A method for preparing an anti-fingerprint coating for anodized alloy laptop casing

By preparing a gradient composite film system of chromium base layer-alumina intermediate layer-silica transition layer on anodized alloy laptop shell, the problems of interface compatibility, adhesion, wear resistance and color difference of the anti-fingerprint coating of anodized alloy laptop shell are solved, thereby improving the appearance and service life of high-end products.

CN123108503APending Publication Date: 2026-11-17SUZHOU DONGXING SURFACE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611465122.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing anti-fingerprint coatings on anodized alloy laptop shells suffer from poor interface compatibility, weak adhesion, poor wear resistance, color difference, and uneven gloss, failing to meet the appearance, texture, and lifespan requirements of high-end products.

Method used

A gradient composite inorganic film system consisting of a chromium underlayer, an alumina intermediate layer, and a silicon dioxide transition layer was formed using a vacuum uniform sputtering deposition process with film thickness controlled at 10nm-20nm. Combined with physical vapor deposition technology, an anti-fingerprint coating was prepared.

Benefits of technology

It achieves a fingerprint-resistant coating with high wear resistance, ultra-low color difference, ultra-low dyne value, and excellent adhesion. It has an excellent appearance and texture, good self-cleaning performance, strong stability in complex environments, and is suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108503A_ABST
    Figure CN123108503A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing an anti-fingerprint coating on an anodized alloy laptop shell, belonging to the field of alloy surface coating technology. Using a hard anodized alloy laptop shell as a substrate, after wiping and blowing pretreatment, a gradient inorganic film system is sequentially deposited by vacuum magnetron sputtering: a chromium underlayer, an alumina intermediate layer, and a silica transition layer. Then, an anti-fingerprint coating is deposited by physical vapor deposition. The chromium underlayer fills the micropores of the substrate to improve adhesion, the alumina intermediate layer buffers film stress, and the silica transition layer connects the organic functional coating. The resulting product has a color difference value ΔE ≤ 1.0, can withstand 2500 steel wool wiping cycles, has a cross-cut adhesion rating of 0, exhibits excellent resistance to temperature and humidity aging, retains a metallic matte texture, and the process is green and controllable, suitable for mass production of laptop shells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of alloy surface coating technology, specifically relating to a method for preparing an anti-fingerprint coating on an anodized alloy laptop shell. Background Technology

[0002] The mainstream base materials for laptop casings are aluminum alloy and magnesium-aluminum alloy. These alloys are lightweight, have high structural strength, and excellent heat dissipation. After electrochemical anodizing, a dense and uniform porous oxide film can be generated on the surface of the base material, which can not only effectively improve the corrosion resistance, oxidation resistance, and weather resistance of the base material, but also give the casing a delicate and high-end metallic matte texture. It is the preferred material for the casing of thin and light consumer electronics devices at present.

[0003] However, the surface of anodized alloy shells has a large number of micro-nano porous structures and high surface free energy. During daily handling and use, it is extremely easy for fingerprints, sebum, sweat, oil, and environmental dust to accumulate. Regular wiping is insufficient to completely remove these residues, which can remain on the surface for a long time, causing the shell to yellow, darken, and become mottled and dull, severely affecting the product's appearance and lifespan. To solve this problem, the industry commonly uses surface treatment methods such as spraying or vapor-depositing anti-fingerprint coatings onto the anodized alloy surface.

[0004] Existing anti-fingerprint coating preparation processes suffer from several core technical defects: First, traditional processes often involve directly depositing a single layer of organic anti-fingerprint coating onto the surface of anodized substrates. The organic coating exhibits poor interfacial compatibility and weak adhesion with the inorganic oxide substrate, resulting in extremely poor abrasion resistance. Prolonged use or frequent wiping easily leads to coating wear, whitening, peeling, and flaking, causing rapid failure of the anti-fingerprint function. Second, a single organic coating cannot fill the microscopic pores of the anodized substrate, resulting in poor coating uniformity. Inconsistent coating thickness at the edges, corners, flat surfaces, and curved areas of the finished casing easily leads to localized color differences and uneven gloss, making it difficult to guarantee product appearance consistency and failing to meet the quality inspection standards for high-end laptops. Third, conventional commercially available anti-fingerprint coating formulations have single components and poor compatibility, resulting in insufficient surface wetting after curing. Dyne values ​​are generally above 30, limiting hydrophobic, oleophobic, anti-fingerprint, and self-cleaning effects. Fourth, the lack of a transitional film buffer results in low stress matching between the coating and the substrate, making the coating prone to cracking and peeling under temperature variations.

[0005] Currently, the industry lacks a process for preparing an anti-fingerprint coating for anodized alloy shells that can simultaneously achieve high wear resistance, ultra-low color difference, ultra-low dyne value, high adhesion, and high stability. Conventional single-layer coating processes cannot overcome performance bottlenecks. Therefore, there is an urgent need to develop a composite coating preparation method with reasonable structure, controllable parameters, excellent performance, and suitability for mass production to solve the core problems of existing technologies. Summary of the Invention

[0006] The technical problem solved by this invention is to provide a method for preparing an anti-fingerprint coating on an anodized alloy laptop shell. This method uses a 10nm-20nm film thickness control + vacuum uniform sputtering deposition process. After coating, the shell has a uniform gloss and color. The color difference value ΔE is less than 1.0 as measured by a colorimeter. There are no obvious color differences, uneven colors, or uneven gloss to the human eye. This method preserves the original delicate and high-end metallic matte texture of the anodized alloy to the greatest extent. The appearance quality far exceeds that of products made with traditional processes.

[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing an anti-fingerprint coating on an anodized alloy laptop casing includes the following steps:

[0009] 1) Select an alloy notebook shell that has undergone hard anodizing treatment as the substrate, and pre-treat the surface of the substrate by wiping and blowing with ethanol;

[0010] 2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, the anti-fingerprint coating particles are placed in the molybdenum boat, and after plasma cleaning under low vacuum, the base vacuum is evacuated and argon gas is introduced. The chromium underlayer is deposited by radio frequency magnetron sputtering.

[0011] 3) Keep the working pressure of the cavity constant, introduce a mixed process gas of argon and oxygen, switch to aluminum target, and deposit an alumina intermediate layer by radio frequency magnetron sputtering;

[0012] 4) Keep the process gas and working pressure in the cavity constant, switch the silicon target, and deposit the silicon dioxide transition layer by radio frequency magnetron sputtering to obtain a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer;

[0013] 5) Re-evacuate the vacuum, heat the molybdenum boat to evaporate the anti-fingerprint coating film, and deposit it on the substrate using physical vapor deposition. After depressurization, the finished anodized alloy notebook shell is obtained.

[0014] Furthermore, the thickness of each of the chromium underlayer, the alumina intermediate layer, and the silicon dioxide transition layer is 10nm-20nm.

[0015] Furthermore, the thickness of the chromium underlayer is 15 nm, the thickness of the alumina intermediate layer is 15 nm, and the thickness of the silicon dioxide transition layer is 10 nm.

[0016] Furthermore, in step 2), the cavity's base vacuum is 8 × 10⁻⁶. -3 Pa ~ 1.2 × 10 -2 Pa; High-purity argon gas is introduced at a flow rate of 300~500 sccm, and the working pressure is 8×10. -3 Pa ~ 1.2 × 10 -2Pa.

[0017] Further, in step 2), the sputtering power is 6~7kW. Further, in step 3), the argon flow rate is 300~500sccm, the oxygen flow rate is 100~200sccm, and the sputtering power is 3~4kW. Further, in step 4), the sputtering power is 4~5kW.

[0018] Furthermore, in step 5), the vacuum degree is 5 × 10⁻⁶. -3 Pa, heating molybdenum boat to evaporate anti-fingerprint coating film, coating heating time is 300s; after stopping heating, maintain 5×10 -3 The pressure was reduced by 200 Pa for 200 seconds before being released.

[0019] Furthermore, in step 5), the thickness of the anti-fingerprint coating film is 8nm-12nm.

[0020] Furthermore, the anodized alloy notebook shell has a surface dyne value of 20~22, an appearance color difference value ΔE≤1.0, and a bonding strength of 0 in the cross-cut adhesion test.

[0021] Compared with the prior art, the present invention has the following advantages:

[0022] (1) Significantly improved abrasion resistance and extended product lifespan: The three-layer inorganic composite film system is densely bonded, with extremely strong interlayer adhesion. The overall film layer has high hardness and excellent scratch resistance, which can form a strong support and protection for the surface anti-fingerprint coating. According to standard abrasion resistance test verification, the finished shell can withstand more than 1,000 steel wool abrasion wipings without problems such as coating peeling, whitening, scratches, or loss of gloss. The anti-fingerprint function is maintained for a long time, completely solving the industry problems of easy wear and failure and short service life of traditional coatings.

[0023] (2) Minimal color difference in appearance, perfectly preserving the original texture of metal: Through 10nm-20nm film thickness control + vacuum uniform sputtering deposition process, the overall gloss of the shell after coating is uniform and the color is consistent. The color difference value ΔE < 1.0 is detected by colorimeter. There are no obvious color difference, yin-yang color, or uneven gloss problems in the human eye. It preserves the original delicate and high-end metallic matte texture of anodized alloy to the greatest extent. The appearance quality far exceeds that of traditional process products.

[0024] (3) Ultra-low dyne value, ultimate anti-fingerprint and anti-fouling self-cleaning performance: The optimized fluorine-modified organosilicon coating formula, combined with a highly adaptable composite film structure, greatly reduces the surface free energy of the shell. The surface dyne value of the finished product is stably controlled at 20±2, which has excellent hydrophobic and oleophobic properties. Human fingerprints, sebum, oil stains and water stains cannot adhere to it. A light wipe can restore the clean surface. It has excellent self-cleaning effect and will not get dirty or yellow after long-term use.

[0025] (4) Strong interlayer bonding and excellent stability in high and low temperature environments: The gradient film system effectively balances the interfacial stress, and the coating is tightly bonded to the substrate and between film layers, with no risk of delamination or edge lifting. After high and low temperature cycling and damp heat aging tests, the coating performance has not degraded and the appearance is normal, making it suitable for complex use environments and significantly improving product stability and yield.

[0026] (5) Wide process adaptability, green and environmentally friendly, suitable for mass production: This process can be adapted to both aluminum alloy and magnesium-aluminum alloy, two mainstream anodized notebook shell substrates. The process parameters are standardized and highly controllable. The vacuum sputtering process has no wastewater, waste gas, or waste liquid pollution, and is a green and environmentally friendly process. The production yield is high, the batch consistency is good, the production cost is controllable, and it is fully adapted to the needs of large-scale industrial mass production. Attached Figure Description

[0027] Figure 1 This is a schematic diagram of the layer structure of the composite coating on the anodized alloy notebook shell prepared in this application. Detailed Implementation

[0028] The present invention will be further illustrated below with reference to specific embodiments. These embodiments are implemented based on the technical solutions of the present invention, and it should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention.

[0029] The anhydrous ethanol (99.9%, analytical grade), high-purity chromium target, high-purity aluminum target, and high-purity silicon target used in the following examples were all commercially available; the anti-fingerprint coating stock solution (X-71-197) was purchased from Shin-Etsu Chemical Industry Co., Ltd.

[0030] like Figure 1 As shown, the composite coating structure provided in this application is a multi-layer gradient stacked structure, consisting of an anodized alloy substrate layer, a chromium underlayer, an alumina intermediate layer, a silica transition layer, and an anti-fingerprint functional coating, from bottom to top. The single-layer thickness of the chromium underlayer, alumina intermediate layer, and silica transition layer is controlled between 10nm and 20nm, while the thickness of the surface anti-fingerprint coating is controlled between 8nm and 12nm. The interfaces between each film layer are dense, pore-free, and free of delamination defects. Through the gradient transition of the inorganic multilayer film system, the technical problems of poor compatibility, weak adhesion, and easy detachment between organic coatings and inorganic anodized substrates are effectively solved.

[0031] Example 1

[0032] A method for preparing an anti-fingerprint coating on an anodized alloy laptop casing includes the following steps:

[0033] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0034] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3 Pa; High-purity argon gas is introduced at a flow rate of 400 sccm, and the stable working pressure is 1.2 × 10⁻⁶. -2 Pa; RF magnetron sputtering process was adopted with a sputtering power of 6.5kW. The sputtering film thickness was accurately monitored by a crystal oscillator film thickness monitoring method, and a 10nm pure chromium underlayer was deposited.

[0035] (3) The working pressure remains unchanged, the argon flow rate is 400 sccm and the oxygen flow rate is 200 sccm. The target material is switched to a high-purity aluminum target. Radio frequency magnetron sputtering is used with a sputtering power of 3.5 kW. The sputtering film thickness is accurately monitored by using a crystal oscillator film thickness monitoring method to deposit a 15 nm aluminum oxide intermediate layer.

[0036] (4) The process gas and pressure in the cavity are kept constant. The high-purity silicon target is replaced. The RF magnetron sputtering power is set to 4.5kW. The sputtering film thickness is accurately monitored by the crystal oscillator film thickness monitoring method. A silicon dioxide transition layer with a thickness of 10nm is deposited to form a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer.

[0037] (5) Evacuate to a vacuum level of 5×10⁻⁶ at the bottom of the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0038] Example 2

[0039] A method for preparing an anti-fingerprint coating on an anodized alloy laptop casing includes the following steps:

[0040] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0041] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶.-3 Pa; High-purity argon gas is introduced at a flow rate of 400 sccm, and the stable working pressure is 1.2 × 10⁻⁶. -2 Pa; RF magnetron sputtering process was adopted with a sputtering power of 7kW. The sputtering film thickness was precisely monitored by a crystal oscillator film thickness monitoring method, and a 15nm pure chromium underlayer was deposited.

[0042] (3) The working pressure remains unchanged, the argon flow rate is 400 sccm and the oxygen flow rate is 200 sccm. The target material is switched to a high-purity aluminum target. Radio frequency magnetron sputtering is used with a sputtering power of 3.5 kW. The sputtering film thickness is accurately monitored by using a crystal oscillator film thickness monitoring method to deposit a 15 nm aluminum oxide intermediate layer.

[0043] (4) The process gas and pressure in the cavity are kept constant. The high-purity silicon target is replaced. The RF magnetron sputtering power is set to 4.5kW. The sputtering film thickness is accurately monitored by the crystal oscillator film thickness monitoring method. A silicon dioxide transition layer with a thickness of 10nm is deposited to form a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer.

[0044] (5) Evacuate to a vacuum level of 5×10⁻⁶ at the bottom of the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0045] Example 3

[0046] A method for preparing an anti-fingerprint coating on an anodized alloy laptop casing includes the following steps:

[0047] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0048] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3 Pa; High-purity argon gas is introduced at a flow rate of 400 sccm, and the stable working pressure is 1.2 × 10⁻⁶. -2 Pa; RF magnetron sputtering process was adopted with a sputtering power of 7kW. The sputtering film thickness was precisely monitored by a crystal oscillator film thickness monitoring method, and a 15nm pure chromium underlayer was deposited.

[0049] (3) The working pressure remains unchanged, the argon flow rate is 400 sccm and the oxygen flow rate is 200 sccm. The target material is switched to a high-purity aluminum target. Radio frequency magnetron sputtering is used with a sputtering power of 4kW. The sputtering film thickness is accurately monitored by using a crystal oscillator film thickness monitoring method to deposit a 20nm aluminum oxide intermediate layer.

[0050] (4) The process gas and pressure in the cavity are kept constant. The high-purity silicon target is replaced. The RF magnetron sputtering power is set to 4.5kW. The sputtering film thickness is accurately monitored by the crystal oscillator film thickness monitoring method. A silicon dioxide transition layer with a thickness of 10nm is deposited to form a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer.

[0051] (5) Evacuate to a vacuum level of 5×10⁻⁶ at the bottom of the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0052] Example 4

[0053] The difference from Example 2 is that a plastic spray-painted part (conventionally used) is used as the substrate instead of the hard anodized magnesium-aluminum alloy laptop shell to obtain an anti-fingerprint coating on the laptop shell.

[0054] Example 5

[0055] The difference from Example 2 is that the anti-fingerprint coating uses Daikin 509 reagent (commercially available) instead of X-71-197 to obtain an anti-fingerprint coating for the laptop shell.

[0056] Example 6

[0057] A method for preparing an anti-fingerprint coating on an anodized alloy laptop casing includes the following steps:

[0058] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0059] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3Pa; High-purity argon and oxygen are introduced, with an argon flow rate of 400 sccm and an oxygen flow rate of 200 sccm, and a stable working pressure of 1.2 × 10⁻⁶ Pa. -2 Pa; RF magnetron sputtering process was adopted with a sputtering power of 3.5kW. The sputtering film thickness was accurately monitored by a crystal oscillator film thickness monitoring method, and a 15nm aluminum oxide layer was deposited.

[0060] High-purity argon gas is introduced at a flow rate of 400 sccm, with a stable working pressure of 1.2 × 10⁻⁶. -2 Pa; RF magnetron sputtering process was adopted with a sputtering power of 7kW. The sputtering film thickness was precisely monitored by a crystal oscillator film thickness monitoring method, and a 15nm pure chromium underlayer was deposited.

[0061] (3) Keep the working pressure unchanged, introduce high-purity argon gas with a flow rate of 400 sccm, switch the target material to a high-purity chromium target, use radio frequency magnetron sputtering with a sputtering power of 7 kW, use crystal oscillator film thickness monitoring method to accurately monitor the sputtering film thickness, and deposit a 15 nm pure chromium intermediate layer.

[0062] (4) The process gas and pressure in the cavity are kept constant. The high-purity silicon target is replaced. The RF magnetron sputtering power is set to 4.5kW. The sputtering film thickness is accurately monitored by the crystal oscillator film thickness monitoring method. A silicon dioxide transition layer with a thickness of 10nm is deposited to form an alumina bottom layer-chromium intermediate layer-silicon dioxide transition layer gradient composite inorganic film system.

[0063] (5) Evacuate to a vacuum level of 5×10⁻⁶ at the bottom of the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0064] Comparative Example 1

[0065] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0066] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3Pa; argon flow rate 400 sccm and oxygen flow rate 200 sccm, replace with high-purity silicon target, RF magnetron sputtering power set to 4.5 kW, use crystal oscillator film thickness monitoring method to accurately monitor sputtering film thickness, deposit 10 nm thick silicon dioxide transition layer.

[0067] (3) Evacuate to a vacuum level of 5×10⁻⁶ at the bottom of the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0068] Comparative Example 2

[0069] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0070] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3 Pa; High-purity argon gas is introduced at a flow rate of 400 sccm, and the stable working pressure is 1.2 × 10⁻⁶. -2 Pa; RF magnetron sputtering technology was employed with a sputtering power of 7kW, and a crystal oscillator was used to precisely monitor the sputtered film thickness, depositing a 15nm pure chromium underlayer.

[0071] (3) The process gas pressure in the cavity remains unchanged, the argon flow rate is 400 sccm and the oxygen flow rate is 200 sccm. The high-purity silicon target is replaced, the radio frequency magnetron sputtering power is set to 4.5 kW, and a 10 nm thick silicon dioxide transition layer is deposited to form a chromium underlayer-silicon dioxide transition layer gradient composite inorganic film system.

[0072] (4) Evacuate to a base vacuum level of 5×10⁻⁶ in the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0073] Comparative Example 3

[0074] (1) Select a magnesium-aluminum alloy notebook shell that has undergone hard anodizing treatment as the substrate; wipe the surface of the substrate with anhydrous ethanol and blow the surface with compressed air. This step is the substrate pretreatment.

[0075] (2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, and the anti-fingerprint coating particles are placed in the molybdenum boat. The low vacuum degree is controlled at 5×10. -1 At Pa, argon gas was introduced, plasma cleaning power was 2kW, cleaning time was 180s, and after plasma cleaning was completed, vacuum was continued until the cavity's base vacuum level was 8×10⁻⁶. -3 Pa; High-purity argon and oxygen are introduced, with an argon flow rate of 400 sccm and an oxygen flow rate of 200 sccm, and a stable working pressure of 1.2 × 10⁻⁶ Pa. -2 Pa; Replace the high-purity aluminum target, adopt the radio frequency magnetron sputtering process, sputtering power of 4kW, and use the crystal oscillator film thickness monitoring method to accurately monitor the sputtering film thickness, and deposit a 20nm aluminum oxide layer.

[0076] (3) The process gas and pressure in the cavity are kept constant. The high-purity silicon target is replaced. The radio frequency magnetron sputtering power is set to 4.5kW. The sputtering film thickness is accurately monitored by the crystal oscillator film thickness monitoring method. A silicon dioxide transition layer with a thickness of 10nm is deposited to form a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer.

[0077] (4) Evacuate to a base vacuum level of 5×10⁻⁶ in the cavity. -3 At 600A, the heating power supply is turned on, and the molybdenum boat is heated to evaporate the anti-fingerprint coating material, which is then deposited onto the substrate via physical vapor deposition. After 300 seconds of heating, heating is stopped, and a stable pressure of 5 × 10⁻⁶ is maintained. -3 Pa, pressure released after 200s, thus obtaining an anti-fingerprint coating on the anodized alloy laptop shell.

[0078] The anti-fingerprint coatings for anodized alloy laptop shells prepared in Examples 1-3 and Comparative Example 1 were subjected to performance tests. The results are shown in Table 1.

[0079] All performance tests of the finished product in this application adopt industry-standard national standards and consumer electronics industry standards: color difference test adopts CIE LAB color difference system test; dyne value adopts standard dyne pen test; abrasion resistance test adopts 0000# steel wool, load 500g, reciprocating wiping test until water contact angle <100° to stop the test; interlayer bonding force adopts the cross-cut adhesion test (GB / T9286-1998); weather resistance adopts constant temperature and humidity test at 45℃ and 95% humidity for 200h, water contact angle >100° is qualified.

[0080] Table 1. Performance test of anti-fingerprint coatings for laptop casings prepared in Examples 1-6 and Comparative Examples 1-3

[0081]

[0082] As shown in Table 1, the synergistic effect of the three-layer gradient film system—chromium underlayer, alumina intermediate layer, and silica transition layer—plays a decisive role in the overall performance of the coating. Examples 1-3 represent the preferred parameter combinations of this application: with a reasonable match between the chromium layer, alumina layer, and silica layer, when the chromium layer thickness is 10-15 nm, the alumina layer thickness is 15-20 nm, and the silica layer thickness is 10 nm, the product's color difference value ΔE ≤ 1.0, surface dyne value stabilizes at around 20, cross-cut adhesion is grade 0, and the appearance, texture, stain resistance, and wear resistance achieve the optimal balance. Under the condition that the thickness of the chromium underlayer and silica transition layer remains unchanged, increasing the thickness of the alumina intermediate layer in the 10-20 nm range can improve the wear resistance of the film system, but the increase in the total thickness of the film layer will lead to the accumulation of internal stress, and the color difference value will increase accordingly. When the total thickness of the film system is higher than 40 nm, the internal stress accumulation of the film layer is severe, which easily causes an increase in appearance color difference and distortion of the metallic matte texture.

[0083] Example 4 uses a plastic spray-painted part substrate instead of anodized magnesium-aluminum alloy substrate. The substrate itself does not have anodized microporous structure, and the anchoring effect between the inorganic film system and the substrate interface is lacking. Although the color difference is acceptable, the cross-cut adhesion test is only level 4, the abrasion resistance is only 300 times, and the weather resistance is NG. This indicates that the gradient inorganic film system of this application is adapted to hard anodized alloy substrates and cannot achieve high adhesion and high weather resistance on non-anodized plastic spray-painted part substrates.

[0084] In Example 5, the anti-fingerprint agent was replaced with Daikin 509 agent. The film structure and sputtering process parameters remained unchanged. Its color difference, dyne value, abrasion resistance, and cross-cut adhesion were comparable to those in Example 2. The weather resistance was OK, proving that the gradient inorganic film system of this application can be adapted to different commercially available fluorine-based anti-fingerprint agents, and the film system structure has good compatibility.

[0085] Example 6 reverses the deposition order of the chromium layer and the alumina layer, adopting an inverted film system structure of alumina bottom layer - chromium intermediate layer - silica transition layer. The chromium layer no longer directly contacts the micropores of the anodic oxide substrate, losing the function of the chromium bottom layer in filling and anchoring the micropores of the substrate. The interlayer stress matching deteriorates, the wear resistance drops to 1000 cycles, the cross-cut adhesion test is grade 2, and the weather resistance is NG. This shows that the chromium bottom layer must be directly deposited on the surface of the anodic oxide alloy substrate to fill the micropores of the substrate. The inverted film layer order cannot achieve the comprehensive performance of this application.

[0086] Comparative Example 1 only has a single-layer silica transition film, lacking a chromium underlayer and an alumina intermediate layer. It lacks micropore filling and stress buffering structures, resulting in poor interfacial bonding. Its abrasion resistance is only 200 cycles, with a cross-cut adhesion rating of 4, and its weather resistance is NG. Comparative Example 2 omits the alumina intermediate layer, retaining only the chromium underlayer-silica bilayer film system. Lacking the stress buffering effect of the alumina intermediate layer, interlayer stress cannot be released. Its abrasion resistance is 500 cycles, with a cross-cut adhesion rating of 3, and its weather resistance is NG. Comparative Example 3 eliminates the chromium underlayer, directly depositing alumina and silica films on the substrate. The chromium underlayer's filling and anchoring effect on the micropores of the anodic oxide substrate is completely lost, leading to a significant decrease in the adhesion between the film and the substrate interface. Its abrasion resistance is 500 cycles, with a cross-cut adhesion rating of 3, and its weather resistance is NG.

[0087] Comparative Examples 1-3 demonstrate that in the three-layer gradient film system, the chromium bottom layer, the alumina intermediate layer, and the silica transition layer are indispensable: the chromium bottom layer is responsible for filling the micropores of the anodized substrate, providing anchoring adhesion between the substrate and the film system; the alumina intermediate layer serves as a stress buffer for the film layer; and the silica transition layer is responsible for connecting the inorganic film system and the organic anti-fingerprint coating. Only through the sequential stacking and synergistic action of these three layers can high wear resistance, grade 0 cross-cut adhesion, excellent resistance to damp heat aging, and low color difference appearance be achieved simultaneously. Traditional single-layer or double-layer simplified film systems show obvious wear and whitening after repeated wiping with steel wool, and their anti-fingerprint performance rapidly declines; while the complete gradient composite film system of this application remains intact and undamaged after more than 2000 wear-resistant wiping cycles, and its anti-fingerprint performance does not show significant decline, fully verifying the significant technical advantages of the process in terms of wear resistance, durability, interfacial bonding, and environmental stability.

[0088] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing an anti-fingerprint coating on an anodized alloy notebook casing, characterized in that: Includes the following steps: 1) Select an alloy notebook shell that has undergone hard anodizing treatment as the substrate, and pre-treat the surface of the substrate by wiping and blowing with ethanol; 2) The pretreated substrate is placed in the vacuum magnetron sputtering chamber, the anti-fingerprint coating particles are placed in the molybdenum boat, and after plasma cleaning under low vacuum, the base vacuum is evacuated and argon gas is introduced. The chromium underlayer is deposited by radio frequency magnetron sputtering. 3) Keep the working pressure of the cavity constant, introduce a mixed process gas of argon and oxygen, switch to aluminum target, and deposit an alumina intermediate layer by radio frequency magnetron sputtering; 4) Keep the process gas and working pressure in the cavity constant, switch the silicon target, and deposit the silicon dioxide transition layer by radio frequency magnetron sputtering to obtain a gradient composite inorganic film system of chromium bottom layer-alumina intermediate layer-silicon dioxide transition layer; 5) Re-evacuate the vacuum, heat the molybdenum boat to evaporate the anti-fingerprint coating film, and deposit it on the substrate using physical vapor deposition. After depressurization, the finished anodized alloy notebook shell is obtained.

2. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: The thickness of each of the chromium underlayer, alumina intermediate layer, and silicon dioxide transition layer is 10nm-20nm.

3. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 2, characterized in that: The thickness of the chromium base layer is 15 nm, the thickness of the aluminum oxide intermediate layer is 15 nm, and the thickness of the silicon dioxide transition layer is 10 nm.

4. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 2), the low vacuum level is 8×10⁻⁶. -1 Pa ~ 1.2 × 10 0 Pa, the cavity's background vacuum is 8 × 10⁻⁶. -3 Pa ~ 1.2 × 10 -2 Pa; High-purity argon gas is introduced at a flow rate of 300~500 sccm, and the working pressure is 8×10. -3 Pa ~ 1.2 × 10 -2 Pa.

5. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 2), the sputtering power is 6~7kW.

6. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 3), the argon flow rate is 300~500 sccm, the oxygen flow rate is 100~200 sccm, and the sputtering power is 3~4 kW.

7. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 4), the sputtering power is 4~5kW.

8. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 5), the vacuum degree is 5 × 10⁻⁶. -3 Pa, heating molybdenum boat to evaporate anti-fingerprint coating film, coating heating time is 300s; after stopping heating, maintain 5×10 -3 The pressure was reduced by 200 Pa for 200 seconds before being released.

9. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: In step 5), the thickness of the anti-fingerprint coating film is 8nm-12nm.

10. The method for preparing the anti-fingerprint coating on the anodized alloy notebook casing according to claim 1, characterized in that: The anodized alloy notebook shell has a dyne value of 20~22, an appearance color difference value ΔE≤1.0, and a bonding strength of 0 in the cross-cut adhesion test.