A method for co-producing aragonite whiskers and solidifying carbon dioxide through solid waste-seawater coupled wet carbonation

Aragonite whiskers were prepared in a seawater system using a coupled alkaline residue-seawater wet carbonation technology, which solved the problems of alkaline residue resource utilization and CO2 capture, and realized the preparation of calcium carbonate whiskers with high efficiency and low energy consumption and the application of high-performance reinforcing materials.

CN123108715APending Publication Date: 2026-11-17QINGDAO UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611255042.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-18
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the alkali residue produced in the ammonia-soda process is difficult to utilize efficiently, and traditional carbonation technology has a lengthy process, high energy consumption, serious equipment corrosion, and secondary pollution risks, making it impossible to achieve high-value utilization and effective CO2 capture.

Method used

A wet carbonation method coupled with alkali residue and seawater was adopted to carry out the carbonation reaction in a seawater system. Seawater was used as a natural reaction medium and crystal form regulator. By controlling the pH value and reaction time, high-purity aragonite-type calcium carbonate whiskers were prepared, achieving low-energy mineralization and sequestration of CO2.

Benefits of technology

High-value-added aragonite whiskers were efficiently prepared under normal pressure and low temperature conditions, reducing energy consumption and cost, improving the morphology control of calcium carbonate whiskers, providing a high-performance reinforcing material suitable for cement-based materials, and improving flexural strength and durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108715A_ABST
    Figure CN123108715A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of industrial waste resource utilization and carbon capture technology, specifically relating to a method for co-producing aragonite whiskers and solidified carbon dioxide through solid waste-seawater coupled wet carbonation. The method includes the following steps: mixing alkali residue powder with natural seawater to obtain a precursor suspension; introducing CO2 into the precursor suspension to carry out a wet carbonation reaction, monitoring pH changes during the reaction, and continuing the reaction after the pH reaches a set value until the set time is reached; and finally, filtering and drying to obtain powder containing aragonite whiskers. This invention utilizes in-situ direct carbonation of seawater, employing the spontaneous dissolution of Ca from the active calcium phase of the alkali residue in the seawater system. 2+ , with natural magnesium from seawater 2+ As a crystal form regulator, it eliminates the need for acid leaching, solid-liquid separation, and reagent regeneration. It achieves the coupling of calcium and magnesium ion dissolution, crystal form regulation, carbonation reaction, aragonite whisker generation, and CO2 solidification in one step, enabling high-value utilization of industrial waste and efficient CO2 capture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of industrial waste resource utilization and carbon capture technology, specifically relating to a method for co-producing aragonite whiskers and solidifying carbon dioxide through solid waste-seawater coupled wet carbonation. Background Technology

[0002] The large amount of soda residue produced during the ammonia-soda process mainly consists of CaO, MgO, CaCO3, CaClOH, CaSO4, and NaCl. Currently, soda residue is mostly disposed of through stockpiling, which not only occupies a large amount of land resources but also easily leads to soil salinization and serious water pollution due to its high salt and alkalinity content.

[0003] Although existing technologies have attempted to utilize ores or calcium-based solid wastes (such as papermaking sludge, red mud, and carbide slag) as CO2 mineralization raw materials, the mainstream processes mostly employ strong acid-assisted indirect carbonation technology. This technology requires the forced destruction of the solid waste crystal lattice by strong acid to leach calcium and magnesium ions, followed by multiple steps of solid-liquid separation, impurity removal, carbonation, and leaching agent regeneration. This process suffers from drawbacks such as lengthy procedures, high energy consumption, severe equipment corrosion, and a high risk of secondary pollution, making it difficult to achieve large-scale low-carbon treatment. Meanwhile, while existing direct wet carbonation technologies have relatively mild reaction conditions, they generally use fresh water or pure chemical reagents as reaction media, and related research is mostly limited to the simple preparation of low-value calcium carbonate powder, lacking the ability to directionally control the crystal form of the product (such as high-value aragonite whiskers). Summary of the Invention

[0004] The purpose of this invention is to provide a method for co-producing aragonite whiskers and solidified carbon dioxide through wet carbonation of solid waste and seawater, thereby overcoming the shortcomings of the prior art. This method uses alkaline residue to wet carbonize CO2 in a seawater system and simultaneously prepares aragonite-type calcium carbonate whiskers, solving the problems of uncontrollable crystal form, low reaction efficiency, and low added value of products in the prior art, and realizing the high-value utilization of industrial waste and the efficient capture of CO2.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: In a first aspect, the present invention provides a method for co-producing aragonite whiskers and solidifying carbon dioxide through a solid waste-seawater coupled wet carbonation process, comprising the following steps: Alkali residue powder was mixed with natural seawater to prepare a precursor suspension. CO2 is introduced into the precursor suspension for wet carbonation reaction. The pH value is monitored during the reaction. Once the pH reaches the set value, the reaction continues until the set time is reached to end the reaction and obtain the reaction product. After filtration and drying, powder containing aragonite whiskers is obtained.

[0006] This invention utilizes seawater as a natural reaction medium and crystal form regulator to construct a dual-source calcium and magnesium supply system of alkali residue and seawater. This eliminates the need for strong acid leaching and chemical additives under mild conditions of normal pressure and low temperature, significantly reducing energy consumption and costs. Simultaneously, the reaction is terminated by continuing aeration after the pH reaches a set value and reaching a set time, thus achieving precise control over the morphology of aragonite whiskers. Ultimately, this simultaneously achieves low-energy mineralization and storage of CO2 and the preparation of high-value-added whisker-reinforced materials, providing a new path for the high-value utilization of bulk solid waste that is both economical and environmentally friendly.

[0007] Secondly, the present invention provides aragonite whiskers prepared by a method of co-producing aragonite whiskers and solidified carbon dioxide by wet carbonation coupled with solid waste-seawater, wherein the mass fraction of amorphous calcium carbonate in the aragonite whiskers is ≤15%.

[0008] Thirdly, this invention provides the application of aragonite whiskers in cement-based materials. This microstructure endows the product with excellent mechanical properties and reinforcing effects, laying a material foundation for the subsequent preparation of high-performance auxiliary cementitious materials.

[0009] Fourthly, the present invention provides a cement-based material that uses aragonite whiskers as a mineral admixture.

[0010] The beneficial effects of this invention are: (1) This invention introduces seawater as a reaction medium into the alkaline slag mineralization process, utilizing the Mg²⁺ content of seawater itself. + As a natural crystal form regulator, it eliminates the high-cost steps of traditional processes involving the addition of chemical reagents or strong acid leaching. The alkaline residue serves as a solid waste substrate for the simultaneous leaching of Ca²⁺. + With Mg² + In synergy with ions in the seawater medium, it precisely maintains the specific ion concentration ratio ([Mg²⁺]) required for the stability of the aragonite phase. + ] / [Ca² + This system can operate efficiently under mild conditions of normal pressure and 40–80℃, which not only significantly reduces the energy consumption threshold for industrial CO2 capture and utilization, but also solves the risks of lengthy strong acid-assisted processes, severe equipment corrosion, and secondary pollution, demonstrating significant environmental friendliness.

[0011] (2) This invention overcomes the thermodynamic barrier of calcium carbonate crystallization phase transformation by precisely controlling the reaction temperature and medium environment, and directionally induces the formation of high-purity aragonite-type calcium carbonate whiskers in a wet carbonation system. The resulting product has a uniform morphology, with micro-sizes controlled within the range of 10-50 μm in length and 1-3 μm in diameter, and an aspect ratio as high as 8:30. This microstructure endows the product with excellent mechanical properties and reinforcing effects.

[0012] (3) This invention is not only applicable to alkali slag, but can also be extended to various calcium-based industrial or construction wastes such as recycled micro powder and steel slag, and has extremely wide applicability to raw materials. More importantly, the auxiliary cementitious material containing aragonite whiskers obtained can directly replace 5-15% of cement clinker. This material can increase the 28-day flexural strength of cement-based materials by ≥10% and reduce the drying shrinkage rate by ≥8%. While improving the durability of building materials, it also achieves permanent CO2 sequestration, which has huge economic and social benefits. Attached Figure Description

[0013] The accompanying drawings, which form part of this invention, are used to provide a further understanding of the invention. The illustrative embodiments of the invention and their descriptions are used to explain the invention and do not constitute an improper limitation of the invention.

[0014] Figure 1 The XRD patterns are of the carbonated products obtained in Examples 1-2 of this invention. Figure 2 This is a diagram showing the crystal form ratio of the carbonated products obtained in Examples 1-2 of the present invention; Figure 3 The Fourier transform infrared spectra of the carbonated products obtained in Examples 1-2 of this invention are shown below. Among them, SR-40-60-SW is the product obtained in Example 1, and SR-60-60-SW and SR-80-60-SW are the products obtained in Example 2. Detailed Implementation

[0015] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention. Specific conditions not specified in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Components whose manufacturers are not specified are all commercially available conventional products.

[0016] Among them, natural seawater has Mg 2+ The concentration is approximately 1100–1300 mg / L, Ca 2+ The concentration is approximately 400–450 mg / L, and the pH is 7.8–8.2. The composition of the residual alkali by mass percentage is shown in Table 1 below: Table 1 Chemical composition of residual alkali

[0017] In a first aspect, the present invention provides a method for co-producing aragonite whiskers and solidifying carbon dioxide through a solid waste-seawater coupled wet carbonation process, comprising the following steps: Alkali residue powder was mixed with natural seawater to prepare a precursor suspension. CO2 is introduced into the precursor suspension for wet carbonation reaction. The pH value is monitored during the reaction. The reaction is stopped when the pH reaches the set value to obtain the reaction product. After filtration and drying, powder containing aragonite whiskers is obtained.

[0018] In some other embodiments, the alkaline slag powder contains 4-4.2 wt% Na2O, 6.4-6.5 wt% MgO, 1.5-1.7 wt% Al2O3, 4.8-5.0 wt% SiO2, 4.6-4.8 wt% SO3, 13-14 wt% Cl, 25-27 wt% CaO, and a loss on ignition of ≤38%.

[0019] The alkaline residue used is mainly composed of active calcium phases such as CaO, with a CaO content of 25-27%. In the weakly alkaline environment of seawater, Ca can be rapidly and fully dissolved. 2+ This process satisfies the requirements of carbonation reactions without the need for strong acids to disrupt the crystal lattice. The unique product CaClOH from the ammonia-soda process exhibits a crystal structure that readily dissociates under the attack of polar water molecules, allowing for rapid hydrolysis at room temperature and under non-acidic conditions to release Ca. 2+ and OH - This method achieves "self-source alkaline activation" of alkali residue without the need for external acidic media. Simultaneously, it enables high-value resource utilization.

[0020] In some other embodiments, the Mg content of the natural seawater 2+ Concentration of 1100–1300 mg / L, Ca 2+ The concentration is 400–450 mg / L, and the pH is 7.8–8.2. The initial pH of seawater is 7.8–8.2, which can be reduced to 5.80–5.94 after the introduction of CO2, providing conditions for the formation of aragonite whiskers.

[0021] Seawater simultaneously acts as a reaction medium, a cheap magnesium source, a crystal form regulator, and an ionic strength modifier, simplifying the previously lengthy and costly chemical additive process into a single step, achieving process streamlining and economic efficiency. Natural seawater requires no purification and completely replaces industrial magnesium salts, significantly reducing production costs. In coastal industrial parks or solid waste disposal sites, seawater can be directly used for solid waste treatment, avoiding competition with residential areas for water resources and realizing an industrial model of "treating waste with waste and utilizing local resources." Furthermore, the carbonized reaction solution mainly contains Na. + Cl - Seawater contains intrinsic ions and a small amount of unreacted inorganic ions, without introducing organic pollutants, making it environmentally friendly. It can be recycled for the next round of carbonization reactions or reused after simple treatment, which helps reduce wastewater discharge. Seawater ions reduce whisker agglomeration, resulting in uniform product dispersion and stable aspect ratio, improving the processing performance of cementitious materials. Seawater is compatible with various calcium-based solid wastes such as alkali slag, steel slag, and recycled micro-powder, enhancing process versatility and industrialization prospects.

[0022] Utilizing Mg² in seawater + SO4² - The synergistic effect of high ionic strength environment regulates the directional preparation of aragonite whiskers. The product is a high-value-added auxiliary cementitious material that can replace cement and significantly improve mechanical properties, achieving the triple effect of solid waste utilization, carbon sequestration, and high-value building materials.

[0023] In some other embodiments, 5-15 mL of natural seawater is added per gram of alkali residue powder; preferably, 10 mL of natural seawater is added per gram of alkali residue powder. Seawater contains Na... + Other ions provide a high ionic strength environment, SO4 2- With Mg 2+ It synergistically stabilizes aragonite crystal nuclei and inhibits calcite formation. Uniform ion dispersion is achieved by pre-stirring at 400 rpm for 5 min with a liquid-to-solid ratio of 10:1, eliminating the influence of concentration fluctuations.

[0024] In some other embodiments, the CO2 flow rate is 0.2-1.0 L / min, and the volume fraction is ≥99.99%; preferably, the CO2 flow rate is 0.5 L / min.

[0025] In some other embodiments, the temperature of the wet carbonation reaction is 40-80°C, the time is 30-90 min, and the pressure is atmospheric pressure; preferably, the temperature of the wet carbonation reaction is 60°C and the time is 60 min.

[0026] In some other embodiments, the pH is set at 5.8-6.0, and the drying temperature is 30-50°C. The pH trend during the reaction is as follows: initial pH 9.79–10.61, decreasing to 5.87–6.00 at 5 min, decreasing to 5.84–5.93 at 30 min, and decreasing to 5.80–5.94 at 60 min, indicating that CO2 continuously dissolves and participates in the carbonation reaction. Considering that pH is affected by factors such as temperature, CO2 dissolution, and ion dissolution, the degree of carbonation reaction cannot be evaluated solely based on pH and requires a comprehensive evaluation combining phase and microscopic characterization results.

[0027] Preferably, the pH value is set at 5.94, and the drying temperature is 40°C. The product is dried at 40°C to constant weight, then vacuum filtered to reduce the Cl content. - Residual amount; during the filtration process, deionized water is used for rapid rinsing to avoid damaging the aragonite whisker structure.

[0028] Secondly, the present invention provides aragonite whiskers prepared by a solid waste-seawater coupled wet carbonation method for co-producing aragonite whiskers and solidifying carbon dioxide, wherein the mass fraction of amorphous calcium carbonate in the aragonite whiskers is ≤15%, and the Mg content in the amorphous calcium carbonate is ≤15%. 2+The doping amount, expressed as a Mg / Ca molar ratio, is 0.05-0.10.

[0029] Alkali residue itself is a calcium- and magnesium-rich industrial solid waste, which can simultaneously and effectively dissolve Ca² in the reaction system. + With Mg² + Together with seawater, they form a dual-source calcium and magnesium supply system, which stably maintains the ion ratio required for aragonite crystal form regulation, and significantly improves the efficiency of mineralization reaction and product stability.

[0030] Thirdly, the present invention provides the application of aragonite whiskers in cement-based materials.

[0031] Fourthly, this invention provides a cement-based material using aragonite whiskers as a mineral admixture. The resulting auxiliary cementitious material containing aragonite whiskers can be used as a mineral admixture in cement-based materials, replacing 5–15% of cement, thereby increasing the 28-day flexural strength by ≥10% and reducing the drying shrinkage by ≥8%.

[0032] The disposal of alkali residue mainly relies on stockpiling, which causes serious land occupation and environmental pollution (soil salinization and water pollution). Although there have been attempts at mineralization utilization, the mainstream strong acid-assisted process is difficult to promote due to its lengthy process, high energy consumption, equipment corrosion and secondary pollution risks. The mild direct wet carbonation technology is limited by freshwater medium and cannot use seawater magnesium source to control crystal form, and can only produce low-value powder, which limits the large-scale resource utilization and high-value utilization of alkali residue.

[0033] This invention employs in-situ direct carbonation of seawater, utilizing the spontaneous dissolution of Ca from the active calcium phase of the alkali residue within the seawater system. 2+ , with natural magnesium from seawater 2+ As a crystal form regulator, it eliminates the need for acid leaching, solid-liquid separation, and reagent regeneration, achieving a one-step coupling of calcium and magnesium ion dissolution, crystal form regulation, carbonation reaction, aragonite whisker generation, and CO2 solidification.

[0034] Example 1 This embodiment provides a method for co-producing aragonite-type calcium carbonate whiskers and simultaneously solidifying CO2 by wet carbonation of alkaline residue in a seawater system, specifically including the following steps: The dried and ground alkali residue powder (CaO=25.98wt%, MgO=6.45wt%) was mixed with natural seawater at a liquid-to-solid ratio of 10:1 (mL / g), and pre-stirred at 400 rpm for 5 min to ensure thorough dispersion and dissolution of the alkali residue and release of Ca. 2+A precursor suspension was formed. 99.99% CO2 (volume fraction) was introduced at 0.5 L / min, and a wet carbonation reaction was carried out at 40℃ and atmospheric pressure for 60 min. The pH value was monitored in real time during the reaction to assess the carbonation rate. Once the pH reached the set value, the reaction was continued until a suitable time point was reached, at which point the reaction was terminated, yielding the product. The product was filtered through medium-speed qualitative filter paper, and the filtered product was dried at 40℃ to constant weight to obtain a powder containing aragonite whiskers, labeled SR-40-60-SW.

[0035] The testing methods used are as follows: X-ray powder diffraction (XRD): The crystal composition of the carbonation products was studied by X-ray powder diffraction. The measurement range was 5–70° with a step size of 0.02°. To quantitatively determine the calcite content, 20% by weight of corundum was added to the carbonated SR, and the XRD patterns were analyzed by Rietveld using TOPAS.

[0036] Fourier Transform Infrared Spectroscopy (FTIR): The carbonated product was evaluated using Fourier transform infrared spectroscopy to obtain its silicon structure. The scanning range was 4000–500 cm⁻¹. -1 1 cm resolution -1 .

[0037] Scanning electron microscopy (SEM) was used to examine the morphology of carbonated SR. The samples were first coated with a gold layer, and then tested under high vacuum conditions with an accelerating voltage of 10 kV.

[0038] Thermogravimetric analysis (TGA) was performed using a thermogravimetric analyzer to obtain thermogravimetric data for carbonated SR. For each test, approximately 12 mg of powder was heated to 1000°C under nitrogen atmosphere at a heating rate of 10°C / min.

[0039] Without the injection of carbon dioxide, the pH value of the SR-seawater system was monitored using a pH meter (model PHS-3E). The values ​​of these solutions were recorded at 40, 60, and 80°C, from the time of CO2 introduction to 60 minutes.

[0040] The results showed that the aragonite phase content was 2.2% as determined by XRD, with whisker lengths of 15–45 μm and aspect ratios of 10:25.

[0041] Example 2 Unlike Example 1, the temperature of the wet carbonation reaction was set to 60°C and 80°C, respectively, while the other conditions were the same as in Example 1. The products were labeled as SR-60-60-SW and SR-80-60-SW, respectively.

[0042] Depend on Figure 1 The results showed that calcite (C), aragonite (A), vaterite (V), and gypsum (G) were detected in all samples, but the relative contents of each crystal phase varied significantly at different temperatures.

[0043] At 40℃, the calcite diffraction peaks in sample SR-40-60-SW are the most prominent, especially with strong characteristic peaks around 28°, while the aragonite characteristic peaks are weaker, with low-intensity diffraction signals appearing only at some angles. This indicates that calcium carbonate mainly precipitates in the thermodynamically stable form of calcite under low-temperature conditions.

[0044] When the temperature is increased to 60℃, the calcite peak intensity decreases significantly, while the aragonite characteristic peaks begin to increase. More obvious aragonite diffraction peaks appear near 26°, 46° and 50°, indicating that the increase in temperature promotes the formation of the aragonite crystal phase.

[0045] When the temperature further increased to 80℃, the characteristic peaks of aragonite were further enhanced, and its diffraction peak intensity reached its maximum, while the calcite peaks were further weakened, indicating that high-temperature conditions are favorable for Mg²⁺. + The inductive effect promotes the formation of aragonite whiskers. Meanwhile, the residual peaks in the raw materials have largely disappeared, indicating that the active components in the alkali residue have undergone more complete transformation.

[0046] Overall, as the reaction temperature increased from 40℃ to 80℃, the calcite in the system gradually transformed into aragonite, and the utilization rate of the active components of the alkali residue continuously improved, indicating that the increase in temperature is conducive to the carbonation reaction and the directional formation of the aragonite crystal phase.

[0047] Depend on Figure 2 The results showed that the initial calcite content remained at around 21.08%, indicating that this part originated from the alkali residue raw material itself.

[0048] As the reaction temperature increases, the content of newly formed calcite shows a significant decreasing trend, from 41.08% at 40℃ to 26.26% at 60℃, and further to 21.96% at 80℃. Correspondingly, the aragonite content continues to increase, from only 2.20% at 40℃ to 7.98% at 60℃, and finally reaching 14.50% at 80℃, an increase of more than 6 times.

[0049] Meanwhile, the content of aragonite increased from 7.88% to 13.06%, then slightly decreased to 9.59%, indicating that aragonite, as a metastable intermediate phase, formed more abundantly at medium temperatures, while some further transformed into aragonite under high-temperature conditions. The content of amorphous phase increased from 7.95% to 9.28%, a relatively small change, indicating a high degree of overall crystallinity in the system. Furthermore, the gypsum content increased from 17.59% to 21.89%, indicating that with the carbonation reaction, some calcium components transformed, leading to a relative enrichment of the gypsum phase.

[0050] Comprehensive analysis shows that increased temperature significantly promotes aragonite formation and inhibits calcite precipitation. The highest aragonite content was obtained at 80℃, indicating that this temperature is most favorable for controlling the crystal form of calcium carbonate and preparing aragonite whiskers.

[0051] Depend on Figure 3 The results showed that the characteristic peak of the Fourier transform infrared spectrum was 1795 cm⁻¹. - ¹ The weak absorption peak is due to the stretching vibration of free CO2 or carbonate C=O, and is a minor interfering peak. 1640 cm⁻¹ - ¹ Strong absorption peak corresponds to hydroxyl bending vibration; 1450 cm⁻¹ - ¹ This represents the asymmetric stretching vibration of the carbonate group, a characteristic peak position for carbonation products; 1264 cm⁻¹ - ¹ Attributable to Si-O stretching vibrations, characterizing the material's bonding properties; 1116 cm⁻¹ - ¹、1063 cm - ¹ The stretching vibrations of Si-O-Si and Si-O confirm the presence of hydration gel and aggregate. 874 cm⁻¹ - ¹、854 cm - ¹ These are characteristic peaks of calcite and aragonite, respectively, 713 cm. - ¹、666 cm - ¹ represents the carbonate bending vibration peak, indicating that the system undergoes carbonation and calcium carbonate is formed.

[0052] Comparison of samples at different temperatures: The sample at 60℃ was at 1420 cm. - ¹、874 cm - ¹、713 cm - ¹ The prescription shows a distinct characteristic peak for calcination, 666 cm⁻¹ - ¹ The silicon-oxygen peak shows slight broadening; the sample at 80℃ has a peak length of 666 cm⁻¹. - ¹ The silicon-oxygen peak is significantly broadened to 854 cm⁻¹. - ¹、874 cm -¹ Shoulder peaks appear. According to Lambert-Beer's law, the absorbance of the characteristic peak of calcium carbonate in the 80℃ sample is higher than that in the 60℃ sample, indicating that more calcium carbonate is generated and the CO2 curing efficiency is higher at this temperature; the characteristic peaks of calcium carbonate in the 40℃ sample are the lowest, indicating the weakest degree of carbonation reaction.

[0053] Reasons for performance differences: Based on XRD phase composition, quantitative proportions, and infrared microstructure evolution, the effects of temperature on reaction efficiency, crystal form evolution, microstructure, and final performance are as follows: 1. For samples at 40℃, at lower temperatures, the dissolution rates of CaO and MgO in the alkali residue are slower, and the Ca²⁺ content in the system is higher. + and Mg² + Insufficient concentration. Mg²⁺ + The adsorption inhibition effect on calcite crystal faces is weak, leading to the preferential formation of thermodynamically stable calcite by calcium carbonate. Due to the low aragonite content of only 2.20%, it is difficult to form a continuous acicular whisker network structure, thus limiting crack bridging and pore filling effects. Simultaneously, the total calcium carbonate formation is low, resulting in insufficient CO2 fixation efficiency. Therefore, this sample exhibits the worst performance in terms of carbon fixation capacity, mechanical strengthening effect, and volume stability.

[0054] 2. For the sample at 60℃, as the temperature increases, Ca²⁺… + and Mg² + The release rate increased significantly, and the system gradually reached a state conducive to aragonite formation. + / Ca² + The proportions show that the aragonite content increased to 7.98%, while the aragonite content reached its highest value of 13.06%, indicating that the system was in an active crystal transformation stage. Numerous needle-like crystals began to form and overlap, effectively filling pores and hindering crack propagation, resulting in better toughening and volume stability. At this point, reaction efficiency, crystal form regulation, and structural stability achieved a good balance, thus the overall performance was significantly better than the sample at 40℃.

[0055] 3. The 80℃ sample exhibited the most complete dissolution of active components from the alkali slag under these conditions, with aragonite content reaching 14.50%, more than six times that of the 40℃ sample. Numerous aragonite whiskers formed a three-dimensional interwoven structure within the system, effectively filling pores and preventing crack propagation through a bridging mechanism, thus significantly improving the material's flexural strength and durability. Simultaneously, calcium carbonate formation was highest, and CO2 mineralization fixation efficiency was optimal, resulting in the best carbon fixation performance. Furthermore, high temperature enhanced Mg²⁺... + The regulation of crystal growth inhibited calcite formation and further promoted the directional growth of aragonite. Therefore, the 80℃ sample exhibited the highest aragonite content, the best carbon fixation ability, and the optimal enhancement effect.

[0056] Overall summary: Increased temperature promotes the growth of Ca²⁺ in the alkali residue. + and Mg² + The release of CO2 increased the rate of CO2 mineralization and enhanced the Mg²⁺ oxidase. + The regulation of calcium carbonate crystal form gradually shifted the system from being predominantly calcite to predominantly aragonite. The aragonite content increased from 2.20% to 14.50%, while the newly formed calcite decreased from 41.08% to 21.96%, indicating a significantly enhanced crystal form regulation effect. The formation of abundant aragonite whiskers further constructed a dense reinforcing network structure, thereby improving CO2 fixation efficiency, mechanical reinforcement, and volume stability. Therefore, within the scope of this invention, the product obtained at 80℃ exhibits the best overall performance.

[0057] Example 3 Unlike Example 1, the alkaline residue powder (CaO=25.98wt%, MgO=6.45wt%) was mixed with natural seawater at liquid-to-solid ratios of 5:1 and 15:1 (mL / g), respectively, with the other conditions being the same as in Example 1.

[0058] The results show that, based on the analysis of wet carbonation reaction kinetics, ion mass transfer behavior and crystal growth theory, the solid-liquid ratio is an important parameter affecting the release rate of calcium and magnesium ions, CO2 mass transfer efficiency and aragonite whisker morphology.

[0059] When the liquid-to-solid ratio is low (around 5 mL / g), the concentration of solid particles in the system is high, and the alkaline residue particles are prone to agglomeration, leading to a thickening of the liquid phase diffusion layer and Ca²⁺. + and Mg² + It is difficult for it to diffuse into the solution in a timely manner. Meanwhile, in localized areas, Ca²⁺… + The concentration rapidly reached a supersaturated state, causing CO3²⁻ - Preferential nucleation occurs on the particle surface, forming disordered, massive calcium carbonate. Due to Mg²⁺... + Diffusion is hindered, preventing effective adsorption onto the active growth surface of calcite and its ability to regulate crystal structure, thus reducing the proportion of aragonite formation. In addition, excessively high slurry viscosity weakens the CO2 gas-liquid mass transfer efficiency, resulting in uneven carbonization reaction and ultimately leading to a wide particle size distribution, short and coarse whiskers, low aspect ratio, and decreased carbon fixation efficiency.

[0060] When the liquid-to-solid ratio is increased to a suitable range (around 10 mL / g), the system exhibits good fluidity and mass transfer conditions, and the Ca²⁺ in the alkali residue... + and Mg² + It can stably release and uniformly disperse in the liquid phase to form suitable Mg²⁺. + / Ca² +Concentration ratio. At this point, the dissolution and diffusion rate of CO2 in the liquid phase reaches a dynamic equilibrium with the ion release rate, and the system has a moderate supersaturation, which is conducive to aragonite crystal growth. Mg² + Preferential adsorption onto calcite crystal faces inhibits their growth, thereby promoting aragonite crystal nucleus formation and directional growth, resulting in needle-like or fibrous aragonite whiskers with longer lengths and larger aspect ratios. This structure not only increases CO2 mineralization fixation but also plays a bridging, toughening, and crack-retarding role in subsequent cement-based materials, optimizing the overall performance of the product.

[0061] When the liquid-to-solid ratio increases further (above 15 mL / g), the Ca²⁺ content in the system... + and Mg² + The concentration is significantly diluted, the probability of ion collisions decreases, and the rate of calcium carbonate crystal nucleation slows down. Due to the reduced supersaturation of the system, the driving force for crystal growth is insufficient, resulting in a decrease in the number of aragonite whiskers and incomplete growth of some crystals. At the same time, excess liquid phase will reduce the CO2 utilization efficiency per unit volume, increase the energy consumption of subsequent processes such as filtration and drying, and is not conducive to industrial applications. Therefore, although an excessively high liquid-to-solid ratio can improve dispersibility, it will reduce the efficiency of the mineralization reaction and the yield of aragonite.

[0062] In summary, the solid-liquid ratio influences ion dissolution, gas-liquid mass transfer, supersaturation establishment, and crystal growth kinetics, collectively determining the crystal composition, whisker morphology, and carbon fixation performance of the carbonation products. A liquid-solid ratio of approximately 10 mL / g achieves the optimal match between ion release and crystal growth, resulting in aragonite whisker products with superior performance.

[0063] Comparative Example 1 Unlike Example 1, natural seawater was replaced with an equal amount of deionized water. Specifically, the alkali residue powder and deionized water were mixed at a liquid-to-solid ratio of 10:1 (mL / g), and the other conditions were the same as in Example 1.

[0064] The results showed that calcite was the main crystal form in the product, with aragonite content ≤10% and indistinct whisker morphology, indicating that Mg... 2+ It plays a crucial role in the formation of aragonite.

[0065] Comparative Example 2 Unlike Example 1, an equal amount of natural seawater was replaced with MgCl2 solution, that is, the alkaline slag powder was mixed with MgCl2 solution (Mg... 2+ Concentration = 1200 mg / L, Mg 2+ Mix the liquid and solid components (with the same concentration as seawater) at a liquid-to-solid ratio of 10:1 (mL / g), and follow the same conditions as in Example 1.

[0066] The results showed that the whisker length was 12–40 μm, with an aspect ratio of 9:22, slightly lower than that of the seawater system, indicating the presence of other ions (such as Na+) in seawater. +SO4 2 It has a synergistic effect on crystal form regulation.

[0067] Comparative Example 3 Unlike Example 1, the alkaline residue powder was replaced in equal amounts with a mixture of CaO and MgO, wherein the mass ratio of CaO to MgO was 4:1, and the other conditions were the same as in Example 1.

[0068] Comparative Example 3 used a mixture of pure CaO and MgO to replace the alkali residue powder, but lost the CaClOH, NaCl, and SO4²⁻ in the residual alkali. - The complex ionic environment and synergistic regulatory effects of components such as SiO2 lead to the transformation of the system from a "residual alkali-seawater dual-source calcium-magnesium system" to a "CaO-MgO single calcium-magnesium system." This transformation significantly alters the ion release behavior, crystal nucleation process, and calcium carbonate crystal evolution, thus affecting the performance of the final product.

[0069] First, during the carbonation reaction, the residual alkali in Example 1 can not only provide Ca²⁺ + and Mg² + The active calcium phase, including CaClOH, can continuously dissolve and release Ca²⁺. + and OH - This maintains a stable ion supply for the system. Simultaneously, the Na in the residual alkali... + Cl - and SO4² - It can improve the ionic strength of the system, regulate the surface energy of the crystal, and react with Mg²⁺ in seawater. + Together, they promote the formation and directional growth of aragonite crystal nuclei. In Comparative Example 3, Ca²⁺… + The primary cause is the rapid hydration and dissolution of CaO, resulting in a large release of calcium carbonate within a short period. This rapidly leads to a highly supersaturated state in localized areas, making it easier for calcium carbonate to precipitate in the thermodynamically stable calcite form. Due to the lack of synergistic regulation from multiple ions, Mg²⁺… + The adsorption inhibition effect of calcite crystal faces is not fully utilized, thus the proportion of calcite formation in the system increases, while aragonite formation is suppressed.

[0070] Secondly, from the perspective of the crystal growth process, the residual alkali and seawater in Example 1 together form a stable dual-source calcium and magnesium supply system, which can maintain a suitable Mg²⁺ level. + / Ca² + The concentration ratio favors the preferential growth of aragonite along the c-axis, forming needle-like whiskers with a large aspect ratio. However, in Comparative Example 3, the dissolution rate of CaO is significantly faster than that of MgO, leading to a decrease in Ca²⁺ concentration in the initial stage of the reaction. + The concentration increased rapidly, while Mg² + The release is relatively delayed, causing the Mg² in the system to... + / Ca² + A low proportion of aragonite is unfavorable for the formation of aragonite whiskers. The resulting calcium carbonate tends to exhibit a granular, short columnar, or agglomerated structure, with significantly reduced whisker length and aspect ratio, making it difficult to form a continuous fiber-reinforced network.

[0071] In addition, the active phases such as CaClOH in the residual alkali can continuously release Ca²⁺. + This ensures the continued progress of the subsequent carbonation reaction, improving CO2 utilization and mineralization. In Comparative Example 3, although CaO exhibits high initial reactivity, as calcium carbonate deposits on the particle surface, a dense coating layer easily forms, hindering further dissolution of the internal CaO and preventing some calcium source from fully participating in the mineralization reaction. Therefore, its CO2 fixation and carbonation conversion rate are expected to be lower than in Example 1, resulting in a decrease in overall carbon fixation efficiency.

[0072] From the perspective of product structure analysis, the residual alkali in Example 1, in addition to providing calcium and magnesium ions, also contains a certain amount of SiO2 and other mineral components. During carbonization, it can form a small amount of silicate gel or composite structure, improving the density of the product and the interparticle bonding ability. In contrast, the product obtained in Comparative Example 3 is mainly composed of calcium carbonate, with a relatively simple microstructure, high porosity, and weak particle bonding ability. Therefore, its structural stability and dispersion performance are reduced.

[0073] Ultimately, in cement-based material applications, the aragonite whiskers prepared in Example 1 significantly improved the flexural strength and durability of the material through bridging toughening, crack deflection, pore filling, and stress transfer, while reducing drying shrinkage. In contrast, Comparative Example 3, due to reduced aragonite content, shorter whisker length, and lower aspect ratio, exhibited significantly weakened crack suppression and strengthening effects, resulting in a decreased expected improvement in flexural strength, a reduced effect on improving drying shrinkage, and limited overall durability improvement.

[0074] In summary, although Comparative Example 3 and Example 1 have the same CaO and MgO content, the residual alkali is not only a source of calcium and magnesium ions, but also an important regulating medium for maintaining ion balance, promoting the directional growth of aragonite whiskers, and improving CO2 mineralization efficiency. After replacing the residual alkali with pure CaO and MgO, the synergistic regulatory effect of multiple ions in the system disappears, leading to a decrease in aragonite formation ability, a deterioration in whisker morphology, a reduction in CO2 solidification efficiency, and a weakening of subsequent reinforcing effects. Therefore, its overall performance is expected to be significantly lower than that of Example 1.

[0075] Application Example 1 The auxiliary cementitious material containing aragonite whiskers obtained in Example 1 was used to replace silicate cement by 10% by mass to prepare mortar specimens. After standard curing for 28 days, the flexural strength was increased by 11% and the drying shrinkage was reduced by 9% compared with pure cement mortar, which met the performance indicators in the claims.

[0076] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for co-producing aragonite whiskers and solidified carbon dioxide through solid waste-seawater coupled wet carbonation, characterized in that, Includes the following steps: Alkali residue powder was mixed with natural seawater to prepare a precursor suspension. CO2 is introduced into the precursor suspension for wet carbonation reaction. The pH value is monitored during the reaction. Once the pH reaches the set value, the reaction continues until the set time is reached to end the reaction and obtain the reaction product. After filtration and drying, powder containing aragonite whiskers is obtained.

2. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, The alkaline slag powder contains 4-4.2 wt% Na2O, 6.4-6.5 wt% MgO, 1.5-1.7 wt% Al2O3, 4.8-5.0 wt% SiO2, 4.6-4.8 wt% SO3, 13-14 wt% Cl, 25-27 wt% CaO, and a loss on ignition of ≤38%.

3. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, The Mg in the natural seawater 2+ Concentration of 1100-1300 mg / L, Ca 2+ The concentration is 400-450 mg / L, and the pH is 7.8–8.

2.

4. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, Add 5-15 mL of natural seawater per gram of alkali residue powder, preferably 10 mL of natural seawater per gram of alkali residue powder.

5. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, The CO2 flow rate is 0.2-1.0 L / min, and the volume fraction is ≥99.99%; preferably, the CO2 flow rate is 0.5 L / min.

6. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, The wet carbonation reaction is carried out at a temperature of 40-80℃ for 30-180 min at atmospheric pressure; preferably, the wet carbonation reaction is carried out at a temperature of 60℃ for 60 min.

7. The method for co-producing aragonite whiskers and solidified carbon dioxide by solid waste-seawater coupled wet carbonation as described in claim 1, characterized in that, The pH setting is 5.8-6.0, the drying temperature is 30-50℃, and the setting time is 30-60 min. Preferably, the pH value is set to 5.94 and the drying temperature is 40°C.

8. Aragonite whiskers prepared by the solid waste-seawater coupled wet carbonation method according to any one of claims 1-7, characterized in that, The mass fraction of amorphous calcium carbonate in aragonite whiskers is ≤15%.

9. The use of aragonite whiskers as described in claim 8 in cement-based materials.

10. A cement-based material, characterized in that, Aragonite whiskers as described in claim 8 are used as mineral admixtures.