A cold spray nozzle with a coating composite structure and its preparation method
By adopting an integrated Laval nozzle structure and composite PVD process in the cold spray nozzle, the problems of brittle cracking, interface bonding failure and rapid throat wear of the cold spray nozzle have been solved. This achieves the effect of high temperature resistance, excellent toughness and strong bonding of the inner wall wear-resistant layer, thus extending the service life and reducing the cost.
Patent Information
- Application Number
- CN202611009679.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-08
- Publication Date
- 2026-11-17
AI Technical Summary
Existing cold spray nozzles are prone to brittleness under high temperature and pressure, interfacial bonding failure, and rapid throat wear, resulting in short service life and high cost.
The heat-resistant alloy steel substrate with an integrated Laval nozzle structure is combined with a multi-arc ion plating and magnetron sputtering composite PVD process to deposit a tungsten carbide-based composite coating layer. The throat is locally thickened and subjected to low-temperature tempering treatment to form a transition layer and a wear-resistant surface layer.
It improves the toughness and high-temperature resistance of the nozzle, enhances the adhesion of the wear-resistant layer on the inner wall, extends the service life, and reduces costs.
Smart Images

Figure CN123108549A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the technical field of cold spray nozzle preparation, specifically a cold spray nozzle with a coating composite structure and its preparation method. Background Technology
[0002] Cold spraying technology, as a solid-state deposition process, is widely used in the repair, strengthening, and remanufacturing of metal surfaces in aerospace, marine equipment, and heavy machinery due to its advantages such as low deposition temperature, minimal workpiece oxidation deformation, and low coating porosity. The nozzle, as the core component of cold spraying equipment, must withstand working pressures of 3-10 MPa, high-temperature gases exceeding 600°C, and high-speed particle erosion at speeds of hundreds or even thousands of meters per second. Therefore, the nozzle's wear resistance, high-temperature stability, and structural strength directly determine the spraying accuracy, operational efficiency, and overall service life of the machine.
[0003] Currently, cold spray nozzles used in industry mainly fall into two technical categories: cemented carbide nozzles and composite structure cold spray nozzles. Cemented carbide nozzles are typically made by integrally sintering ultrafine-grained WC-CoCr cemented carbide. While they possess good erosion resistance, the scarcity of raw materials and the extreme difficulty in precision machining result in high overall costs, often several times that of ordinary steel nozzles. Furthermore, cemented carbide is inherently brittle and susceptible to mechanical impact and pressure fluctuations, especially during the thermal shock generated during the start-up and shutdown phases of cold spraying. This can easily lead to microcracks developing inside the nozzle, resulting in cracking and failure. Secondly, due to material properties, it is difficult to fabricate complex cooling channels in integral cemented carbide nozzles, limiting their application under higher power conditions.
[0004] In the field of composite cold spray nozzles, existing technologies attempt to employ a split composite structure, such as embedding a ceramic liner in a metal substrate or preparing a wear-resistant coating on the surface of the metal substrate. Patent document CN102892926A discloses a cold spray nozzle in which the inner wall of the diverging section is made of quartz glass or borosilicate glass to solve the powder adhesion problem. However, such solutions have serious interfacial bonding problems: the thermal expansion coefficients of glass or ceramic materials and metal substrates differ greatly. Under the high temperature, high pressure, and frequent thermal cycling conditions of cold spraying, thermal stress concentration is easily generated at the interface, leading to cracking, peeling, or even nozzle blockage of the liner. In addition, glass and ordinary ceramic materials have low fracture toughness. Under long-term erosion by high-speed hard particles such as tungsten carbide and ceramic powder, the wear rate is much higher than that of cemented carbide, making it difficult to meet the requirements of long-term continuous operation.
[0005] To improve the surface wear resistance of metal substrate nozzles, physical vapor deposition (PVD) technology has been gradually introduced. Patent document CN109023202A discloses a composite coating structure combining flame spraying and PVD coating. A nickel-based tungsten carbide transition layer is first prepared on a 316L stainless steel substrate, and then chromium and chromium nitride films are prepared by multi-arc ion plating, which is applied to the surface protection of ball valves. However, this technology cannot be directly applied to the manufacture of cold spray nozzles: First, the throat of a cold spray nozzle is the core area where fluids accelerate to the speed of sound, and the particle erosion intensity is much higher than that of ordinary valve cavities. Conventional uniform thickness coatings cannot withstand the high-intensity wear of the throat. Second, the aforementioned existing technologies mostly use ordinary austenitic stainless steel as the substrate, which has limited high-temperature strength and oxidation resistance, and cannot withstand the working environment of ≥600℃ for cold spray nozzles for a long time. Furthermore, if the substrate temperature is too high in conventional PVD processes, it will cause annealing and softening of high-performance high-temperature alloy substrates such as GH4169 and Inconel718, reducing the structural strength of the nozzle. On the other hand, if the parameters of a simple low-temperature tempering process are not matched, it cannot effectively eliminate the internal stress generated during the PVD coating process, causing the coating to peel off under thermal cycling conditions.
[0006] In summary, existing technologies, whether the expensive integral cemented carbide approach or the conventional split composite or coating approach, cannot simultaneously solve the problems of brittle cracking, interfacial bonding failure, high-temperature softening, and rapid throat wear. Therefore, developing a low-cost, high-toughness, high-temperature resistant, and durable cold spray nozzle with a firmly bonded inner wear-resistant layer is a pressing technical problem that needs to be solved in this field. Summary of the Invention
[0007] This application provides a cold spray nozzle with a coating composite structure and its preparation method, which provides a solution for a cold spray nozzle that is low in cost, has excellent toughness, high temperature resistance, strong adhesion of the wear-resistant inner wall layer, and long service life.
[0008] This application provides a cold spray nozzle with a coated composite structure, comprising: a heat-resistant alloy steel substrate with an integrated Laval nozzle structure, wherein the substrate is formed from one of 310S high-temperature stainless steel, GH4169 high-temperature alloy, or Inconel 718 alloy; a tungsten carbide-based composite coating layer deposited on the inner wall of the substrate, wherein the composite coating layer is a two-layer structure of a transition layer plus a wear-resistant surface layer, fully covering the inner wall of the nozzle's constriction section, throat, and expansion section, with the wear-resistant surface layer at the throat being thicker than that at the constriction and expansion sections; the composite coating layer is deposited on the inner wall of the substrate using a multi-arc ion plating and magnetron sputtering composite PVD process.
[0009] By adopting the above technical solutions, this application employs an integrated Laval nozzle structure with a heat-resistant alloy steel substrate and a continuous PVD coating on the entire inner wall. The heat-resistant alloy steel substrate offers good toughness, allows for the fabrication of complex cooling channels, and avoids the risk of brittle fracture of the entire WC under start-up and shutdown thermal shock. Furthermore, the throat of the cold spray nozzle is the core area for particle acceleration to the speed of sound. This application introduces a gradient design with localized thickening of the throat in the PVD coating scheme, matching the wear life of the weakest throat with the contraction / expansion section, thus preventing a decrease in spraying accuracy due to rapid orifice expansion.
[0010] Preferably, the transition layer is a titanium layer, a chromium layer, or a titanium-chromium alloy layer; the wear-resistant surface layer is a WC layer or a WC-Co layer.
[0011] By adopting the above technical solution, the transition layer in this application is Ti / Cr / TiCr; the wear-resistant surface layer is WC or WC-Co. This solves the problem of peeling caused by the difference in thermal expansion between WC and the high-temperature alloy substrate. Ti, Cr, and TiCr, as transition layers, act as a buffer for the thermal expansion gradient, significantly reducing the interfacial shear stress under thermal cycling and preventing coating peeling. The WC-Co surface layer has better toughness than pure WC and can better withstand the impact of high-speed particles; the Ti / Cr transition layer itself also has a certain degree of corrosion resistance and oxidation resistance, making it suitable for cold spraying and high-temperature oxidation conditions.
[0012] Preferably, the thickness of the transition layer is 0.5-2 μm; the wall thickness of the wear-resistant surface layer in the contraction and expansion sections is 5-20 μm, and the thickness of the wear-resistant surface layer at the throat position is 15-30 μm.
[0013] On the other hand, this application provides a method for preparing a cold spray nozzle with a coating composite structure, comprising the following steps: S1, integrally forming a Laval nozzle substrate using 310S, GH4169 or Inconel 718 high-temperature alloy steel; S2, performing degreasing, pickling, and plasma etching micro-roughening pretreatment on the inner wall of the substrate in sequence to control the roughness of the inner wall; S3, using a multi-arc ion plating and magnetron sputtering composite PVD process, first depositing a transition layer on the inner wall of the substrate, and then depositing a WC or WC-Co wear-resistant surface layer; S4, subjecting the coated nozzle to low-temperature tempering treatment, and heat preservation to eliminate the internal stress of the coating, and obtaining the finished product after furnace cooling.
[0014] By adopting the above technical solution, the preparation method of this application ensures consistent performance through a complete process chain. The four steps are interconnected, from substrate forming, surface cleaning, film deposition to stress relief, forming a complete closed-loop process to ensure consistent nozzle performance during mass production. Finally, low-temperature tempering is used to eliminate PVD internal stress. During the deposition process, Ar ion bombardment and thermal mismatch can leave residual internal stress. Low-temperature tempering can effectively release stress and prevent the film from cracking and peeling off under cold spray thermal cycling conditions.
[0015] Preferably, in step S2, the plasma etching uses an Ar+H2 mixed gas, with H2 accounting for 5%-10% of the volume, a vacuum degree of 15-25Pa, a power of 400-500W, and an etching time of 4-6min.
[0016] Preferably, in step S2, degreasing is performed using a mixed degreasing solution of sodium hydroxide 10-18 g / L, sodium carbonate 6-10 g / L, sodium silicate 3-5 g / L, and OP-10 surfactant 1-3 g / L, with ultrasonic-assisted cleaning at 65-75°C for 6-10 min; pickling is performed using a mixed acid solution of nitric acid 10-15% and hydrofluoric acid 3-5% at room temperature for 2-4 min.
[0017] Preferably, in step S3, the cathode current is 75-80A when the transition layer is deposited by multi-arc ion plating, and the substrate bias voltage is -70~-150V when the WC surface layer is deposited by magnetron sputtering.
[0018] Preferably, in step S4, the low-temperature tempering treatment is performed at a temperature of 180-220°C for 1-2 hours, which is used to match the annealing window of GH4169 or Inconel718 high-temperature alloy matrix above 650°C.
[0019] One or more technical solutions provided in this application have at least the following technical effects or advantages: 1. This application adopts an integrated heat-resistant alloy steel substrate, a double-layer PVD gradient coating on the inner wall, local thickening and strengthening of the throat, and low-temperature tempering as a synergistic process, which reduces the overall cost and provides good substrate toughness, allowing for the processing of complex cooling channels.
[0020] 2. The process in this application enables the cold spray nozzle to have high temperature resistance and thermal shock resistance, avoids the softening of the substrate during annealing, and greatly improves the thermal cycling stability; in addition, the thickened throat design is precisely matched with the erosion distribution of the cold spray flow field, and the nozzle deviation after continuous spraying is better than that of the glass-lined nozzle.
[0021] 3. This application employs double-layer coating, micro-roughening pretreatment, and composite PVD process to increase the adhesion of WC coating and solve the industry problem of interface peeling of split composite nozzles. Attached Figure Description
[0022] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0023] Figure 1This is a cross-sectional view of the nozzle structure in this invention; Figure 2 This is a magnified view of a portion of the nozzle throat area.
[0024] Explanation of reference numerals in the attached drawings: 1. Nozzle substrate; 2. Transition layer; 3. Wear-resistant layer. Detailed Implementation
[0025] This application provides a cold spray nozzle with a coating composite structure and its preparation method, which provides a solution for a cold spray nozzle that is low in cost, has excellent toughness, high temperature resistance, strong adhesion of the wear-resistant inner wall layer, and long service life.
[0026] The technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of this application, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without creative effort are within the scope of protection of this application.
[0027] It should be noted that the terms "first," "second," etc., in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that the embodiments of this application described herein can be implemented in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or server that comprises a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or modules not explicitly listed or inherent to such processes, methods, products, or devices.
[0028] Example 1
[0029] GH4169 high-temperature alloy was selected, and the Laval nozzle substrate was integrally formed by CNC precision machining. The pretreatment used a mixed degreasing solution of sodium hydroxide 15g / L, sodium carbonate 8g / L, sodium silicate 4g / L, and OP-10 surfactant 2g / L. The substrate was ultrasonically assisted cleaned for 8 minutes at 70±5℃. After rinsing and drying, it was acid-washed at room temperature for 3 minutes with a mixed acid solution of 12% nitric acid and 4% hydrofluoric acid. After rinsing, neutralization, and drying, it was etched for 5 minutes using an RF vacuum plasma cleaner with Ar+H2 mixed gas (H2 content 8%) as the working gas at a vacuum degree of 20Pa and a power of 450W. After etching, a multi-arc ion plating and magnetron sputtering composite PVD process was used within 30 minutes to deposit a 1μm titanium transition layer and a 10μm WC-Co wear-resistant surface layer (throat thickened to 20μm). The substrate temperature was controlled at 420℃ during the coating process. Finally, the finished product was obtained by low-temperature tempering at 200℃ for 1.5 hours.
[0030] Furthermore, this application conducts performance tests on the obtained finished product, including testing the inner wall hardness, bonding strength, and nozzle size deviation. The testing standards are as follows: 1. Inner wall hardness test: According to GB / T230.1 "Rockwell hardness test of metallic materials", five test points are evenly selected on the inner wall of the nozzle using a Rockwell hardness tester (HRA scale), and the average value is taken as the final hardness value; for non-metallic materials such as glass lining, the hardness is tested with a micro Vickers hardness tester (HV5) and then converted to HRA equivalent value.
[0031] 2. Adhesion strength test: For coated samples, according to GB / T30706 "Determination of adhesion strength of physical vapor deposition coatings - scratch method", a scratch method coating adhesion strength tester is used, and the critical load (unit: N) when the coating peels off continuously is used as the adhesion strength judgment value.
[0032] 3. Nozzle size deviation detection: A high-precision tool microscope with an accuracy of ±0.001mm was used to measure the minimum diameter of the nozzle throat before and after the test. Three cross sections were taken along the axial direction for each sample, and the maximum diameter change was taken as the nozzle size deviation value.
[0033] Based on the above performance tests, the inner wall hardness of the finished product is HRA89, the coating bonding strength is 60N, there is no peeling or softening after 2 hours of constant temperature at 600℃, the nozzle size deviation is ≤0.02mm after 50 hours of continuous spraying of hard alloy powder, and the overall cost is 30% of that of the overall tungsten carbide nozzle.
[0034] Example 2 The Laval nozzle substrate is made of 310S high-temperature resistant stainless steel and is integrally formed by CNC precision machining. The pretreatment uses a mixed degreasing solution of sodium hydroxide 18g / L, sodium carbonate 10g / L, sodium silicate 5g / L, and OP-10 surfactant 3g / L. It is ultrasonically assisted cleaned for 10 min at 75±5℃. After rinsing and drying, it is acid-washed at room temperature for 4 min with a mixed acid solution of 15% nitric acid and 5% hydrofluoric acid. After rinsing, neutralization, and drying, it is etched for 6 min at 25Pa vacuum and 500W power using an RF vacuum plasma cleaner with Ar+H2 mixed gas (H2 content 10%) as the working gas. After etching, a multi-arc ion plating and magnetron sputtering composite PVD process is used within 25 min to deposit a 1.5μm chromium transition layer and a 12μm WC wear-resistant surface layer (throat thickened to 25μm). The substrate temperature is controlled at 440℃ during the coating process. Finally, the finished product is obtained by low-temperature tempering at 220℃ for 2 h.
[0035] Performance testing: The inner wall hardness of the finished product is HRA90, the coating bonding strength is 65N, there is no peeling or softening after 2 hours of constant temperature at 650℃, the nozzle size deviation is ≤0.02mm after 60 hours of continuous spraying of ceramic powder, and the overall cost is 35% of that of the overall tungsten carbide nozzle.
[0036] Example 3 Inconel 718 high-temperature alloy was selected, and the Laval nozzle substrate was integrally formed by CNC precision machining. The pretreatment used a mixed degreasing solution of sodium hydroxide 12g / L, sodium carbonate 6g / L, sodium silicate 3g / L, and OP-10 surfactant 1g / L. The substrate was ultrasonically assisted to clean for 6 minutes at 65±5℃. After rinsing and drying, the substrate was acid-washed at room temperature for 2 minutes with a mixed acid solution of 10% nitric acid and 3% hydrofluoric acid. After rinsing, neutralization, and drying, the substrate was etched for 4 minutes using an RF vacuum plasma cleaner with a mixture of Ar and H2 gas (H2 content 5%) as the working gas at a vacuum of 15Pa and a power of 400W. After etching, a multi-arc ion plating and magnetron sputtering composite PVD process was used within 20 minutes to deposit a 0.8μm titanium-chromium alloy transition layer and an 8μm WC-Co wear-resistant surface layer (thickened to 18μm at the throat). The substrate temperature was controlled at 400℃ during the coating process. Finally, the substrate was tempered at 180℃ for 1 hour to obtain the finished product.
[0037] Performance testing: The inner wall hardness of the finished product is HRA88, the coating bonding strength is 55N, there is no peeling or softening after 2 hours of constant temperature at 600℃, the nozzle size deviation is ≤0.02mm after 45 hours of continuous spraying of hard alloy powder, and the overall cost is 28% of that of the integral tungsten carbide nozzle.
[0038] Comparative Example 1 Comparative Example 1 uses a split structure with a metal substrate and a borosilicate glass inlay liner. The specific preparation steps are as follows: The nozzle base is made of 304 stainless steel bar and manufactured by CNC precision machining. It consists of two parts: a front base and a rear outer sleeve. The front base is machined with a complete constriction section and throat flow channel, and the throat dimensions are the same as in Example 1. The rear outer sleeve is a cylindrical structure with a reserved allowance for inlay fitting in the inner hole. The inner hole diameter and the outer diameter of the glass liner are designed with an interference fit tolerance of H7 / p6. The outer wall of the outer sleeve is machined with connecting threads that match those of the front base.
[0039] High borosilicate glass blanks are selected, and the expansion section flow channel surface is processed by precision internal cylindrical grinding and surface polishing. The inlet end angle is smoothly connected with the throat outlet of the front substrate. The outer cylindrical grinding is made to the target size for interference fit with the rear jacket. The inner liner is chamfered at both ends with 0.5×45° to remove burrs. After ultrasonic cleaning with deionized water and dust-free drying, it is ready for use.
[0040] The rear metal jacket is placed in a box furnace and heated to 350°C and held for 20 minutes. After being removed, the borosilicate glass liner is quickly pressed axially into the inner hole of the jacket and allowed to cool naturally to room temperature. The interference fit is achieved through the thermal expansion and contraction of the metal. The front substrate and the rear jacket are then assembled into an integral nozzle by tightening the threads. A coaxiality gauge is used to ensure that the coaxiality between the throat and the glass liner inlet is ≤0.02mm, thus obtaining the finished product.
[0041] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses a common austenitic stainless steel substrate and a single magnetron sputtering uniform coating process, omitting the plasma etching for micro-roughening, throat coating thickening, and low-temperature tempering post-treatment steps. The specific preparation steps are as follows: The Laval nozzle substrate was integrally formed using 316L austenitic stainless steel bars and precision CNC machining. The flow channel profile, throat dimensions, and overall shape were completely identical to the substrate in Example 1. Only a conventional alkaline degreasing process was used, employing an alkaline degreasing solution containing 20 g / L sodium hydroxide and 10 g / L sodium carbonate. Ultrasonic cleaning was performed at 60°C for 10 minutes to remove machining oil stains from the inner wall. After rinsing with pure water and hot air drying, it was directly transferred to the coating process without acid pickling activation or plasma etching. The original roughness Ra of the inner wall was ≤0.8 μm.
[0042] The pretreated substrate was loaded into a single magnetron sputtering coating device, and the vacuum was evacuated to a base vacuum level of 5×10⁻⁶. -3 The working pressure was 0.5 Pa by introducing high-purity argon gas. First, a pure chromium target was used to deposit a 1 μm Cr transition layer at 80 W sputtering power. Then, a WC alloy target was switched to deposit a WC wear-resistant surface layer at 120 W sputtering power. The substrate heating temperature was controlled at 330℃ throughout the coating process, without applying a negative bias voltage. The coating thickness was uniform across the entire flow channel, with a total wear-resistant surface layer thickness of 15 μm. After coating, the film was cooled to room temperature in the furnace and removed directly without low-temperature tempering to relieve stress, yielding the finished product.
[0043] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 was prepared using an industrially common ultrafine-grained WC-CoCr integral sintering process, which is the standard preparation route for currently commercially available high-end cold spray nozzles. It uses an integrated synthesis method, and its specific preparation steps are as follows: Ultrafine WC powder with an average particle size of 0.8 μm was selected and mixed with 10 wt% metallic Co powder and 4 wt% metallic Cr powder as binder phases. Anhydrous alcohol was used as the ball milling medium and the mixture was ball-milled in a planetary ball mill for 24 hours to achieve uniform mixing. After adding paraffin forming agent, the mixture was spray-dried to obtain a cemented carbide mixture.
[0044] The mixture is filled into the nozzle forming mold and pressed into a nozzle blank by holding the pressure at 200MPa for 30s using a cold isostatic pressing process. The blank is reserved with a dimensional allowance of about 18% based on the sintering shrinkage rate, and also with allowance for subsequent finishing.
[0045] The compact is placed in a vacuum sintering furnace, where it is first held at 500°C for 1 hour to remove the forming agent, and then heated to 1420°C for vacuum sintering for 2 hours to achieve complete densification of the alloy. After cooling in the furnace, a cemented carbide sintered compact is obtained.
[0046] The sintered blank is precision machined using CNC internal and external cylindrical grinding machines in conjunction with slow wire EDM to produce a complete Laval flow channel consisting of a contraction section, throat, and expansion section. Finally, the throat dimensional accuracy is ensured to be ±0.01mm and the inner wall roughness Ra≤0.4μm through grinding and polishing to obtain the finished integral cemented carbide nozzle.
[0047] The test results of Comparative Examples 1-3 and Examples 1-3 are integrated into the following table.
[0048] Table 1. Detection results of Examples 1-3 and Comparative Examples 1-3
[0049] Example 1 achieved a bonding strength of 60N, thanks to the 200℃ tempering and strict control of the substrate processing temperature, which avoided performance degradation caused by high temperatures. Example 2 achieved the highest hardness of HRA90, indicating that the 25μm throat thickening layer effectively resists ceramic powder erosion and is suitable for high-wear conditions. In addition, Example 3 improved surface activity through Ar+H2 plasma etching, combined with low-temperature tempering at 180℃, maintaining a high bonding strength of 55N at the lowest cost.
[0050] Analysis of Example 1, in conjunction with Comparative Example 1, shows that although the glass liner exhibits certain corrosion resistance at room temperature, under the conditions of high temperature, high pressure, and frequent thermal shock during cold spraying, the nozzle deviation reaches as high as 0.062 mm, and the cost increases by as much as 45%. This exposes the fundamental flaw of the significant difference in thermal expansion coefficients between inorganic non-metallic materials and metallic substrates. Furthermore, because the inner wall uses a glass liner, its hardness fractured during testing, and the two materials are nested together with low bonding strength, leading to fracture under thermal cycling conditions.
[0051] Furthermore, Comparative Example 2 lacked plasma etching for micro-roughening and low-temperature tempering processes specifically for high-temperature alloys, resulting in high internal stress and weak adhesion in the coating. It employed a uniform thickness coating, neglecting the unique flow field characteristics of the throat of the cold spray nozzle, where particle velocities are highest and erosion is most severe. This demonstrates that this application, by introducing a localized thickening design at the throat and a transition layer buffer structure, improves the adhesion to approximately 60N, with deviations controlled to ≤0.02mm.
[0052] Comparative Example 3 utilizes existing technology, specifically the integral sintering of ultrafine-grained WC-CoCr cemented carbide. While it exhibits good erosion resistance, the raw materials are scarce and precision machining is extremely difficult, resulting in high overall costs. Furthermore, due to material properties, it is difficult to fabricate complex cooling channels in integral cemented carbide nozzles, limiting their application under higher power conditions.
[0053] It should be further noted that the integrated heat-resistant alloy steel matrix used in the cold spray nozzle of this application has strict annealing window constraints. The maximum stable temperature of the main strengthening phase of GH4169 is 650℃, and it tends to transform into the δ phase above 650℃. After annealing in the 650-700℃ range, the yield strength of Inconel 718 can decrease by 15-20%, and above 700℃, the γ″ phase coarsens rapidly and transforms into the δ phase. Therefore, when high-temperature alloys such as GH4169 / Inconel 718 are used as load-bearing matrices, their long-term operating temperature and associated process temperature must be strictly controlled below 650℃; otherwise, annealing softening will occur, leading to bulging or even instability of the nozzle outer circumference under pressure.
[0054] In addition, the design for locally thickening the wear-resistant layer in the throat of the cold spray nozzle is because the working gas flow velocity reaches the speed of sound in the throat, and the particle velocity accelerates from subsonic to supersonic in the 50mm range from the throat to the expansion section. The throat and the front section of the expansion section are the areas with the most severe particle erosion. According to ANSYS Fluent erosion simulation (or actual measurement by high-speed camera), the erosion rate of the throat is about 3-5 times that of the contraction section and 2-3 times that of the rear section of the expansion section. Therefore, the wear-resistant layer in the throat needs to be locally thickened.
[0055] It should be noted that the order of the embodiments described above is merely for descriptive purposes and does not represent the superiority or inferiority of the embodiments. Furthermore, specific embodiments have been described above. Other embodiments are within the scope of the appended claims. In some cases, the actions or steps described in the claims can be performed in a different order than that shown in the embodiments and still achieve the desired result. Additionally, the processes depicted in the drawings do not necessarily require a specific or sequential order to achieve the desired result. In some embodiments, multitasking and parallel processing are also possible or may be advantageous.
[0056] The above description is only a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the protection scope of this application.
[0057] This specification and accompanying drawings are merely illustrative examples of this application and are intended to cover any and all modifications, variations, combinations, or equivalents within the scope of this application. Clearly, those skilled in the art can make various alterations and modifications to this application without departing from its scope. Therefore, if such modifications and modifications fall within the scope of this application and its equivalents, this application intends to include such modifications and modifications.
Claims
1. A cold spray nozzle with a coating composite structure, characterized in that, include: The heat-resistant alloy steel substrate of the integrated Laval nozzle structure is formed from one of 310S high-temperature stainless steel, GH4169 high-temperature alloy or Inconel 718 alloy. A tungsten carbide-based composite coating layer is deposited on the inner wall of the substrate. The composite coating layer is a two-layer structure consisting of a transition layer and a wear-resistant surface layer, which fully covers the inner wall of the nozzle's constriction section, throat, and expansion section. The thickness of the wear-resistant surface layer at the throat position is greater than that at the constriction and expansion sections. The composite coating layer is deposited on the inner wall of the substrate using a multi-arc ion plating and magnetron sputtering combined PVD process.
2. The cold spray nozzle with a coating composite structure as described in claim 1, characterized in that, The transition layer is a titanium layer, a chromium layer, or a titanium-chromium alloy layer; The wear-resistant surface layer is a WC layer or a WC-Co layer.
3. The cold spray nozzle with a coating composite structure as described in claim 2, characterized in that, The thickness of the transition layer is 0.5-2 μm; the wall thickness of the wear-resistant surface layer in the contraction and expansion sections is 5-20 μm, and the thickness of the wear-resistant surface layer at the throat position is 15-30 μm.
4. A method for preparing a cold spray nozzle with a coating composite structure as described in any one of claims 1-3, characterized in that, Includes the following steps: S1. The Laval nozzle substrate is integrally machined from 310S, GH4169 or Inconel 718 heat-resistant alloy steel. S2. The inner wall of the substrate is subjected to degreasing, pickling, and plasma etching micro-roughening pretreatment in sequence to control the roughness of the inner wall. S3. A multi-arc ion plating and magnetron sputtering composite PVD process is adopted to first deposit a transition layer on the inner wall of the substrate, and then deposit a WC or WC-Co wear-resistant surface layer. S4. After coating, the nozzle is subjected to low-temperature tempering and heat preservation to eliminate internal stress of the coating. After cooling in the furnace, the finished product is obtained.
5. The method for preparing a cold spray nozzle with a coating composite structure as described in claim 4, characterized in that, In step S2, the plasma etching uses an Ar+H2 mixed gas, with H2 accounting for 5%-10% of the volume, a vacuum degree of 15-25Pa, a power of 400-500W, and an etching time of 4-6min.
6. The method for preparing a cold spray nozzle with a coating composite structure as described in claim 5, characterized in that, In step S2, degreasing is performed using a mixed degreasing solution of sodium hydroxide 10-18 g / L, sodium carbonate 6-10 g / L, sodium silicate 3-5 g / L, and OP-10 surfactant 1-3 g / L, with ultrasonic-assisted cleaning at 65-75°C for 6-10 min; pickling is performed using a mixed acid solution of nitric acid 10-15% and hydrofluoric acid 3-5% at room temperature for 2-4 min.
7. The method for preparing a cold spray nozzle with a coating composite structure as described in claim 4, characterized in that, In step S3, the cathode current is 75-80A when the transition layer is deposited by multi-arc ion plating, and the substrate bias voltage is -70~-150V when the WC surface layer is deposited by magnetron sputtering.
8. The method for preparing a cold spray nozzle with a coating composite structure as described in claim 4, characterized in that, In step S4, the low-temperature tempering treatment is performed at a temperature of 180-220°C for 1-2 hours, which is used to match the annealing window of GH4169 or Inconel718 high-temperature alloy matrix above 650°C.
Citation Information
Patent Citations
Nozzle for cold spray, and cold spray device using nozzle for cold spray
CN102892926A
Structure of flame spraying+PVD coating composite spraying-coating film layer and preparation method thereof
CN109023202A