A method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating

By electrodepositing a Mn-Co-Cu-Ce quaternary spinel coating on the surface of the metal connector and performing gradient heat treatment, the problems of high-temperature oxidation and Cr volatilization of the metal connector are solved, achieving the effects of low impedance, oxidation resistance and low pollution, meeting the high cleanliness requirements of semiconductor manufacturing.

CN123108682APending Publication Date: 2026-11-17SHANGHAI HENGXIN METAL PROD MFG CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611182843.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-05
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In the semiconductor chip manufacturing process, metal connectors are easily oxidized in high-temperature oxidizing atmospheres, which leads to increased interfacial contact resistance, Cr volatilization and contamination of the chamber, affecting chip yield. Existing technologies are difficult to effectively suppress oxidation and Cr diffusion.

Method used

Mn, Co, Cu and Ce layers are sequentially deposited on the surface of the metal connector by electrodeposition to form a Mn-Co-Cu-Ce quaternary spinel coating, and then subjected to gradient heat treatment in an oxidizing atmosphere to form a dense coating.

Benefits of technology

It significantly reduces interface resistance, improves oxidation resistance, prevents Cr volatilization, meets the cleanliness requirements of semiconductor manufacturing, shortens the production cycle, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108682A_ABST
    Figure CN123108682A_ABST
Patent Text Reader

Abstract

This application discloses a method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating. The method includes depositing an Mn layer, a Co layer, a Cu layer and a Ce layer sequentially on the surface of a substrate defined by a semiconductor metal connector by electrodeposition; and forming the Mn-Co-Cu-Ce quaternary spinel coating on the substrate surface by gradient heating in an oxygen-containing atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of metal coating materials, and more particularly to a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating and its preparation method. Background Technology

[0002] Chemical vapor deposition (CVD) is one of the core processes in semiconductor chip manufacturing, widely used for depositing thin film materials such as dielectric layers, semiconductor layers, conductive layers, and barrier layers. As integrated circuit feature sizes continue to shrink and chip integration density continues to increase, CVD processes place increasingly stringent demands on the cleanliness, temperature uniformity, and process stability of the chamber environment. In the CVD reactor, metal connectors perform multiple functions, including structural support, circuit connection, and heat conduction, and must operate stably for extended periods in high-temperature environments (600–900°C) and alternating oxidizing / reducing atmospheres.

[0003] However, metal connectors face severe surface degradation problems during long-term service. Firstly, the metal substrate, especially chromium-containing ferritic stainless steels such as Crofer 22 APU and SUS 430, is prone to oxidation in high-temperature oxidizing atmospheres, forming an oxide layer primarily composed of Cr2O3. With prolonged oxidation, the Cr2O3 layer thickens, and its low conductivity significantly increases the interfacial contact resistance of the connector, affecting the stable transmission of electrical signals in the reactor and the precise control of the temperature field. More seriously, under high temperatures and in the presence of trace amounts of water vapor, Cr2O3 further transforms into volatile chromium compounds. These gaseous chromium species escape from the connector surface, diffuse into the reaction chamber, and may deposit on the wafer surface or adhere to the chamber walls. Chromium contamination severely affects the quality of the deposited film, leading to particle defects and significantly reducing chip yield. Therefore, effectively suppressing high-temperature oxidation of metal connectors in CVD reactors, reducing interfacial resistance, and preventing chromium volatilization and contamination have become critical technical issues urgently needing to be addressed in the field of high-end semiconductor equipment manufacturing.

[0004] Chinese patent application CN201710426053.3 discloses a method for preparing a spinel coating by plasma spraying a Cu-Mn-Co alloy coating onto a stainless steel substrate and then pre-sintering it. The specific technical solution includes: preparing Cu-Mn-Co alloy powder through mechanical alloying; forming an alloy coating on the substrate surface using atmospheric plasma spraying; and then pre-sintering it in air at 750-800℃ for 10-20 hours to transform the alloy coating into a Cu-containing spinel oxide coating in situ. This patent claims to improve high-temperature oxidation resistance and electrical conductivity. However, the pre-sintering time in this patent is excessive, resulting in high energy consumption and a narrow process window. Furthermore, it does not address the problem that Cu doping exacerbates Cr volatilization.

[0005] Chinese patent application CN121718876A discloses a gradient composite manganese-cobalt spinel interconnect coating and its preparation method. The technical solution involves forming an FeCr alloy nano-oxide layer on a substrate surface using a plasma flow as the inner layer, followed by atmospheric plasma spraying to prepare a manganese-cobalt spinel composite coating on the outer layer. This solution aims to improve oxidation resistance and reduce surface resistivity by utilizing the inner nano-oxide layer to block chromium diffusion and the outer spinel layer to provide a conductive path. However, the coating obtained by the plasma spraying process in this patent has inherently high porosity, making it difficult to completely block the diffusion of oxygen and chromium. Furthermore, the improvement in conductivity is limited, and the method does not optimize for the specific surface smoothness requirements of the CVD reactor. Summary of the Invention

[0006] To address the aforementioned technical problems, this application discloses a method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating, characterized in that the preparation method includes:

[0007] Mn, Co, Cu, and Ce layers are deposited sequentially on the substrate surface defined by the semiconductor metal interconnect using an electrodeposition method, wherein the thickness of the Mn layer is 0.5–1.0 μm, the thickness of the Co layer is 10–20 μm, the thickness of the Cu layer is 0.5–1.0 μm, and the thickness of the Ce layer is 0.1–0.2 μm.

[0008] Then, in an oxygen-containing atmosphere, a Mn-Co-Cu-Ce quaternary spinel coating is formed on the substrate surface through gradient heating.

[0009] According to one embodiment of this application, the Mn electrolyte comprises MnSO4·H2O 0.2~0.4 mol / L, H3BO3 0.1~0.3 mol / L, sodium citrate 0.10~0.20 mol / L, saccharin 0.5~1.5 g / L, sodium dodecyl sulfate 0.05~0.10 g / L, and Na2SO4 0.4~0.6 mol / L.

[0010] According to one embodiment of this application, when depositing an Mn layer on the substrate, at least one of the following conditions is satisfied:

[0011] The current density is controlled at 50~100 mA / cm²;

[0012] pH value is 3.0~4.0;

[0013] The concentration of sodium citrate is 0.10~0.20 mol / L;

[0014] Deposit at room temperature for 5-20 minutes.

[0015] According to one embodiment of this application, the composition of the Co electrolyte is: CoSO4·7H2O 0.1~0.3 mol / L, H3BO3 0.1~0.3 mol / L, Na2SO4 0.4~0.6 mol / L, saccharin 0.5~1.5 g / L, and sodium dodecyl sulfate 0.05~0.10 g / L.

[0016] According to one embodiment of this application, at least one of the following conditions is satisfied during the deposition and formation of the Co layer:

[0017] The current density is controlled at 10~20 mA / cm²;

[0018] pH value is 3.0~4.0;

[0019] Deposit at room temperature for 2-10 minutes.

[0020] According to one embodiment of this application, a Ni transition layer with a thickness of 0.5 to 5 μm is electroplated between the Mn layer and the Co layer.

[0021] According to one embodiment of this application, at least one of the following conditions is satisfied during the deposition of a Ni layer:

[0022] The current density is controlled to be 10~30 mA / cm²;

[0023] pH value is 3.0~4.0;

[0024] Deposit at room temperature for 0.5 to 2 minutes.

[0025] According to one embodiment of this application, when depositing to form a Cu-Ce composite layer, the substrate after depositing the Co layer is placed in a Cu electrolyte containing CeO2 nanoparticles. The current density is controlled at 10~20 mA / cm², the pH value is 7.5~9.0, the sodium citrate concentration is 0.30~0.50 mol / L, and the CeO2 nanoparticle addition amount is 0.5~3.0 g / L. The deposition is carried out at room temperature for 2~10 minutes to form a Cu-Ce composite layer on the surface of the Co layer.

[0026] According to one embodiment of this application, the gradient heat treatment process includes:

[0027] First, heat to 350-450℃ at a heating rate of 10-20℃ / min and hold for 0.5-1.5 hours.

[0028] Then raise the temperature to 550~650℃ and hold for 0.5~1.5 hours;

[0029] Finally, the temperature is raised to 750~850℃ and held for 4~10 hours, then cooled to room temperature in the furnace to obtain a dense Mn-Co-Cu-Ce quaternary spinel coating on the surface of the metal connector.

[0030] According to another aspect of this application, this application also provides a spinel coating or semiconductor metal connector prepared based on the preparation method described above.

[0031] The present invention has the following advantages over the prior art:

[0032] (1) Significantly improved electrical conductivity: This invention forms Mn³⁺ / Mn in Mn-Co spinel through synergistic doping of Cu and Ce. 4 ⁺、Co²⁺ / Co³⁺、Cu⁺ / Cu²⁺、Ce³⁺ / Ce 4 The coexisting mixed valence states provide abundant electronic transition sites for small polaron hopping, forming a stable electron transport channel. Experimental results show that the Mn-Co-Cu-Ce quaternary spinel coating prepared in this invention has an area resistivity (ASR) as low as 0.17 Ω·cm² at 750℃ and an activation energy of approximately 95 kJ·mol⁻¹, significantly lower than that of traditional Mn-Co coatings, effectively ensuring stable transmission of electrical signals in the CVD reactor.

[0033] (2) Excellent antioxidant and anti-Cr volatilization capabilities: This invention introduces Ce element and utilizes Ce³⁺ / Ce 4 The reversible mutation of ⁺ modulates the oxygen vacancy concentration in the coating, inhibiting the inward diffusion of oxygen anions and the outward diffusion of Cr from the matrix. Simultaneously, the dense spinel structure itself physically blocks Cr volatilization. Experimental results show that after 1000 hours of oxidation at 800℃, the oxidation weight gain per unit area of ​​the coating is only 1.78 mg·cm⁻², approximately 52.3% lower than the undoped sample, while maintaining a coating coverage of over 97%. Cr is strictly confined within the matrix, significantly reducing the risk of chromium contamination in the CVD chamber.

[0034] (3) High interfacial bonding strength: This invention innovatively introduces a Ni metal transition layer between the Mn layer and the Co layer. Through the lattice matching and stress relief effect of the Ni layer, the thermal compatibility between the spinel coating and the ferritic stainless steel substrate is effectively improved. After long-term high-temperature service, the coating and the substrate interface are tightly bonded, and no obvious cracking or peeling occurs. It can resist the thermal stress impact caused by frequent thermal cycling in the CVD reactor.

[0035] (4) Controllable process and low energy consumption: The present invention adopts layered electrodeposition technology, and the composition and thickness of each metal layer can be independently controlled, with a wide process window. At the same time, the gradient heat treatment process can achieve efficient transformation and densification of spinel phase at 800℃ for 6 hours. Compared with the existing technology, which requires 10 to 20 hours of pre-sintering after plasma spraying, the energy consumption is significantly reduced and the production cycle is shortened.

[0036] (5) Meets the special requirements of semiconductor CVD: The coating surface of the present invention is flat with low particle adhesion, and the coating has good stability in a reducing atmosphere, which can meet the stringent requirements of semiconductor manufacturing for chamber cleanliness and metal contamination control at the ppt level. Attached Figure Description

[0037] Figure 1 The surface SEM morphology of Mn-Co-Cu coatings with different CeO2 concentrations after 6 h of heat treatment is shown: (a) 0.3 g / L; (b) 0.9 g / L; (c) 1.8 g / L; (d) 3.0 g / L.

[0038] Figure 2 The SEM-EDS element distribution diagram of the 1.8 g / L CeO2-doped Mn-Co-Cu coating after 6 h of heat treatment is shown.

[0039] Figure 3 The unit area oxidation weight gain curves and fitting results for samples with different CeO2 addition amounts are shown.

[0040] Figure 4 ASR variation with temperature and its Arrhenius fitting curve for different coating systems: (a) ASR-Temperature curve; (b) Arrhenius fitting curve. Detailed Implementation

[0041] The following description is intended to disclose the present invention and enable those skilled in the art to implement it. The preferred embodiments described below are merely examples, and other obvious variations will occur to those skilled in the art. The basic principles of the invention defined in the following description can be applied to other embodiments, modifications, improvements, equivalents, and other technical solutions that do not depart from the spirit and scope of the invention.

[0042] refer to Figures 1 to 4 According to a preferred embodiment of the present invention, a method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating includes:

[0043] S101, depositing a Mn plating layer on the substrate surface defined by the metal connector to be plated.

[0044] Preferably, a Mn coating is deposited on the substrate surface using a direct current electrodeposition method.

[0045] Preferably, the metal connector is made of Crofer 22 APU ferritic stainless steel as the base material.

[0046] Preferably, the electrolyte used for depositing the Mn coating on the substrate surface includes MnSO4·H2O 0.2~0.4 mol / L, H3BO3 0.1~0.3 mol / L, sodium citrate 0.10~0.20 mol / L, saccharin 0.5~1.5 g / L, sodium dodecyl sulfate 0.05~0.10 g / L, and Na2SO4 0.4~0.6 mol / L. A platinum electrode is used as the anode, and the substrate as the cathode.

[0047] Also preferably, when depositing the Mn coating on the substrate surface, the current density is controlled to be 50~100 mA / cm²; the pH value is 3.0~4.0; the sodium citrate concentration is 0.10~0.20 mol / L; and the deposition time is 5~20 minutes at room temperature.

[0048] In a more preferred embodiment, prior to depositing the Mn coating on the substrate surface, the method for preparing the low-resistivity Mn-Co-Cu-Ce quaternary spinel coating includes:

[0049] S201, perform surface pretreatment on the substrate. As an example, the method for performing surface pretreatment on the substrate includes:

[0050] The surface is sanded step by step with 800#, 1000#, and 1200# SiC sandpaper until it is smooth and free of scratches. Then, it is mechanically polished with polishing liquid until it achieves a mirror finish.

[0051] The polished sample was placed in acetone and then in ethanol, and ultrasonically cleaned for 5 minutes each time to remove surface oil and organic residues. After cleaning, it was rinsed with deionized water and dried.

[0052] More preferably, the method for surface pretreatment of the substrate further includes:

[0053] Before electrodeposition begins, the sample is immersed in an activation solution for 30 seconds to remove the surface passivation film, then rinsed with deionized water and dried. Activation with the activation solution helps to improve the density, uniformity, and coverage of the Mn layer during subsequent electrodeposition.

[0054] In a preferred embodiment, the activation solution is a 15 vol.% HCl solution.

[0055] The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating includes:

[0056] S102, and then a Ni transition layer is formed on the surface of the Mn layer.

[0057] The electrolyte for electrodepositing the Ni layer comprises 0.1 mol / L NiSO4·6H2O, 0.1 mol / L Na2SO4, and 0.2 mol / L H3BO3, with the pH adjusted to 3.5. The current density is controlled at 10~30 mA / cm². 2 With a pH value of 3.0~4.0, a Ni transition layer is formed on the surface of the Mn layer by deposition at room temperature for 0.5~2 minutes.

[0058] The method for preparing the low-resistivity Mn-Co-Cu-Ce quaternary spinel coating includes:

[0059] S103, continue to deposit a Co coating on the surface of the Ni transition layer;

[0060] The electrolyte comprises 0.1–0.3 mol / L CoSO4·7H2O, 0.1–0.3 mol / L H3BO3, 0.4–0.6 mol / L Na2SO4, 0.5–1.5 g / L saccharin, and 0.05–0.10 g / L sodium dodecyl sulfate. The electrolyte is controlled at 10–15 mA / cm², pH 3.0–3.5, and deposition is performed at room temperature for 2–10 minutes to form a high-purity, high-coverage Co layer on the surface of the Ni transition layer.

[0061] Furthermore, the method for preparing the low-resistivity Mn-Co-Cu-Ce quaternary spinel coating includes:

[0062] S104: The substrate after depositing the Co layer is placed in a Cu electrolyte containing CeO2 nanoparticles. The current density is controlled at 10~20 mA / cm², the pH value is 7.5~9.0, the sodium citrate concentration is 0.30~0.50 mol / L, and the CeO2 nanoparticle addition amount is 0.5~3.0 g / L. The deposition is carried out at room temperature for 2~10 minutes to form a Cu-Ce composite layer on the surface of the Co layer.

[0063] Methods for placing the metal connector after depositing the Cu-Ce composite layer in a heat treatment furnace for gradient heat treatment include:

[0064] First, heat to 350-450℃ at a heating rate of 10-20℃ / min and hold for 0.5-1.5 hours.

[0065] Then raise the temperature to 550~650℃ and hold for 0.5~1.5 hours;

[0066] Finally, the temperature is raised to 750~850℃ and held for 4~10 hours, then cooled to room temperature in the furnace to obtain a dense Mn-Co-Cu-Ce quaternary spinel coating on the surface of the metal connector.

[0067] Preferably, the temperature is increased to 400°C and held for 1 hour at a heating rate of 15°C / min, then increased to 600°C and held for 1 hour, and finally increased to 800°C and held for 6 hours.

[0068] Example 1

[0069] This embodiment provides a method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating for a semiconductor CVD reactor, including the following steps:

[0070] Step 1: Matrix Pretreatment

[0071] Crofer 22 APU ferritic stainless steel was selected as the base material for the metal connectors, with dimensions of 15 mm × 15 mm × 0.3 mm. The surface was sequentially sanded with 800#, 1000#, and 1200# SiC sandpaper until smooth and scratch-free, followed by mechanical polishing with polishing fluid to achieve a mirror finish. The polished samples were then ultrasonically cleaned for 5 minutes each in acetone and ethanol to remove surface oil and organic residues. After cleaning, the samples were rinsed with deionized water and dried. Before electrodeposition, the samples were immersed in a 15 vol.% HCl solution for 30 seconds to remove the surface passivation film, followed by rinsing with deionized water and drying.

[0072] Step 2: Layered electrodeposition of metal precursor layers

[0073] A direct current electrodeposition method was used to sequentially deposit a Mn layer, a Ni transition layer, a Co layer, and a Cu-Ce composite layer on the pretreated substrate surface. The deposition parameters for each layer are as follows:

[0074] (1) Deposition of Mn layer: The electrolyte composition was 0.3 mol / L MnSO4·H2O, 0.25 mol / L H3BO3, 0.15 mol / L sodium citrate, 1 g / L saccharin, 0.06 g / L sodium dodecyl sulfate (SDS), and 0.5 mol / L Na2SO4. The pH was adjusted to 3.5 with dilute sulfuric acid. A platinum electrode was used as the anode and the substrate as the cathode. The current density was controlled at 75 mA / cm², and the deposition was carried out at room temperature (25℃) for 15 minutes to form a Mn layer on the substrate surface.

[0075] (2) Deposition of Ni transition layer: The electrolyte composition is 0.1 mol / L NiSO4·6H2O, 0.1 mol / L Na2SO4, and 0.2 mol / L H3BO3, and the pH is adjusted to 3.5. The current density is controlled at 20 mA / cm², and the deposition is carried out at room temperature for 1 minute to form a Ni transition layer on the surface of the Mn layer.

[0076] (3) Co layer deposition: The electrolyte composition was 0.2 mol / L CoSO4·7H2O, 0.25 mol / L H3BO3, 0.5 mol / L Na2SO4, 1 g / L saccharin, and 0.06 g / L SDS, with pH adjusted to 3.5. The current density was controlled at 15 mA / cm², and deposition was carried out at room temperature for 5 minutes to form a Co layer on the surface of the Ni transition layer.

[0077] (4) Deposition of Cu-Ce composite layer: The electrolyte composition was 0.1 mol / L CuSO4·5H2O, 0.3 mol / L H3BO3, 0.40 mol / L sodium citrate, 1 g / L saccharin, 0.06 g / L SDS, and 0.2 mol / L Na2SO4, with 1.8 g / L CeO2 nanoparticles and 0.9 g / L cetyltrimethylammonium bromide (CTAB) added as dispersants, and the pH was adjusted to 8. The current density was controlled at 15 mA / cm², and deposition was carried out at room temperature for 4 minutes to form a Cu-Ce composite layer on the Co layer surface.

[0078] It is worth mentioning that the thickness of the Mn layer is 0.5–1.0 μm, the thickness of the Co layer is 10–20 μm, the thickness of the Cu layer is 0.5–1.0 μm, and the thickness of the Ce layer is 0.1–0.2 μm.

[0079] Step 3: Gradient heat treatment conversion

[0080] The sample with the deposited multilayer metal precursor was placed in a box furnace and subjected to gradient heat treatment in an air atmosphere. The heating rate was 15℃ / min, and the specific holding program was as follows: first, the temperature was raised to 400℃ and held for 1 hour, then raised to 600℃ and held for 1 hour, and finally raised to 800℃ and held for 6 hours. After the holding period, the sample was cooled to room temperature with the furnace, resulting in a Mn-Co-Cu-Ce quaternary spinel coating on the Crofer 22 APU substrate.

[0081] like Figure 1 As shown in (c), the coating surface is dense and uniform, with consistent grain distribution and no obvious cracks or pores. Figure 2 The cross-section shows that the coating is about 4~5μm thick and tightly bonded to the substrate, and the Cr element is effectively blocked inside the substrate; as shown in Table 1, the sample with 1.8g / L CeO2 added (corresponding to Example 1) only gained 1.78 mg·cm⁻² per unit area after oxidation at 800℃ for 1000 h. Figure 4 Table 2 shows that the ASR is as low as 0.17 Ω·cm² at 750℃, and the activation energy for conduction is about 95 kJ·mol⁻¹.

[0082] Example 2

[0083] The only difference between this embodiment and Embodiment 1 is that in step 2 (4), the amount of CeO2 added is 0.3 g / L and the amount of CTAB is 0.15 g / L. The remaining steps are the same as in Embodiment 1.

[0084] Figure 1 (a) shows the surface SEM morphology of the coating obtained in this comparative example. As shown in Table 1, the sample gained 2.95 mg·cm⁻² of oxidation weight after 1000 hours, and its antioxidant performance was significantly worse than that of Example 1.

[0085] Example 3

[0086] The only difference between this embodiment and Embodiment 1 is that in step 2 (4), the amount of CeO2 added is 0.9 g / L and the amount of CTAB is 0.45 g / L. The remaining steps are the same as in Embodiment 1.

[0087] like Figure 1 As shown in (b), the resulting coating has a relatively dense surface and uniform grain distribution. As shown in Table 1, the weight gain per unit area of ​​this sample after oxidation at 800℃ for 1000 h is 2.35 mg·cm⁻².

[0088] Example 4

[0089] The only difference between this embodiment and Embodiment 1 is that in step 2 (4), the amount of CeO2 added is 3.0 g / L and the amount of CTAB is 1.50 g / L. The remaining steps are the same as in Embodiment 1.

[0090] like Figure 1 As shown in (d), the surface of the resulting coating retains the spinel structure, but slight agglomeration occurs locally. As shown in Table 1, the weight gain per unit area of ​​this sample after oxidation at 800℃ for 1000 h is 2.18 mg·cm⁻².

[0091] Table 1. Oxidation weight gain per unit area for samples with different CeO2 addition amounts

[0092]

[0093] Comparative Example 1

[0094] Step 2 (4) is omitted in this comparative example, and the holding time at 800℃ in step 3 is changed to 4 hours. The resulting coating is MnCo2O4 spinel, as shown in Table 2. The ASR at 750℃ is 0.53 Ω·cm², the activation energy for conductivity is about 105.6 kJ·mol⁻¹, and the weight gain due to oxidation is significantly higher than that in Example 1.

[0095] Comparative Example 2

[0096] The difference between this comparative example and Example 1 is that CeO2 nanoparticles are not added in step 2 (4). As shown in Table 1, the weight gain of the resulting coating after 1000 hours of oxidation is 3.73 mg·cm³. ⁻2 Its antioxidant properties are significantly inferior to those of Example 1.

[0097] Table 2. ASR / Ω·cm for different coating systems at various temperatures 2 value

[0098]

[0099] Those skilled in the art should understand that the embodiments of the present invention described above and shown in the accompanying drawings are merely examples and do not limit the invention. The advantages of the present invention have been fully and effectively realized. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments; any variations or modifications can be made to the implementation of the present invention without departing from these principles.

Claims

1. A method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating, characterized in that, The preparation method includes: Using a semiconductor metal connector as the cathode, Mn, Co, Cu, and Ce layers are deposited sequentially on the substrate surface defined by the semiconductor metal connector using an electrodeposition method; wherein the thickness of the Mn layer is 0.5–1.0 μm, the thickness of the Co layer is 10–20 μm, the thickness of the Cu layer is 0.5–1.0 μm, and the thickness of the Ce layer is 0.1–0.2 μm. Then, in an oxygen-containing atmosphere, a Mn-Co-Cu-Ce quaternary spinel coating is formed on the substrate surface through gradient heating.

2. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 1, characterized in that, The Mn electrolyte comprises MnSO4·H2O 0.2~0.4 mol / L, H3BO3 0.1~0.3 mol / L, sodium citrate 0.10~0.20 mol / L, saccharin 0.5~1.5 g / L, sodium dodecyl sulfate 0.05~0.10 g / L, and Na2SO4 0.4~0.6 mol / L.

3. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 2, characterized in that, When depositing an Mn layer on the substrate, at least one of the following conditions must be met: The current density is controlled at 50~100 mA / cm²; pH value is 3.0~4.0; The concentration of sodium citrate is 0.10~0.20 mol / L; Deposit at room temperature for 5-20 minutes.

4. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 1, characterized in that, The composition of the Co electrolyte is as follows: CoSO4·7H2O 0.1~0.3 mol / L, H3BO3 0.1~0.3 mol / L, Na2SO4 0.4~0.6 mol / L, saccharin 0.5~1.5 g / L, and sodium dodecyl sulfate 0.05~0.10 g / L.

5. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 4, characterized in that, When a Co layer is deposited and formed, at least one of the following conditions must be met: The current density is controlled at 10~20 mA / cm²; pH value is 3.0~4.0; Deposit at room temperature for 2-10 minutes.

6. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 1, characterized in that, A Ni transition layer with a thickness of 0.5–5 μm is electroplated between the Mn layer and the Co layer.

7. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 6, characterized in that, When the Ni transition layer is deposited, at least one of the following conditions must be met: The current density is controlled to be 10~30 mA / cm²; pH value is 3.0~4.0; Deposit at room temperature for 0.5 to 2 minutes.

8. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to any one of claims 1-7, characterized in that, During the deposition of the Cu-Ce composite layer, the substrate after the Co layer is deposited is placed in a Cu electrolyte containing CeO2 nanoparticles. The current density is controlled at 10~20 mA / cm², the pH value is 7.5~9.0, the sodium citrate concentration is 0.30~0.50 mol / L, and the CeO2 nanoparticle addition amount is 0.5~3.0 g / L. The deposition is carried out at room temperature for 2~10 minutes to form a Cu-Ce composite layer on the surface of the Co layer.

9. The method for preparing a low-resistivity Mn-Co-Cu-Ce quaternary spinel coating according to claim 1, characterized in that, The gradient heat treatment process includes: First, heat to 350-450℃ at a heating rate of 10-20℃ / min and hold for 0.5-1.5 hours. Then raise the temperature to 550~650℃ and hold for 0.5~1.5 hours; Finally, the temperature is raised to 750~850℃ and held for 4~10 hours, then cooled to room temperature in the furnace, resulting in a dense Mn-Co-Cu-Ce quaternary spinel coating on the surface of the metal connector.

10. A spinel coating or semiconductor metal connector prepared by the preparation method described in claims 1-9.

Citation Information

Patent Citations

  • Spinel / metal linker composite material for solid oxide fuel cells and its preparation method

    CN107275656B

  • Gradient composite manganese-cobalt spinel SOFC connector coating and preparation method thereof

    CN121718876A