Preparation method of gradient thickening and strengthening copper foil based on secondary electrodeposition of finished lithium battery copper foil

By forming a gradient structure of interface transition zone, fine grain reinforcement zone and surface toughening zone on the surface of finished lithium battery copper foil through staged electrodeposition, the problem of improving tensile strength and folding life after thickening copper foil in the prior art has been solved, and high-strength and high-toughness copper foil preparation has been achieved.

CN123108675APending Publication Date: 2026-11-17SHANDONG QIYE ELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611537588.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-30
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve both room temperature tensile strength exceeding 400 MPa and folding life improvement exceeding 20% ​​during the secondary thickening process of finished lithium-ion battery copper foil without introducing a polymer interlayer and adhesives, through the synergistic control of interface, grain size, and residual stress.

Method used

A secondary electrodeposition method based on finished lithium-ion battery copper foil is adopted. By controlling the current density and additive concentration in stages, a gradient structure of interface transition zone, fine grain reinforcement zone and surface toughening zone is formed on the copper foil surface, realizing direct metallurgical bonding of copper reinforcement layer.

Benefits of technology

It achieves a tensile strength of over 400 MPa for copper foil, an elongation at break of no less than 3.5%, and a folding life that is more than 20% higher. It avoids problems such as interface porosity and uneven thickness, and improves the mechanical properties of the finished copper foil.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of electrochemical technology and discloses a method for preparing gradient-thickened reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil: A finished lithium-ion battery copper foil is taken and electroplated to form a copper reinforcement layer on at least one side of the finished lithium-ion battery copper foil; after electroplating, it is washed, passivated, and dried to obtain the desired product; the electroplating is carried out in at least two stages: in the first stage, electrodeposition forms an interface transition zone; in the second stage, electrodeposition forms a fine-grained reinforcement zone. This invention discloses a gradient-thickened reinforced copper foil prepared using this method. The method of this invention uses a finished lithium-ion battery copper foil that has completed foil production, surface treatment, inspection, and roll-to-roll transport as a continuous metal substrate, and directly performs secondary electrodeposition of copper on one or both sides, increasing the total thickness by 1–8 μm. The secondary deposition layer of this invention simultaneously undertakes the functions of thickening, fine-grained reinforcement, crack passivation, and interface stress buffering, achieving a synergistic improvement in strength and folding resistance through the grain gradient along the thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing gradient-thickened reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil, belonging to the field of electrochemical technology. Background Technology

[0002] Lithium-ion batteries typically use copper foil as the carrier of the negative electrode active material and the electron current collector. The thickness, tensile strength, elongation after fracture, roughness, thickness uniformity, oxidation resistance, and surface wettability of the copper foil collectively affect the yield of coating, rolling, slitting, and winding processes, and further influence the battery's internal resistance and cycle stability. As copper foil becomes thinner, roll-to-roll tension, coating drying shrinkage, rolling, and changes in the volume of the active material are more likely to cause wrinkles, cracks, or breaks.

[0003] Existing high-strength copper foil technologies mostly start with the formulation of the raw foil electrolyte, refining the grain size through sulfur-containing brighteners, polyethers, collagen, or cellulose-based additives. This approach can improve tensile strength, but it cannot directly upgrade existing finished coils, and there are mutual constraints between strength, elongation, warpage, and surface quality. Existing folding-resistant copper foil solutions focus on controlling chloride ions and adhesive additives to achieve better fatigue ductility. Existing secondary deposition copper foil solutions mainly serve double-textured copper foil or polymer composite current collectors, and their purpose is usually to improve surface bonding or conductive layer thickness, without establishing a gradient microstructure to address the technical problem of "achieving both high tensile strength and longer folding life in finished pure copper lithium battery copper foil after thickening." If copper is uniformly plated on the surface of the finished copper foil using a conventional acidic sulfate system, only an increase in thickness and mass per unit area can usually be expected; if strong refining additives are used, an increase in strength but a decrease in plasticity is usually expected. How to achieve a room temperature tensile strength of over 400 MPa calculated based on the total cross-sectional area of ​​the final copper foil within the secondary thickness range of 1–8 μm through the coordinated control of interface, grain, and residual stress, while simultaneously increasing the lifespan by more than 20% compared to the original foil under the same bending conditions, is a technical problem that urgently needs to be solved. Summary of the Invention

[0004] To address the aforementioned prior art, this invention provides a method for directly thickening and strengthening existing finished lithium-ion battery copper foil rolls—a method for preparing gradient-thickened and strengthened copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil, the gradient-thickened and strengthened copper foil prepared using this method, and the application of this gradient-thickened and strengthened copper foil as or in the preparation of negative electrode current collectors for lithium-ion batteries. The technical solution of this invention forms an all-copper structure with direct metallurgical bonding between the base copper and the secondary electrodeposited copper without introducing a polymer interlayer or adhesive, and achieves a synergistic improvement in strength and folding resistance through grain gradient along the thickness direction.

[0005] This invention is achieved through the following technical solution:

[0006] A method for preparing gradient thickened and strengthened copper foil based on secondary electrodeposition of finished lithium battery copper foil includes the following steps: taking finished lithium battery copper foil, electroplating it, and electrodepositing a copper strengthening layer on at least one side of the finished lithium battery copper foil; after electroplating, washing, passivating and drying are performed to obtain gradient thickened and strengthened copper foil.

[0007] The electroplating is carried out in at least two stages, which can be carried out in separate tanks or in the same tank by adding additives online and changing the current density in stages or continuously.

[0008] In the first stage, the current density is 5–15 A / dm. 2 Electrodeposition forms an interfacial transition zone with a thickness of 0.2–1.2 μm; a lower SPS / hydroxyethyl cellulose concentration is used in this stage to reduce internal stress and fill activation micropits;

[0009] In the second stage, the current density is 15–45 A / dm². 2 Electrodeposition forms a fine-grained reinforcement region with a thickness of 0.7–6.8 μm; during this stage, the concentration of SPS and / or hydroxyethyl cellulose is increased to refine the average grain size to 0.05–0.40 μm.

[0010] Furthermore, the electroplating also includes a third stage, the parameters of which are: current density 8–20 A / dm³. 2 Electrodeposition forms a surface toughening zone with a thickness of 0.1–0.8 μm.

[0011] Furthermore, depending on the downstream coating requirements, corona or plasma cleaning can be performed after electroplating to ensure that the surface wetting tension is not less than 38 mN / m.

[0012] Furthermore, during the electroplating process, the theoretical thickness of the copper reinforcement layer can be calculated according to Faraday's law δ=ηJtM / (nFρ), and corrected using the results of online surface density or X-ray thickness measurement in a closed loop, where η is the current efficiency, J is the current density, t is the energizing time, M is the molar mass of copper, n is the number of electrons transferred, F is the Faraday constant, and ρ is the copper density.

[0013] Furthermore, copper reinforcement layers are electrodeposited on both sides of the finished lithium battery copper foil, with the thickness difference between the two sides not exceeding 10% of the total thickness of the copper reinforcement layers; electroplating can be performed simultaneously or sequentially symmetrically.

[0014] Furthermore, the electroplating solution used in the electroplating includes a base plating solution, which is an acidic sulfate system, and the electroplating temperature is 35–55°C. The composition of the base plating solution is: 180–260 g / L copper sulfate pentahydrate, 40–100 g / L sulfuric acid, and chloride ions (added in the form of HCl or NaCl, and in the form of Cl). -(Calculated concentration) 15-60 mg / L, with the remainder being water.

[0015] Furthermore, the electroplating solution contains any two or more of the following components: sodium polydisulfide dipropane sulfonate (SPS), i.e., disodium bis(3-sulfopropyl) disulfide, 0.2–10 mg / L; polyethylene glycol (PEG, weight average molecular weight 6000–10000), 20–120 mg / L; hydroxyethyl cellulose, 0.5–15 mg / L; and gelatin, 0.5–8 mg / L.

[0016] Furthermore, before electroplating, the finished lithium-ion battery copper foil undergoes pretreatment, which may be one or more of the following: alkaline degreasing, deionized water washing, low-damage micro-etching, acid pickling activation, and deionized water washing. Preferably, the pretreatment methods are as follows: alkaline degreasing, deionized water washing, low-damage micro-etching, acid pickling activation, and deionized water washing.

[0017] Furthermore, the specific operation method of alkaline washing and degreasing is as follows: the finished lithium battery copper foil is placed in an alkaline washing solution and immersed at 35-50°C for 15-45 seconds; the alkaline washing solution is composed of sodium hydroxide, sodium carbonate, nonionic surfactant and water, wherein the concentration of sodium hydroxide is 15-30 g / L, the concentration of sodium carbonate is 10-25 g / L, and the concentration of nonionic surfactant is 0.2-1.0 g / L; the nonionic surfactant is selected from fatty alcohol polyoxyethylene ether (AEO-9).

[0018] Furthermore, the specific operation method of the low-damage micro-etching is as follows: the finished lithium battery copper foil is placed in the micro-etching solution and immersed at 20-35°C for 5-20 seconds; then activated in a 50-120 g / L sulfuric acid solution for 5-30 seconds; the micro-etching solution is composed of sulfuric acid, hydrogen peroxide and water, wherein the concentration of sulfuric acid is 50-100 g / L and the concentration of hydrogen peroxide is 5-15 g / L.

[0019] Furthermore, the specific operation method of passivation is as follows: placing the electroplated product in a passivation solution and treating it at 20-40℃ for 5-30 seconds; rinsing with deionized water; the passivation solution is composed of benzotriazole, aminosilane and water, with the concentration of benzotriazole being 0.1-1.0 g / L, the concentration of aminosilane being 0.05-0.5 g / L, and the pH being 5.0-8.0.

[0020] Furthermore, the drying temperature is 60–100°C.

[0021] A gradient-thickened reinforced copper foil prepared by the above preparation method is composed of a lithium-ion battery copper foil substrate and a copper reinforcement layer directly electrodeposited on at least one side of the lithium-ion battery copper foil substrate, wherein the thickness of the lithium-ion battery copper foil substrate is 4 to 12 μm and the total thickness of the copper reinforcement layer is 1 to 8 μm.

[0022] The copper reinforcement layer has at least an interface transition region and a fine grain reinforcement region along the direction away from the substrate. The average grain size of the interface transition region is 0.30 to 1.50 μm, the average grain size of the fine grain reinforcement region is 0.05 to 0.40 μm, and the ratio of the average grain size of the interface transition region to the average grain size of the fine grain reinforcement region is not less than 1.5.

[0023] The thickness of the interface transition region accounts for 5% to 40% of the total thickness of the copper reinforcement layer, and the thickness of the fine grain reinforcement region accounts for 60% to 95% of the total thickness of the copper reinforcement layer.

[0024] Furthermore, the copper strengthening layer also has a surface toughening region. Along the direction away from the substrate, the surface toughening region is outside the fine grain strengthening region, and the average grain size of the surface toughening region is 0.25 to 0.80 μm. The thickness of the interface transition region accounts for 5% to 25% of the total thickness of the copper strengthening layer, the thickness of the fine grain strengthening region accounts for 60% to 90% of the total thickness of the copper strengthening layer, and the thickness of the surface toughening region accounts for 5% to 20% of the total thickness of the copper strengthening layer.

[0025] The application of the gradient thickened reinforced copper foil in the preparation of lithium-ion batteries, and its application in the preparation of negative electrode current collectors for lithium-ion batteries.

[0026] The gradient-thickened reinforced copper foil of this invention does not have a resin, adhesive, or polymer support layer between the interface transition zone and the substrate, and no continuous interface pores are observed in cross-section. Its room temperature tensile strength is not less than 400 MPa, its elongation after fracture is not less than 3.5%, and its bending life is at least 20% higher than that of the same batch of unthickened base foil.

[0027] This invention does not generate a single sheet of copper foil of the target thickness through a one-time electrolysis process on a cathode roller. Instead, it uses a finished lithium-ion battery copper foil that has already undergone foil production, surface treatment, inspection, and roll-to-roll transport as a continuous metal substrate. After removing oil and the original surface passivation film, copper is directly electrodeposited on one or both sides of the foil, increasing the total thickness by 1–8 μm. The secondary deposition layer simultaneously serves to thicken the foil, refine the grains, passivate cracks, and buffer interfacial stress.

[0028] The present invention provides a method for preparing gradient-thickened and strengthened copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil. Applicable scenarios include: converting existing 4-10 μm thin finished products into thicker and higher-strength specifications required by specific customers; improving dimensional stability and resistance to strip breakage during high-silicon anodes, thick-coated electrodes, fast charging, and wide-roll-to-roll processing; and carrying out high-value-added remanufacturing of finished copper foils that do not meet the high-strength grade mechanical properties but have qualified surface and purity.

[0029] The present invention provides a method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil, which solves the following technical problems and achieves the following technical effects:

[0030] (1) Conventional thickening methods only increase the cross-sectional area and cannot guarantee that the tensile strength calculated based on the "final total thickness" will reach more than 400 MPa. This invention adopts a gradient thickening method to make the final tensile strength reach more than 400 MPa.

[0031] (2) Although uniform nanocrystalline coatings can improve strength, they often result in limited improvement in folding life due to decreased elongation and increased internal stress. This invention uses gradient deposition to form a copper reinforcement layer consisting of an interface transition region, a fine grain reinforcement region, and a surface toughening region, which significantly improves folding life.

[0032] (3) The finished copper foil already has a passivation layer and organic residues. Direct secondary electroplating is prone to problems such as interface porosity, localized missed plating, peeling, and delamination after heat treatment. The present invention performs pretreatment before electroplating, thus avoiding problems such as interface porosity, localized missed plating, peeling, and delamination after heat treatment.

[0033] (4) Single-sided rapid deposition is prone to plate warping and uneven lateral thickness, which affects coating and rolling. The present invention uses double-sided electroplating, which avoids problems such as plate warping and uneven lateral thickness.

[0034] The various terms and phrases used in this invention have their general meanings known to those skilled in the art. Detailed Implementation

[0035] The present invention will be further described below with reference to embodiments. However, the scope of the present invention is not limited to the following embodiments. Those skilled in the art will understand that various changes and modifications can be made to the present invention without departing from the spirit and scope thereof.

[0036] Unless otherwise specified, the instruments, reagents, and materials used in the following embodiments are all conventional instruments, reagents, and materials already available in the prior art and can be obtained through legitimate commercial channels. Unless otherwise specified, the experimental methods and detection methods used in the following embodiments are all conventional experimental methods and detection methods already available in the prior art. Example 1

[0037] Preparation of gradient thickening and strengthening copper foil based on secondary electrodeposition of finished lithium battery copper foil;

[0038] Experimental materials: The same roll of 6.0 μm double-sided finished lithium-ion battery electrolytic copper foil was selected as the lithium-ion battery copper foil substrate. The room temperature tensile strength of the substrate was 360±7 MPa, the elongation after fracture was 5.2%±0.2%, and the bending life was 1290±60 times.

[0039] Equipment: The main equipment used in the preparation process includes roll-to-roll alkaline washing / micro-etching lines, continuous electroplating tank for acidic copper sulfate, programmable rectifier power supply, online X-ray thickness gauge, universal material testing machine, MIT-type bending fatigue testing machine, four-probe resistivity tester, cross-sectional SEM / EBSD and FIB-TEM.

[0040] The steps are as follows (each step is completed continuously on the roll-to-roll production line):

[0041] (1) Pre-processing:

[0042] Before electroplating, the finished lithium battery copper foil is pretreated in the following order: alkaline washing to remove oil, deionized water washing, low-damage micro-etching, acid washing to activate, and deionized water washing.

[0043] The specific operation method for alkaline washing and degreasing is as follows: the finished lithium battery copper foil is placed in an alkaline washing solution and immersed at 45°C for 30 seconds. The alkaline washing solution is composed of sodium hydroxide, sodium carbonate, fatty alcohol polyoxyethylene ether (AEO-9), and water, wherein the concentration of sodium hydroxide is 20 g / L, the concentration of sodium carbonate is 15 g / L, and the concentration of AEO-9 is 0.5 g / L.

[0044] The specific operation method of the low-damage micro-etching is as follows: the finished lithium battery copper foil is placed in the micro-etching solution and immersed at 30°C for 15 seconds to control the thickness removed on one side to be 0.02-0.15 μm; then activated in an 80 g / L sulfuric acid solution for 20 seconds; the surface is kept moist before entering the electroplating tank to avoid re-oxidation. The micro-etching solution is composed of sulfuric acid, hydrogen peroxide, and water, wherein the concentration of sulfuric acid is 80 g / L and the concentration of hydrogen peroxide is 10 g / L.

[0045] (2) Electroplating thickening and strengthening: a double-layer gradient structure with a thickness of 1.0 μm;

[0046] After the base foil pretreatment is completed, electroplating is performed to form a copper reinforcement layer on both sides of the base foil by electrodeposition.

[0047] The electroplating solution used includes a base plating solution, which is an acidic sulfate system. Its components are: 220 g / L copper sulfate pentahydrate, 70 g / L sulfuric acid, and chloride ions (added as NaCl, and Cl-). -(Calculated) 30 mg / L, balance is water; electroplating temperature 45℃.

[0048] The electroplating solution may contain any two or more of the following components: sodium polydisulfide dipropane sulfonate (SPS), i.e., disodium salt of bis(3-sulfopropyl) disulfide, 0.2–10 mg / L; polyethylene glycol (PEG, weight average molecular weight 6000–10000), 20–120 mg / L; hydroxyethyl cellulose, 0.5–15 mg / L; gelatin, 0.5–8 mg / L;

[0049] Electroplating is carried out in two stages, each in the same tank by adding additives online and continuously changing the current density:

[0050] In the first stage, the electroplating solution contained the following components at the following concentrations: SPS, 0.5 mg / L; PEG (weight average molecular weight 8000), 50 mg / L; hydroxyethyl cellulose, 1.0 mg / L; and a current density of 8 A / dm³. 2 Symmetrical electroplating on both sides, electrodeposition to form an interface transition zone with a total thickness of 0.25 μm on both sides;

[0051] In the second stage, the concentrations of each component in the electroplating solution were adjusted as follows: SPS, 4.0 mg / L; PEG (weight-average molecular weight 8000), 60 mg / L; hydroxyethyl cellulose, 8.0 mg / L; current density 28 A / dm³. 2 Electrodeposition forms a fine-grained reinforcement region with a total thickness of 0.75 μm on both sides.

[0052] (3) Finished product post-processing:

[0053] After electroplating, the product is washed with water, passivated, and dried (at 80°C) to obtain a gradient-thickened reinforced copper foil with a total thickness of 7.0 μm. The specific passivation procedure is as follows: the electroplated product is placed in a passivation solution and treated at 30°C for 20 seconds; then washed with deionized water. The passivation solution is composed of benzotriazole, aminosilane, and water, with a benzotriazole concentration of 0.5 g / L, an aminosilane concentration of 0.3 g / L, and a pH of 7.0. Example 2

[0054] The difference from Example 1 is that the electroplating is a three-layer gradient structure with a thickness of 3.0 μm, and there is a third stage after the second stage.

[0055] In the first stage, the current density was 8 A / dm. 2 Symmetrical electroplating on both sides, electrodeposition to form an interface transition zone with a total thickness of 0.60 μm on both sides;

[0056] In the second stage, the concentrations of each component in the electroplating solution were adjusted as follows: SPS, 5.0 mg / L; PEG (weight-average molecular weight 8000), 60 mg / L; hydroxyethyl cellulose, 9.0 mg / L; current density 32 A / dm³. 2 Electrodeposition forms a fine-grained reinforcement region with a total thickness of 2.00 μm on both sides;

[0057] In the third stage, the concentrations of each component in the electroplating solution were adjusted as follows: SPS was reduced to 1.0 mg / L, and gelatin 2.0 mg / L was added; the current density was 14 A / dm³. 2 Electrodeposition forms a surface toughening region with a thickness of 0.40 μm. The thickness difference between the two sides is 0.12 μm, and the total thickness is 9.0 μm. Example 3

[0058] The difference from Example 2 is that the total thicknesses of the interface transition region, the grain refinement reinforcement region, and the surface toughening region are 0.80 μm, 3.60 μm, and 0.60 μm, respectively; and the current densities of the three stages are 10 A / dm³, respectively. 2 35 A / dm 2 and 15 A / dm 2 The final thickness is 11.0 μm. Example 4

[0059] The difference from Example 2 is that the total thicknesses of the interface transition region, the grain refinement reinforcement region, and the surface toughening region are 1.20 μm, 6.00 μm, and 0.80 μm, respectively; and the current densities of the three stages are 12 A / dm³, respectively. 2 38 A / dm 2 and 16 A / dm 2 The final thickness is 14.0 μm.

[0060] Comparative Example 1: 6.0 μm base foil from the same batch that was not subjected to thickening treatment.

[0061] Comparative Example 2: Conventional uniform thickness increase of 3.0 μm: 12 A / dm throughout. 2 Under low additive conditions, coarse crystals of about 1.1 μm are formed.

[0062] Comparative Example 3: Uniform fine grain thickness increased by 3.0 μm: 32 A / dm throughout. 2 A high concentration of SPS / HEC was used to form a uniform fine-grained layer of about 0.2 μm, without setting an interface transition zone or a surface toughening zone.

[0063] Experiment: Performance testing and comparison;

[0064] The products of Examples 1, 2, and 3 and Comparative Examples 1, 2, and 3 were subjected to performance testing and compared.

[0065] The test results of mechanical properties and flexural life are shown in Table 1.

[0066] Table 1:

[0067] ;

[0068] Interpretation of results: Under the same conditions of 3.0 μm thickness increase and final thickness of 9.0 μm, the ordinary coarse-grained coating in Comparative Example 2 could not achieve a final tensile strength of 400 MPa; while the uniform fine-grained layer in Comparative Example 3 achieved a tensile strength of 450 MPa, the elongation decreased to 3.2%, and the bending life was only improved by 11.5%. Example 2 had a tensile strength similar to Comparative Example 3, but maintained an elongation of 4.7% and improved bending life by 32.4%. This indicates that the improved bending resistance is not solely due to increased thickness or fine-grained reinforcement, but rather a combination of the low-stress interface region, the fine-grained load-bearing region, and the surface toughening region.

[0069] The detection results of microstructure, interface, and plate shape are shown in Table 2. As can be seen from Table 2, the three grain sizes in Example 2 exhibit a gradient distribution of "coarse-fine-coarse". The uniform fine-grained layer of Comparative Example 3 has similar strength, but cracks easily penetrate from the outer surface when bent.

[0070] Table 2:

[0071] ;

[0072] The above embodiments are provided to those skilled in the art to fully disclose and describe how the claimed implementations can be carried out and used, and are not intended to limit the scope of the disclosure herein. Modifications that will be obvious to those skilled in the art will be within the scope of the appended claims.

Claims

1. A method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil, characterized in that, The steps are as follows: Take the finished lithium battery copper foil and electroplate it to form a copper reinforcement layer on at least one side of the finished lithium battery copper foil; after electroplating, wash, passivate and dry it to obtain the gradient thickened reinforced copper foil. The electroplating is performed in at least two stages: In the first stage, the current density is 5–15 A / dm. 2 Electrodeposition forms an interfacial transition region with a thickness of 0.2–1.2 μm; In the second stage, the current density is 15–45 A / dm². 2 Electrodeposition forms a fine-grained reinforcement region with a thickness of 0.7–6.8 μm.

2. The method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil according to claim 1, characterized in that: The electroplating process also includes a third stage, with parameters for the third stage being: current density of 8–20 A / dm³. 2 Electrodeposition forms a surface toughening zone with a thickness of 0.1–0.8 μm.

3. The method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil according to claim 1 or 2, characterized in that: Copper reinforcement layers are electrodeposited on both sides of the finished lithium battery copper foil, and the thickness difference between the two sides of the copper reinforcement layers is no more than 10% of the total thickness of the copper reinforcement layers.

4. The method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil according to claim 1 or 2, characterized in that: The electroplating solution used in the electroplating includes a base plating solution, which is an acidic sulfate system. The composition of the base plating solution is: copper sulfate pentahydrate 180-260 g / L, sulfuric acid 40-100 g / L, chloride ions 15-60 mg / L, and the balance is water.

5. The method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil according to claim 4, characterized in that, The electroplating solution contains any two or more of the following components: sodium polydithiopropane sulfonate, 0.2–10 mg / L; polyethylene glycol, 20–120 mg / L; hydroxyethyl cellulose, 0.5–15 mg / L; and gelatin, 0.5–8 mg / L.

6. The method for preparing gradient-thickness reinforced copper foil based on secondary electrodeposition of finished lithium-ion battery copper foil according to claim 1 or 2, characterized in that: Before electroplating, the finished lithium battery copper foil is pretreated. The pretreatment methods are one or more of the following: alkaline washing to remove oil, deionized water washing, low-damage micro-etching, acid washing to activate, and deionized water washing.

7. A gradient-thickened reinforced copper foil prepared by the preparation method according to any one of claims 1 to 6, characterized in that: It consists of a lithium-ion battery copper foil substrate and a copper reinforcement layer directly electrodeposited on at least one side of the lithium-ion battery copper foil substrate. The thickness of the lithium-ion battery copper foil substrate is 4 to 12 μm, and the total thickness of the copper reinforcement layer is 1 to 8 μm. The copper reinforcement layer has at least an interface transition region and a fine grain reinforcement region along the direction away from the substrate. The average grain size of the interface transition region is 0.30 to 1.50 μm, the average grain size of the fine grain reinforcement region is 0.05 to 0.40 μm, and the ratio of the average grain size of the interface transition region to the average grain size of the fine grain reinforcement region is not less than 1.

5. The thickness of the interface transition region accounts for 5% to 40% of the total thickness of the copper reinforcement layer, and the thickness of the fine grain reinforcement region accounts for 60% to 95% of the total thickness of the copper reinforcement layer.

8. The gradient-thickness reinforced copper foil according to claim 7, characterized in that: The copper strengthening layer also has a surface toughening region. Along the direction away from the substrate, the surface toughening region is outside the fine grain strengthening region, and the average grain size of the surface toughening region is 0.25 to 0.80 μm. The thickness of the interface transition region accounts for 5% to 25% of the total thickness of the copper strengthening layer, the thickness of the fine grain strengthening region accounts for 60% to 90% of the total thickness of the copper strengthening layer, and the thickness of the surface toughening region accounts for 5% to 20% of the total thickness of the copper strengthening layer.

9. The gradient-thickness reinforced copper foil according to claim 8, characterized in that: The thickness of the lithium-ion battery copper foil substrate is 6.0 micrometers; The total thicknesses of the interface transition region, the grain refinement reinforcement region, and the surface toughening region are 0.60 μm, 2.00 μm, and 0.40 μm, respectively. The total thickness is 9.0 μm; Alternatively: the total thicknesses of the interface transition zone, the fine-grained strengthening zone, and the surface toughening zone are 0.80 μm, 3.60 μm, and 0.60 μm, respectively; the total thickness is 11.0 μm. Alternatively: The total thicknesses of the interface transition zone, the fine grain strengthening zone, and the surface toughening zone are 1.20 μm, 6.00 μm, and 0.80 μm, respectively; the total thickness is 14.0 μm.

10. The application of the gradient thickening reinforced copper foil according to claim 7, 8 or 9 in the preparation of lithium-ion batteries, or in the preparation of negative electrode current collectors for lithium-ion batteries.