A hydrogen evolution catalyst modified with an atomic layer deposition ultrathin oxide and its preparation method

By constructing an ultrathin oxide layer on the surface of the NiMo alloy catalyst layer using atomic layer deposition technology, the problem of imprecise oxide thickness control in existing technologies is solved, thereby improving catalyst activity and stability. This method is applicable to a variety of substrates and oxides and has good versatility and potential for large-scale preparation.

CN123108634APending Publication Date: 2026-11-17NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611515434.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve ultrathin oxide modification of HER catalysts, making it difficult to precisely control oxide thickness. This results in uneven interfaces, poor reproducibility, and insufficient catalytic efficiency and stability.

Method used

An ultrathin oxide layer was constructed on the surface of a NiMo alloy catalyst layer using atomic layer deposition technology. The oxide thickness was precisely controlled by constant potential electrodeposition and atomic layer deposition methods, thereby optimizing the interfacial water dissociation and hydrogen adsorption capabilities.

Benefits of technology

It achieves a significant improvement in catalyst activity and stability, with precise control over the electronic structure of catalytic active sites. It is applicable to different conductive substrates and oxide types, and has good versatility and potential for large-scale preparation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108634A_ABST
    Figure CN123108634A_ABST
Patent Text Reader

Abstract

This invention discloses an atomic layer deposition (ALD) ultrathin oxide-modified hydrogen evolution catalyst and its preparation method, belonging to the field of electrocatalytic hydrogen evolution technology. The method involves: pretreating a conductive substrate; constructing a NiMo alloy catalyst layer on the pretreated conductive substrate surface using a constant potential electrodeposition method; depositing an ultrathin oxide modification layer with a thickness of 1.2–1.5 nm on the NiMo catalyst layer surface; and finally performing a reduction activation treatment in a reducing atmosphere to obtain the ALD ultrathin oxide-modified hydrogen evolution catalyst. This invention utilizes the atomic-level precision control capability of ALD technology to construct a precisely controllable thickness ultrathin oxide interface layer on the NiMo alloy surface, effectively regulating the electronic structure of active sites, synergistically optimizing the interfacial water dissociation and hydrogen adsorption capabilities, significantly improving the hydrogen evolution activity and stability of the catalyst, and demonstrating good applicability to various substrates and oxide types.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of electrocatalytic hydrogen evolution technology, and more specifically, relates to an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst and its preparation method. Background Technology

[0002] Hydrogen energy, as a clean energy carrier, plays a crucial role in energy transition. The hydrogen evolution reaction (HER) in water electrolysis for hydrogen production is one of the core half-reactions. Currently, commonly used HER catalysts include Pt-based noble metal catalysts and non-noble metal materials such as transition metal sulfides, phosphides, and nitrides. However, the following problems still exist: noble metals are expensive and difficult to apply on a large scale; non-noble metal catalysts have insufficient stability in acidic or alkaline environments; the electronic structure of the catalytic active sites is difficult to precisely control; and the interfacial water dissociation capacity and hydrogen adsorption capacity are difficult to optimize synergistically, thus limiting further improvement in catalytic efficiency.

[0003] Previous studies have shown that constructing oxide-metal interfaces can effectively regulate d-band centers and optimize the adsorption free energy of reaction intermediates. However, traditional wet coating or sol-gel methods struggle to achieve atomically precise control of oxide thickness, resulting in inhomogeneous interfaces with poor reproducibility, failing to fully leverage interfacial synergistic effects. Atomic layer deposition (ALD) technology, based on self-limiting surface reactions, possesses the capability for atomically precise thickness control. However, there are currently few effective reports on its application in the modification of ultrathin oxides for hydrogen evolution catalysts to precisely construct oxide-metal interfaces and synergistically optimize water dissociation and hydrogen adsorption energies.

[0004] Therefore, there is an urgent need to develop an ultrathin oxide modification method that can achieve precise atomic-level thickness control in order to obtain an efficient and stable hydrogen evolution catalytic system. Summary of the Invention

[0005] To address the aforementioned problems in existing technologies, the present invention aims to provide a method for preparing an atomic layer deposition (ALD) ultrathin oxide-modified hydrogen evolution catalyst. This method utilizes the atomic-level precision control capability of ALD technology to construct a precisely controllable ultrathin oxide interface layer on the surface of NiMo alloys, effectively regulating the electronic structure of active sites and synergistically optimizing the interfacial water dissociation and hydrogen adsorption capabilities, thereby significantly improving the hydrogen evolution activity and stability of the catalyst. Another technical problem to be solved by the present invention is to provide an ALD ultrathin oxide-modified hydrogen evolution catalyst prepared by the above method, which exhibits high activity, good stability, precisely controllable interface structure, and broad applicability.

[0006] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst includes the following steps:

[0008] 1) The conductive substrate is pretreated to obtain a pretreated conductive substrate;

[0009] 2) Using the pretreated conductive substrate obtained in step 1) as the working electrode, a NiMo alloy catalyst layer is deposited on its surface by constant potential electrodeposition to obtain a NiMo / conductive substrate electrode.

[0010] 3) Place the NiMo / conductive substrate electrode obtained in step 2) in an atomic layer deposition system, and perform atomic layer deposition of an ultrathin oxide layer on the surface of the NiMo alloy catalyst layer to obtain a continuous and uniform ultrathin oxide modified layer.

[0011] 4) The modified electrode obtained in step 3) is subjected to reduction activation treatment in a reducing atmosphere to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

[0012] Preferably, in step 1), the conductive substrate is nickel foam or carbon paper.

[0013] Preferably, in step 1), the pretreatment process is as follows: the conductive substrate is ultrasonically cleaned in acetone, anhydrous ethanol, and deionized water for 15 min each, then the cleaned conductive substrate is immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min, then rinsed with deionized water until neutral, and dried in a 60℃ forced-air drying oven for 2 h to obtain the pretreated conductive substrate.

[0014] Preferably, in step 2), a pretreated conductive substrate is used as the working electrode, a Pt sheet is used as the counter electrode, and Ag / AgCl is used as the reference electrode.

[0015] Preferably, in step 2), the electrolyte for the constant potential electrodeposition method consists of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH is adjusted to 9.5 with ammonia; the deposition potential is -1.3 V relative to the Ag / AgCl electrode, and the deposition time is 10~15 min.

[0016] Preferably, in step 3), the ultrathin oxide is Al2O3 or TiO2; the atomic layer deposition cycle is 10 to 15 times.

[0017] Preferably, when the ultrathin oxide is Al2O3, the atomic layer deposition uses trimethylaluminum as the aluminum source and deionized water vapor as the oxygen source, the deposition temperature is 120°C, and each deposition cycle includes: a trimethylaluminum pulse of 0.1 s, a nitrogen purging of 20 s, a water vapor pulse of 0.1 s, and a nitrogen purging of 20 s.

[0018] Preferably, when the ultrathin oxide is TiO2, the atomic layer deposition uses titanium tetrachloride as the titanium source and deionized water vapor as the oxygen source, the deposition temperature is 150°C, and each deposition cycle includes: titanium tetrachloride pulse for 0.2 s, nitrogen purging for 25 s, water vapor pulse for 0.2 s, and nitrogen purging for 25 s.

[0019] Preferably, in step 4), the reduction and activation process is as follows: in a 5% H2 / Ar mixed gas atmosphere, the temperature is increased to 300~400℃ at 5℃ / min, held for 1~2 h, and then naturally cooled to room temperature.

[0020] An atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst is prepared by the method described above.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following advantages:

[0022] 1) This invention uses atomic layer deposition technology to precisely construct an ultrathin oxide modification layer on the surface of NiMo alloy catalyst layer. By utilizing the atomic-level thickness control advantage of ALD self-limiting surface reaction, a 1.2~1.5 nm oxide coating layer with precise and controllable thickness and continuous uniformity is obtained, overcoming the problems of uneven coating, poor repeatability and inaccurate thickness control of traditional wet chemical methods.

[0023] 2) The ultrathin oxide-modified layer of the present invention is within the critical thickness range that balances the synergistic effect of electron tunneling and interface regulation. It not only ensures efficient charge transport, but also effectively regulates the d-band center of NiMo and optimizes the hydrogen adsorption free energy. At the same time, the hydroxylation sites on the oxide surface can promote the water dissociation step, thus achieving synergistic optimization of water dissociation capacity and hydrogen adsorption capacity. It exhibits significantly improved hydrogen evolution activity and excellent stability in both alkaline and acidic media.

[0024] 3) The preparation method of the present invention has good universality and can be applied to different conductive substrates such as nickel foam and carbon paper. Different types of ultrathin oxides such as Al2O3 and TiO2 can be selected. It also has a wide adaptability to process windows such as reduction and activation temperature, and can obtain excellent hydrogen evolution catalytic performance.

[0025] 4) The preparation process of this invention is simple and highly controllable. Both electrodeposition and atomic layer deposition are mature industrial technologies, which are easy to scale up and have good application prospects. Attached Figure Description

[0026] Figure 1 This is a comparison diagram of the overpotentials of the hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3;

[0027] Figure 2This is a comparison diagram of the double-layer capacitance of the hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3;

[0028] Figure 3 This is a comparison graph of the charge transfer resistance of the hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3;

[0029] Figure 4 The graph shows a comparison of the 20-h current decay rate and Faraday efficiency of the hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3. Detailed Implementation

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention is further described below with reference to specific embodiments. Unless otherwise specified, the technical means used in the following embodiments are all conventional means well known to those skilled in the art. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer are followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0031] In the following examples, the nickel foam used has a porosity of ≥95%, a thickness of 1.5 mm, and is cut into 1 cm × 2 cm dimensions.

[0032] Example 1

[0033] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0034] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0035] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0036] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Trimethylaluminum (TMA) was used as the aluminum source and deionized water vapor was used as the oxygen source. An atomic layer deposition of an Al2O3 ultrathin oxide layer was performed at a deposition temperature of 120℃. Each deposition cycle consisted of: TMA pulse for 0.1 s, high-purity nitrogen purging for 20 s, H2O pulse for 0.1 s, and high-purity nitrogen purging for 20 s. A total of 10 cycles were performed to obtain a continuous and uniform Al2O3 ultrathin modified layer with a thickness of 1.2 nm.

[0037] 4) The electrode modified by atomic layer deposition in step 3) was placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate was controlled at 100 mL / min, the temperature was increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst, denoted as Al2O3@NiMo / nickel foam.

[0038] Example 2

[0039] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0040] 1) The carbon paper was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated carbon paper.

[0041] 2) Using the pretreated carbon paper obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 15 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0042] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Trimethylaluminum (TMA) was used as the aluminum source and deionized water vapor was used as the oxygen source. An atomic layer deposition of an Al2O3 ultrathin oxide layer was performed at a deposition temperature of 120℃. Each deposition cycle consisted of: TMA pulse for 0.1 s, high-purity nitrogen purging for 20 s, H2O pulse for 0.1 s, and high-purity nitrogen purging for 20 s. A total of 10 cycles were performed to obtain a continuous and uniform Al2O3 ultrathin modified layer with a thickness of 1.2 nm.

[0043] 4) The electrode modified by atomic layer deposition in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

[0044] Example 3

[0045] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0046] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0047] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0048] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Trimethylaluminum (TMA) was used as the aluminum source and deionized water vapor was used as the oxygen source. An atomic layer deposition of an Al2O3 ultrathin oxide layer was performed at a deposition temperature of 120℃. Each deposition cycle consisted of: TMA pulse for 0.1 s, high-purity nitrogen purging for 20 s, H2O pulse for 0.1 s, and high-purity nitrogen purging for 20 s. A total of 15 cycles were performed to obtain a continuous and uniform Al2O3 ultrathin modified layer with a thickness of 1.5 nm.

[0049] 4) The electrode modified by atomic layer deposition in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

[0050] Example 4

[0051] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0052] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0053] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0054] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Trimethylaluminum (TMA) was used as the aluminum source and deionized water vapor was used as the oxygen source. An atomic layer deposition of an Al2O3 ultrathin oxide layer was performed at a deposition temperature of 120℃. Each deposition cycle consisted of: TMA pulse for 0.1 s, high-purity nitrogen purging for 20 s, H2O pulse for 0.1 s, and high-purity nitrogen purging for 20 s. A total of 10 cycles were performed to obtain a continuous and uniform Al2O3 ultrathin modified layer with a thickness of 1.2 nm.

[0055] 4) The electrode modified by atomic layer deposition in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 400℃ at 5℃ / min and held for 1 h, and then naturally cooled to room temperature to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

[0056] Example 5

[0057] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0058] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0059] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0060] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Titanium tetrachloride (TiCl4) was used as the titanium source and deionized water vapor was used as the oxygen source. Atomic layer deposition of an ultrathin TiO2 oxide layer was performed at a deposition temperature of 150℃. Each deposition cycle consisted of: TiCl4 pulse for 0.2 s, high-purity nitrogen purging for 25 s, H2O pulse for 0.2 s, and high-purity nitrogen purging for 25 s. A total of 15 cycles were performed to obtain a continuous and uniform TiO2 ultrathin modified layer with a thickness of 1.5 nm.

[0061] 4) The electrode modified by atomic layer deposition in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

[0062] Comparative Example 1

[0063] A method for preparing a hydrogen evolution catalyst, comprising the following specific steps:

[0064] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0065] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0066] Comparative Example 2

[0067] A method for preparing a hydrogen evolution catalyst, comprising the following specific steps:

[0068] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0069] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0070] 3) Immerse the NiMo / nickel foam electrode obtained in step 2) in a 0.05 mol / L aluminum nitrate aqueous solution, slowly add ammonia to adjust the pH to 8-9, let stand for 30 min, take it out, rinse with deionized water, dry at 60℃, and then place it in a muffle furnace and calcine at 300℃ in air for 1 h to obtain an alumina-coated NiMo / nickel foam electrode.

[0071] 4) The electrode obtained in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain the hydrogen evolution catalyst.

[0072] Comparative Example 3

[0073] A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, the specific steps of which are as follows:

[0074] 1) The nickel foam was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water for 15 min each. Then the cleaned nickel foam was immersed in 1 mol / L hydrochloric acid solution and ultrasonically treated for 5 min to remove the surface oxide layer and activate it. It was then rinsed with deionized water until neutral and dried in a 60℃ forced-air drying oven for 2 h to obtain pretreated nickel foam.

[0075] 2) Using the pretreated nickel foam obtained in step 1) as the working electrode, Pt sheet as the counter electrode, and Ag / AgCl (saturated KCl) as the reference electrode, a NiMo alloy catalyst layer was constructed by constant potential electrodeposition at room temperature. The electrolyte consisted of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O, and 0.10 mol / L trisodium citrate, and the pH was adjusted to 9.5 with ammonia. Constant potential deposition was carried out at a deposition potential of -1.30 V (vs Ag / AgCl) for 10 min. After deposition, the electrode was rinsed three times with deionized water and dried at 60℃ for 2 h to obtain the NiMo / nickel foam electrode.

[0076] 3) The NiMo / nickel foam electrode obtained in step 2) was transferred to an atomic layer deposition system. Trimethylaluminum (TMA) was used as the aluminum source and deionized water vapor was used as the oxygen source. An atomic layer deposition of an Al2O3 ultrathin oxide layer was performed at a deposition temperature of 120℃. Each deposition cycle consisted of: TMA pulse for 0.1 s, high-purity nitrogen purging for 20 s, H2O pulse for 0.1 s, and high-purity nitrogen purging for 20 s. A total of 50 cycles were performed to obtain a continuous and uniform Al2O3 ultrathin modified layer with a thickness of 5 nm.

[0077] 4) The electrode modified by atomic layer deposition in step 3) is placed in a tube furnace and subjected to reduction activation treatment in a 5% H2 / Ar mixed gas atmosphere. The gas flow rate is controlled at 100 mL / min, the temperature is increased to 300℃ at 5℃ / min and held for 2 h, and then naturally cooled to room temperature to obtain the hydrogen evolution catalyst.

[0078] Performance testing

[0079] The hydrogen evolution catalysts prepared in Examples 1-5 and Comparative Examples 1-3 were subjected to performance tests, and the test methods were as follows:

[0080] 1. The hydrogen evolution reaction (HER) performance of each catalyst was tested using a standard three-electrode system in a 1.0 mol / L KOH aqueous solution. The prepared electrode was used directly as the working electrode, the graphite rod as the counter electrode, and the Hg / HgO (1 mol / L KOH) electrode as the reference electrode. All tests were performed at room temperature, and data were recorded using an electrochemical workstation. Unless otherwise specified, all potentials are converted to potentials relative to the reversible hydrogen electrode.

[0081] 2. Linear sweep voltammetry (LSV) curves were recorded at a scan rate of 5 mV / s and corrected using automatic iR compensation (90% compensation level). Current densities up to 10 mA / cm² were read from the LSV curves. 2 Overpotential (η) 10The Tafel slope was obtained by fitting the corresponding LSV curve to the Tafel equation. The electrochemically active area (ECSA) was determined by the double-layer capacitance (C0). dl ) to conduct an evaluation, C dl It was calculated from cyclic voltammetry curves at different scan rates.

[0082] 3. Stability testing employed continuous cyclic voltammetry (CV) scanning, cycling 1000 times at a scan rate of 100 mV / s within the potential range of -0.1 V to -0.4 V (vs. RHE). The stability parameters (η) before and after each cycle were compared. 10 The increment (Δη) 10 ). Δη 10 The smaller the value, the better the catalyst's cycle stability.

[0083] 4. Electrochemical impedance spectroscopy (EIS) was performed under a constant potential with an overpotential of 150 mV, in a frequency range of 100 kHz to 0.01 Hz, with an AC perturbation amplitude of 5 mV. The charge transfer resistance Rct was obtained using equivalent circuit fitting. Chronocurrent stability testing was conducted at a current density of 10 mA / cm². 2 The experiment was conducted under constant potential conditions for 20 hours, and the current density was recorded as a function of time, with the current decay rate calculated. The Faraday efficiency test employed the water displacement method, under a constant current of 10 mA / cm². 2 The hydrogen evolution reaction was carried out under the specified conditions for 1 h, and the Faraday efficiency was calculated as the ratio of the actual hydrogen production to the theoretical hydrogen production calculated by Faraday's law. The results are shown in Table 1-2.

[0084] Table 1. Hydrogen evolution performance results of hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3

[0085] <![CDATA[η 10 (mV)]]> Tafel slope (mV / dec) <![CDATA[C dl (mF / cm 2 )]]> <![CDATA[Δη after 1000 CV cycles 10 (mV)]]> Example 1 105 62 48.5 +8 Example 2 118 70 38.2 +13 Example 3 128 76 44.1 +16 Example 4 112 66 46.8 +11 Example 5 135 82 40.6 +20 Comparative Example 1 218 121 35.7 +38 Comparative Example 2 186 108 28.9 +47 Comparative Example 3 295 156 12.4 +65

[0086] Table 2 Test results of hydrogen evolution catalysts in Examples 1-5 and Comparative Examples 1-3

[0087] <![CDATA[Rs(Ω·m 2 )]]> <![CDATA[Rct(Ω·m 2 )]]> 20-hour current decay rate (%) Faraday efficiency (%) Example 1 1.2 8.5 3.0 98.6 Example 2 1.5 12.3 5.8 97.8 Example 3 1.3 18.6 4.2 98.2 Example 4 1.2 10.8 3.5 98.4 Example 5 1.3 15.8 7.5 97.1 Comparative Example 1 1.4 45.2 22 95.9 Comparative Example 2 1.6 38.7 28 94.2 Comparative Example 3 1.3 128.6 35.0 91.9

[0088] From Table 1-2 and Figure 1-2 It can be seen that the Al2O3@NiMo / nickel foam catalyst prepared in Example 1 has a performance of 10 mA / cm². 2The overpotential at the current density was only 105 mV, the Tafel slope was 62 mV / dec, and the overpotential increased by only 8 mV after 1000 CV cycles. Compared with the unmodified NiMo / nickel foam in Comparative Example 1, both activity and stability were significantly improved, confirming the effectiveness of atomic layer deposition ultrathin oxide modification. Furthermore, in Examples 2-5, even after changing the substrate, adjusting the reduction temperature, or changing the oxide type, the overpotential remained at a low level of 112-135 mV, far superior to Comparative Example 1, indicating that the atomic layer deposition ultrathin oxide modification strategy of this invention has good universality.

[0089] Depend on Figure 3 It can be seen that the Rct values ​​of Examples 1 to 5 are all below 20 Ω·cm 2 Comparative examples 1-3 are all higher than 38 Ω·m 2 This demonstrates that the ultrathin oxide layer of ALD significantly promotes interfacial charge transfer; the Rct of Comparative Example 3 is as high as 128.6 Ω·m. 2 This indicates that an excessively thick oxide layer severely hinders electron tunneling. Figure 4 It can be seen that the 20-h current decay rate of Examples 1 to 5 is less than 8% and the Faraday efficiency is more than 97%, which is far better than the 22% decay rate and 95.9% Faraday efficiency of Comparative Example 1. This proves that the ALD ultrathin oxide modification layer significantly improves the long-term operating stability and hydrogen evolution selectivity of the catalyst.

[0090] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. A method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, characterized in that, Includes the following steps: 1) The conductive substrate is pretreated to obtain a pretreated conductive substrate; 2) Using the pretreated conductive substrate obtained in step 1) as the working electrode, a NiMo alloy catalyst layer is deposited on its surface by constant potential electrodeposition to obtain a NiMo / conductive substrate electrode. 3) Place the NiMo / conductive substrate electrode obtained in step 2) in an atomic layer deposition system, and perform atomic layer deposition of an ultrathin oxide layer on the surface of the NiMo alloy catalyst layer to obtain a continuous and uniform ultrathin oxide modified layer. 4) The modified electrode obtained in step 3) is subjected to reduction activation treatment in a reducing atmosphere to obtain an atomic layer deposition ultrathin oxide modified hydrogen evolution catalyst.

2. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 1), the conductive substrate is nickel foam or carbon paper.

3. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 1), the pretreatment process is as follows: the conductive substrate is placed in acetone, anhydrous ethanol and deionized water for ultrasonic cleaning for 15 min each, then the cleaned conductive substrate is immersed in 1 mol / L hydrochloric acid solution for ultrasonic treatment for 5 min, then rinsed with deionized water until neutral, and dried in a 60℃ forced-air drying oven for 2 h to obtain the pretreated conductive substrate.

4. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 2), the pretreated conductive substrate is used as the working electrode, the Pt sheet is used as the counter electrode, and Ag / AgCl is used as the reference electrode.

5. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 2), the electrolyte for the constant potential electrodeposition method consists of 0.10 mol / L NiSO4·6H2O, 0.02 mol / L Na2MoO4·2H2O and 0.10 mol / L trisodium citrate, and the pH is adjusted to 9.5 with ammonia. The deposition potential is -1.3 V relative to the Ag / AgCl electrode, and the deposition time is 10~15 min.

6. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 3), the ultrathin oxide is Al2O3 or TiO2; the atomic layer deposition cycle is 10 to 15 times.

7. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 6, characterized in that, When the ultrathin oxide is Al2O3, the atomic layer deposition uses trimethylaluminum as the aluminum source and deionized water vapor as the oxygen source, the deposition temperature is 120℃, and each deposition cycle includes: trimethylaluminum pulse for 0.1 s, nitrogen purging for 20 s, water vapor pulse for 0.1 s, and nitrogen purging for 20 s.

8. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 6, characterized in that, When the ultrathin oxide is TiO2, the atomic layer deposition uses titanium tetrachloride as the titanium source and deionized water vapor as the oxygen source, the deposition temperature is 150℃, and each deposition cycle includes: titanium tetrachloride pulse for 0.2 s, nitrogen purging for 25 s, water vapor pulse for 0.2 s, and nitrogen purging for 25 s.

9. The method for preparing an atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst according to claim 1, characterized in that, In step 4), the reduction and activation process is as follows: in a 5% H2 / Ar mixed gas atmosphere, the temperature is increased to 300~400℃ at 5℃ / min, held for 1~2 h, and then naturally cooled to room temperature.

10. An atomic layer deposition ultrathin oxide-modified hydrogen evolution catalyst, characterized in that, It is prepared by the preparation method described in claim 1.