark to colorful, through deposition in an atmosphere of reacting acetylene and nitrogen gases, meeting the appearance requirements of different products. Simultaneously, the pretreatment steps of alkaline degreasing and ion cleaning, along with stable vacuum and temperature control throughout the process, further ensure the density and uniformity of the coating, enabling it to possess high insulation properties while also exhibiting good corrosion resistance and long-term stability. Detailed Implementation

[0026] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with embodiments, is provided below.

[0027] Example 1

[0028] A method for processing a PVD coating on the surface of a workpiece, the method comprising the following steps:

[0029] S1. After alkaline degreasing and plasma cleaning, the pretreated substrate is obtained;

[0030] S2. The pretreated substrate surface is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate.

[0031] S3. Heat-treat the coated substrate and allow it to cool naturally to room temperature to complete the preparation.

[0032] The composite target material is composed of molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio of 30:20:15:5; the average particle size of the molybdenum powder, tungsten powder and chromium powder is 6μm, and the average particle size of the silicon powder is 2μm.

[0033] The composite target material is prepared by mixing molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio, placing them in a ball mill, and ball milling them under an argon atmosphere. The resulting ball-milled mixture is then placed in a graphite mold for vacuum hot pressing treatment to obtain the target material.

[0034] The vacuum hot pressing operation is performed at a vacuum degree of 5×10. -3 Under argon protection, the temperature is raised to 1300℃ and held for 1~3h. At the same time, the uniaxial pressure is increased to 20MPa at 800℃ and maintained for 1h.

[0035] The heat treatment operation is as follows: under argon protection, anneal at 600°C for 4 hours at a medium temperature, air cool to 450°C, hold at a low temperature for 0.5 hours, and then heat up to 800°C for 2 hours at a high temperature.

[0036] The continuous magnetron sputtering process includes the sequential deposition of an underlayer, a transition layer, a structural layer, and a color layer.

[0037] The base layer is a metal layer containing molybdenum, tungsten, and chromium, with a thickness of 0.1 μm; the transition layer is a buffer layer containing molybdenum, tungsten, chromium, silicon, carbon, and nitrogen, with a thickness of 0.5 μm; the structural layer is a nanocomposite ceramic layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 1.5 μm; and the color layer is a coloring layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 0.3 μm.

[0038] The conditions for preparing the substrate layer are as follows: argon flow rate of 250 sccm, negative bias voltage of 80 V, and sputtering power of 5.5 kW.

[0039] The preparation conditions for the transition layer are as follows: argon flow rate of 400 sccm, acetylene and nitrogen are introduced and the flow rate is slowly increased to 140 sccm, negative bias voltage is 120V, and sputtering power is 6.0kW.

[0040] The structural layer was prepared under the following conditions: argon flow rate of 200 sccm, acetylene flow rate of 180 sccm, nitrogen flow rate of 100 sccm, negative bias voltage of 120 V, and sputtering power of 5.0 kW.

[0041] The conditions for preparing the color layer are as follows: stop the introduction of acetylene and nitrogen, argon flow rate is 350 sccm, negative bias voltage is 80~100V, and sputtering power is 5.0kW.

[0042] Example 2

[0043] A method for processing a PVD coating on the surface of a workpiece, the method comprising the following steps:

[0044] S1. After alkaline degreasing and plasma cleaning, the pretreated substrate is obtained;

[0045] S2. The pretreated substrate surface is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate.

[0046] S3. Heat-treat the coated substrate and allow it to cool naturally to room temperature to complete the preparation.

[0047] The composite target material is composed of molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio of 40:30:17:8; the average particle size of the molybdenum powder, tungsten powder and chromium powder is 8 μm, and the average particle size of the silicon powder is 3 μm.

[0048] The composite target material is prepared by mixing molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio, placing them in a ball mill, and ball milling them under an argon atmosphere. The resulting ball-milled mixture is then placed in a graphite mold for vacuum hot pressing treatment to obtain the target material.

[0049] The vacuum hot pressing operation is performed at a vacuum degree of 5×10. -3 Under argon protection, the temperature was raised to 1800℃ and held for 3 hours. At the same time, the uniaxial pressure was increased to 45MPa at 800℃ and maintained for 3 hours.

[0050] The heat treatment operation is as follows: under argon protection, anneal at 800°C for 6 hours at a medium temperature, air cool to 500°C, hold at a low temperature for 1.5 hours, and then heat up to 900°C for 3 hours at a high temperature.

[0051] The continuous magnetron sputtering process includes the sequential deposition of an underlayer, a transition layer, a structural layer, and a color layer.

[0052] The base layer is a metal layer containing molybdenum, tungsten, and chromium, with a thickness of 0.3 μm; the transition layer is a buffer layer containing molybdenum, tungsten, chromium, silicon, carbon, and nitrogen, with a thickness of 1.0 μm; the structural layer is a nanocomposite ceramic layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 2.0 μm; and the color layer is a coloring layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 0.5 μm.

[0053] The conditions for preparing the substrate layer are as follows: argon flow rate of 250 sccm, negative bias voltage of 100 V, and sputtering power of 5.5 kW.

[0054] The preparation conditions for the transition layer are as follows: argon flow rate of 400 sccm, acetylene and nitrogen are introduced and the flow rate is slowly increased to 140 sccm, negative bias voltage is 180 V, and sputtering power is 6.0 kW.

[0055] The structural layer was prepared under the following conditions: argon flow rate of 200 sccm, acetylene flow rate of 180 sccm, nitrogen flow rate of 100 sccm, negative bias voltage of 180 V, and sputtering power of 5.0 kW.

[0056] The conditions for preparing the color layer are as follows: stop the introduction of acetylene and nitrogen, argon flow rate is 350 sccm, negative bias voltage is 100V, and sputtering power is 5.0kW.

[0057] Example 3

[0058] A method for processing a PVD coating on the surface of a workpiece, the method comprising the following steps:

[0059] S1. After alkaline degreasing and plasma cleaning, the pretreated substrate is obtained;

[0060] S2. The pretreated substrate surface is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate.

[0061] S3. Heat-treat the coated substrate and allow it to cool naturally to room temperature to complete the preparation.

[0062] The composite target material is composed of molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio of 45:35:20:10; the average particle size of the molybdenum powder, tungsten powder and chromium powder is 12 μm, and the average particle size of the silicon powder is 5 μm.

[0063] The composite target material is prepared by mixing molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio, placing them in a ball mill, and ball milling them under an argon atmosphere. The resulting ball-milled mixture is then placed in a graphite mold for vacuum hot pressing treatment to obtain the target material.

[0064] The vacuum hot pressing operation is performed at a vacuum degree of 5×10. -3 Under argon protection, the temperature was raised to 300℃ and held for 2 hours. At the same time, the uniaxial pressure was increased to 35MPa at 800℃ and maintained for 2.5 hours.

[0065] The heat treatment operation is as follows: under argon protection, anneal at 700°C for 5 hours at a medium temperature, air cool to 480°C, keep at a low temperature for 1 hour, and then heat up to 85°C for 2.5 hours at a high temperature.

[0066] The continuous magnetron sputtering process includes the sequential deposition of an underlayer, a transition layer, a structural layer, and a color layer.

[0067] The base layer is a metal layer containing molybdenum, tungsten, and chromium, with a thickness of 0.2 μm; the transition layer is a buffer layer containing molybdenum, tungsten, chromium, silicon, carbon, and nitrogen, with a thickness of 0.7 μm; the structural layer is a nanocomposite ceramic layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 1.8 μm; and the color layer is a coloring layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 0.4 μm.

[0068] The conditions for preparing the substrate layer are as follows: argon flow rate of 250 sccm, negative bias voltage of 90 V, and sputtering power of 5.5 kW.

[0069] The preparation conditions for the transition layer are as follows: argon flow rate of 400 sccm, acetylene and nitrogen are introduced and the flow rate is slowly increased to 140 sccm, negative bias voltage is 140 V, and sputtering power is 6.0 kW.

[0070] The structural layer was prepared under the following conditions: argon flow rate of 200 sccm, acetylene flow rate of 180 sccm, nitrogen flow rate of 100 sccm, negative bias voltage of 140 V, and sputtering power of 5.0 kW.

[0071] The conditions for preparing the color layer are as follows: stop the introduction of acetylene and nitrogen, argon flow rate is 350 sccm, negative bias voltage is 90V, and sputtering power is 5.0kW.

[0072] Comparative Example 1

[0073] Compared with Example 1, Comparative Example 1 differs in that the composite target material is composed of tungsten, chromium, and silicon, while the other components, preparation steps, and parameters are the same.

[0074] Comparative Example 2

[0075] Compared with Example 1, Comparative Example 2 differs in that the composite target material is composed of molybdenum, chromium, and silicon, while the other components, preparation steps, and parameters are the same.

[0076] Comparative Example 3

[0077] Compared with Example 1, Comparative Example 3 differs in that the composite target is composed of molybdenum, tungsten, and silicon, while the other components, preparation steps, and parameters are the same.

[0078] Comparative Example 4

[0079] Compared with Example 1, Comparative Example 3 differs in that the composite target is composed of molybdenum, tungsten, and chromium, while the other components, preparation steps, and parameters are the same.

[0080] The following performance tests were performed on the products obtained from Examples 1-3 and Comparative Examples 1-3:

[0081] The thickness of the PVD film was determined using a scanning electron microscope (SEM) cross-sectional method. Specifically, the film thickness was measured by directly observing the sample cross-section using an SEM.

[0082] Referring to GB / T 1031, the surface roughness of PVD films was measured using the optical sectioning method. The surface roughness of the samples was obtained by direct inspection using a 9J / JBQ dual-tube optical sectioning microscope.

[0083] Referring to GB / T 30707-2014, the Rockwell indentation method is used to test the adhesion of the PVD film. Specifically, the load is increased by gradually increasing the load with a Rockwell C diamond indenter, and the cracking and peeling of the film around the indentation are observed. The adhesion is judged according to the HF grade (HF1~2: excellent; HF3: qualified; HF4~6: unqualified).

[0084] Referring to GB / T 22458-2008: The hardness of PVD films is tested using the nanoindentation method. Specifically, a diamond Berkovich indenter is used to set 5 test points on the sample, with the depth controlled within 1 / 10 of the sample thickness. A small load is applied, and the load-displacement curve is collected. After verification, the nanohardness is recorded.

[0085] Referring to GB / T 43853-2024, the ball-disc friction test method was used to test the abrasion resistance of the PVD film. Specifically, a tribological testing machine was used, with Al2O3 / GCr15 as the dual balls, and the load force was set to 8N, the rotation speed to 300r / min, and the friction radius to 4mm. Continuous friction was performed; the coefficient of friction was recorded, and the specific wear rate was calculated.

[0086] The corrosion resistance of PVD films was tested using the neutral salt spray test method according to GB / T 12444-2022. A neutral salt spray chamber was used with a 5% NaCl solution, and continuous spraying was performed at 37°C. The samples were sealed at the edges, and rust spots on the sample surface were observed periodically, with the time of rust appearance recorded. The test results are shown in Table 1.

[0087] Table 1

[0088]

[0089] According to the test results in Table 1, compared with Comparative Examples 1-4, the overall performance of the PVD film prepared by the present invention is significantly better than that of Comparative Examples 1-4 in Examples 1-3.

[0090] Comparative analysis shows that Examples 1-3 were prepared using composite targets composed of molybdenum, tungsten, chromium, and silicon in specific mass ratios. Molybdenum and tungsten, with their high melting points, enhance the energy of sputtered particles, significantly strengthening the adhesion between the film and the substrate. Chromium, with its high hardness, imparts wear resistance and salt spray resistance to the film. Silicon alleviates stress abrupt changes between the metal film and the substrate, inhibits abnormal grain growth, and prevents large-sized cells from forming protrusions on the film surface. Together with silicon, it forms a stable "Mo-W-Cr-Si-C" nanocomposite ceramic structure, significantly increasing the smoothness of the coated surface and further enhancing wear and corrosion resistance. In Comparative Examples 1-4, the absence of molybdenum, tungsten, chromium, and silicon, respectively, resulted in varying degrees of reduction in hardness, wear and corrosion resistance, adhesion, and smoothness.

[0091] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any indirect modifications, equivalent changes, and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.

Claims

1. A method for processing a PVD coating on the surface of a workpiece, characterized in that, The processing method includes the following steps: S1. After alkaline degreasing and plasma cleaning of the substrate, a pretreated substrate is obtained; the substrate includes stainless steel, cemented carbide, and glass; S2. The pretreated substrate surface is subjected to continuous magnetron sputtering using a composite target to obtain a coated substrate. S3. Heat-treat the coated substrate and allow it to cool naturally to room temperature to complete the preparation. The composite target material is composed of molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio of 30~45:20~35:15~20:5~10; the average particle size of the molybdenum powder, tungsten powder and chromium powder is 6~12μm, and the average particle size of the silicon powder is 2~5μm.

2. The method for processing a PVD coating on a workpiece surface according to claim 1, characterized in that, In step S3, the heat treatment operation is as follows: under argon protection, at 600~800℃, anneal at a medium temperature for 4~6 hours, air cool to 450~500℃, keep at a low temperature for 0.5~1.5 hours, and then heat up to 800~900℃ for high temperature heat treatment for 2~3 hours.

3. The method for processing a PVD coating on a workpiece surface according to claim 1, characterized in that, In step S2, the composite target material is prepared by mixing molybdenum powder, tungsten powder, chromium powder and silicon powder in a mass ratio, placing them in a ball mill, and ball milling them under an argon atmosphere. The resulting ball-milled mixture is then placed in a graphite mold for vacuum hot pressing treatment to obtain the target material.

4. The method for processing a PVD coating on a workpiece surface according to claim 3, characterized in that, The vacuum hot pressing operation is performed at a vacuum degree of 5×10. -3 Under argon protection, the temperature is raised to 1300~1800℃ and held for 1~3h. At the same time, the uniaxial pressure is increased to 20~45MPa at 800℃ and maintained for 1~3h.

5. The method for processing a PVD coating on a workpiece surface according to claim 1, characterized in that, In step S2, the continuous magnetron sputtering process includes the sequential deposition of an underlayer, a transition layer, a structural layer, and a color layer.

6. The method for processing a PVD coating on a workpiece surface according to claim 5, characterized in that, The base layer is a metal layer containing molybdenum, tungsten, and chromium, with a thickness of 0.1~0.3μm; the transition layer is a buffer layer containing molybdenum, tungsten, chromium, silicon, carbon, and nitrogen, with a thickness of 0.5~1.0μm; the structural layer is a nanocomposite ceramic layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 1.5~2.0μm; and the color layer is a coloring layer containing molybdenum, tungsten, chromium, silicon, and carbon, with a thickness of 0.3~0.5μm.

7. A PVD coating on the surface of a workpiece prepared by the processing method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • A vacuum electroplating PVD coating process

    CN111850482B

  • A PVD coating process method applied to a galvanized sheet stamping die

    CN121320894B