SiC raw material preparation method and SiC raw material

By setting placer rods inside the crucible to form a placer region and then removing the placer rods, a honeycomb-like raw material is formed, which solves the problem of low sublimation rate of SiC powder and improves the sublimation rate and crystal quality.

CN123108739APending Publication Date: 2026-11-17NINGXIA CHUANGSHENG NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611347152.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-01
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

In existing technologies, the sublimation rate of SiC powder is low and unstable, resulting in low efficiency in the PVT method for preparing silicon carbide crystals.

Method used

Multiple spacer rods are set inside the crucible to form a spacer area. After silicon carbide powder is added, it is sintered at high temperature. The spacer rods are removed to form a honeycomb-like raw material. The spacer area is used as a gas phase sublimation channel. The fluid channel is formed by crushing to improve the sublimation rate.

Benefits of technology

It significantly improves the sublimation rate and crystal growth efficiency of silicon carbide powder, thereby improving crystal quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108739A_ABST
    Figure CN123108739A_ABST
Patent Text Reader

Abstract

This application provides a method for preparing SiC raw materials and the SiC raw materials themselves, belonging to the field of SiC raw material preparation technology, and solves the problem of low sublimation rate of silicon carbide powder in existing technologies. The SiC raw material preparation method of this application includes setting multiple spacer rods in a crucible, each spacer rod occupying a spacer region; adding silicon carbide powder into the crucible to fill the non-spacer regions, while controlling the upper surface height of the silicon carbide powder to be lower than the top of the spacer rods; sintering the silicon carbide powder at high temperature to form a sintered raw material; and removing the spacer rods to form a honeycomb-shaped final raw material. By installing multiple spacer rods in the crucible, multiple spacer regions are formed. When silicon carbide powder is manually added to the crucible, the powder cannot fill all the spacer regions, resulting in a honeycomb-shaped final sintered raw material. The original spacer regions become vapor-phase sublimation channels for subsequent crystal growth, which can improve the sublimation rate during crystal growth.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of silicon core preparation technology, specifically, it relates to a method for preparing SiC raw materials and SiC raw materials. Background Technology

[0002] When growing SiC single crystals using the PVT method, the particle size of the selected SiC powder affects the Si / C ratio in the growth atmosphere and the growth rate. Considering the vapor-phase evaporation rate and crystal quality, larger SiC particles are typically chosen as the growth source. However, many SiC powder manufacturers currently face the challenge of synthesizing a large amount of small SiC particles along with large-particle SiC. This waste of small-particle SiC (<0.18mm) is one of the main reasons for the high cost of SiC in the industry.

[0003] Small-particle SiC powder has a high packing density in the crucible, resulting in smaller channels for sublimation gas during sublimation and consequently, a smaller amount of gas generated, leading to a slow sublimation rate. Furthermore, the sublimation gas tends to become trapped within the silicon carbide powder, and sintering occurs between the powder particles as the sublimation reaction progresses, ultimately causing the sublimation rate to gradually decrease and become unstable. Therefore, in existing PVT methods for preparing silicon carbide crystals, small-particle-size silicon carbide powder exhibits a low and unstable sublimation rate.

[0004] Based on the above, the technical problem of this application is: how to improve the sublimation rate of silicon carbide powder. Summary of the Invention

[0005] The purpose of this application is to address the aforementioned problems in the prior art by proposing a method for preparing SiC raw materials and SiC raw materials, thereby solving the problem of low sublimation rate of silicon carbide powder in the prior art and effectively improving the sublimation rate of silicon carbide powder.

[0006] The objective of this application can be achieved through the following technical solution: a method for preparing SiC raw materials, comprising: Multiple spacer rods are placed inside the crucible, each occupying a spacer area. Silicon carbide powder is added to the crucible to fill the non-spacer areas, ensuring the upper surface of the powder is lower than the top of the spacer rods. The crucible is then sealed, and the silicon carbide powder is sintered at high temperature to form a sintered raw material. The sintered raw material is removed, and the spacer rods are removed to form a honeycomb-shaped final raw material. It should be noted that the spacer area is defined as the spatial region occupied by the spacer rods within the crucible. By installing multiple spacer rods inside the crucible, multiple spacer zones are formed. When silicon carbide powder is manually added to the crucible, the silicon carbide powder cannot fill each spacer zone. For example, the closed crucible can be transferred to a resistance furnace for high-temperature sintering, which causes the loose silicon carbide powder to form columnar sintering raw material. Then the spacer rods are removed, and the final raw material is honeycomb-shaped. The original spacer zones become vapor sublimation channels for subsequent crystal growth processes, which can improve the sublimation rate of silicon carbide raw material during crystal growth.

[0007] In the above-described SiC raw material preparation method, the placer rod is made of a material capable of generating gaseous products under an oxidizing atmosphere. The process of removing the sintered raw material and eliminating the placer rod to form a honeycomb-like final raw material includes: partially crushing the placer rod along its length to create a fluid channel; placing the sintered raw material in an oxidation furnace and heating it to oxidize the placer rod to form the final raw material. For example, the placer rod can be made of graphite or a carbon-carbon composite material. It is understood that by partially crushing the placer rod along its length, a fluid channel can be formed for oxygen flow in subsequent processes. The crushing method can be mechanical impact or laser projection. After crushing, the sintered raw material is placed in an oxidation furnace, which provides a high-temperature environment with sufficient oxygen to oxidize and remove the placer rod from the sintered raw material.

[0008] In the above-described SiC raw material preparation method, the step of removing the sintered raw material and removing the placer rods to form the final honeycomb-like raw material includes: using laser projection processing to project a laser onto the placer area to remove the placer rods. It is understood that, as an optional solution, the placer rods can also be made of other materials, but laser projection is required to remove the entire placer rod.

[0009] In the above-described SiC raw material preparation method, the step of installing multiple spacer rods inside the crucible, each spacer rod occupying a spacer area, includes: pre-setting multiple recessed mounting holes on the bottom surface of the crucible, with a spacer rod inserted into each mounting hole. It can be understood that the mounting holes are recessed relative to the bottom surface of the crucible, facilitating the insertion and positioning of the spacer rods, and the inner diameter of the mounting holes matches the outer diameter of the spacer rods, ensuring that the outer periphery of the bottom of the spacer rod is substantially in contact with the inner wall of the mounting hole.

[0010] In the above-described SiC raw material preparation method, the distribution density of the multiple mounting holes on the bottom surface of the crucible gradually decreases from near the outer peripheral wall of the crucible to near the center of the crucible. It is understood that, because the temperature near the center of the crucible is relatively low, at high temperatures, the sublimated gases Si, Si2C, and SiC2 are prone to blockage in the central region. Therefore, by increasing the distribution density of graphite pillars near the center of the crucible, the sublimation rate during subsequent crystal growth in each region of the raw material is ensured to remain relatively uniform.

[0011] In the above-described SiC raw material preparation method, the placer rod is hollow, with an open end and a closed end at its two ends along its length. During installation, the open end is inserted into the mounting hole to complete the connection, and the thickness of the closed end is configured to be less than or equal to 10 mm. It is understood that since dust particles are easily generated inside the crucible during subsequent material feeding, positioning the closed end away from the bottom of the crucible can prevent dust particles from entering the placer rod and causing blockages in subsequent processes. By making the placer rod hollow and providing an open end and a closed end at its two ends along its length, and configuring the thickness of the closed end to be less than or equal to 10 mm, the closed end can be easily broken after the raw material is sintered, thus achieving continuity along the length of the placer rod and facilitating the subsequent inflow of oxygen for rapid oxidation.

[0012] In the above-described SiC raw material preparation method, the step of adding silicon carbide powder into the crucible to fill the non-occupied area includes controlling the height of the upper surface of the silicon carbide powder in the crucible to be lower than the top tip of the occupier. It can be understood that by controlling the height of the upper surface of the silicon carbide powder in the crucible to be lower than the top tip of the occupier, it is ensured that after the occupier is oxidized and removed, the sintering raw material is penetrated along its length, thereby facilitating the sublimation of the gas phase from the penetrated region and increasing the crystal growth rate.

[0013] In the above-described SiC raw material preparation method, in the step of adding silicon carbide powder into the crucible to fill the non-occupying area within the crucible, the particle size of the added silicon carbide powder is configured to be less than 0.25 mm. It is understood that because large-particle-size SiC powder has a low density, the raw materials are not tightly packed together, and the morphology of large-particle-size raw materials varies greatly, making it difficult to control the thermal field inside the crucible. Conversely, small-particle-size SiC powder has a high density, the raw materials are tightly packed together, and the thermal field uniformity is good. Therefore, adding silicon carbide powder with a particle size of less than 0.25 mm is preferred.

[0014] In the aforementioned SiC raw material preparation method, before the step of adding silicon carbide powder into the crucible to fill the non-occupying area within the crucible, a layer of graphite paper is circumferentially arranged on the inner peripheral wall of the crucible, with a thickness of not less than 1.5 mm. It is understood that circumferentially arranging a layer of graphite paper on the inner peripheral wall of the crucible prevents the graphite crucible and SiC powder from sticking together during the subsequent high-temperature sintering process, which could prevent the sintered raw material from being poured out and affect the subsequent high-temperature oxidation process.

[0015] In the above-mentioned SiC raw material preparation method, the sealing of the crucible and the transfer of the crucible to a resistance furnace for high-temperature sintering to form sintered raw material includes: sealing the crucible with a crucible lid and transferring the entire crucible to the resistance furnace; filling the crucible with high-purity argon gas and performing three gas purging operations to remove air from the inside of the crucible; controlling the bottom temperature of the crucible to 2000℃~2200℃, while simultaneously introducing hydrogen gas to remove nitrogen gas adsorbed on the surface of the silicon carbide powder; controlling the bottom temperature of the crucible to 2200℃~2400℃, controlling the top temperature of the crucible to 2000℃~2100℃, controlling the synthesis pressure to 5000pa~10000pa, and the synthesis time to 20h~45h. Understandably, by raising the crucible bottom temperature to 2000℃~2200℃ at a heating rate of 1℃~5℃, controlling the flow rate of hydrogen gas to 200sccm~800sccm, after synthesizing and sintering the raw materials, they are naturally cooled to room temperature and then transferred to the next process.

[0016] In the above-described SiC raw material preparation method, the step of placing the sintered raw material into an oxidation furnace and heating it to oxidize the occupant rods to form the final raw material includes: placing the sintered raw material in an oxidation furnace, heating it to 900°C, and maintaining the temperature for 12 hours to form a honeycomb-like final raw material. It can be understood that the 12-hour high-temperature oxidation effectively removes the remaining occupant rods within the sintered raw material, thereby forming multiple through-holes in the sintered raw material, resulting in an overall honeycomb-like structure.

[0017] Another object of this application is to provide a SiC raw material prepared by the SiC raw material preparation method as described in any one of claims 1-9. It is understood that the SiC raw material prepared by the SiC raw material preparation method of this application can significantly improve the gas phase transport rate and improve crystal quality during the subsequent crystal growth stage.

[0018] Compared with the prior art, this application has the following beneficial effects: This application creates multiple occupant regions by installing multiple occupant rods inside a crucible. When silicon carbide powder is manually added to the crucible, the powder cannot fill the occupant regions. The sealed crucible is then transferred to a resistance furnace for high-temperature sintering, causing the loose silicon carbide powder to form columnar sintering material. By breaking the occupant rods along their length, fluid channels can be formed for oxygen flow in subsequent processes. After breaking, the sintering material is placed in an oxidation furnace. The oxidation furnace provides a high-temperature environment with sufficient oxygen to oxidize and remove the occupant rods from the sintering material. The final sintering material is honeycomb-shaped, and the original occupant regions become vapor-phase sublimation channels for subsequent crystal growth processes, significantly improving the sublimation rate during silicon carbide crystal growth. Attached Figure Description

[0019] Figure 1 This is a schematic flowchart of the SiC raw material preparation method of this application; Figure 2 This is a schematic diagram of the crucible used in the SiC raw material preparation method of this application; Figure 3 This is a schematic diagram of the crucible structure after the placeholder rod is installed in this application; Figure 4 This is a schematic diagram of the structure after material is added into the crucible equipped with a placeholder rod according to this application; Figure 5 This is a schematic diagram of the structure of the SiC raw material of this application; Figure 6 This is a schematic diagram of the SiC raw material synthesized in Example 1; 100, Crucible; 110, Mounting hole; 200, Placeholder rod; 210, Closed end; 300, SiC raw material; 310, Cylindrical hole. Detailed Implementation

[0020] To make the above-mentioned objectives, features, and advantages of this application more apparent and understandable, specific embodiments of this application are described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of this application. However, this application can be implemented in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of this application. Therefore, this application is not limited to the specific embodiments disclosed below.

[0021] In the description of this application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "upper", "lower", "front", "rear", "left", "right", "vertical", "horizontal", "top", "bottom", "inner", "outer", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc., indicating the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings, are only for the convenience of describing this application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation, and therefore should not be construed as a limitation of this application.

[0022] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0023] In this application, unless otherwise expressly specified and limited, the terms "installation," "connection," "joining," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise expressly limited. Those skilled in the art can understand the specific meaning of the above terms in this application according to the specific circumstances.

[0024] In this application, unless otherwise expressly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "on top of," and "over" the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0025] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only embodiments.

[0026] First, refer to Figure 1 The SiC raw material preparation method of this application includes: S100: Install multiple spacer rods 200 inside the crucible 100, with each spacer rod 200 occupying a space to form a spacer area; S200: Silicon carbide powder is added into crucible 100 to fill the non-occupied area of ​​crucible 100, and the height of the upper surface of the silicon carbide powder is controlled to be lower than the top of the occupier 200. S300, a sealed crucible 100, is used to sinter the silicon carbide powder inside the crucible 100 at high temperature to form a sintered raw material; S400: Remove the sintering raw material and remove the placer rod 200 to form the final raw material in the shape of honeycomb briquettes.

[0027] It should be noted that the occupancy zone is defined as the space occupied by the occupancy rod 200 within the crucible 100. By installing multiple occupancy rods 200 within the crucible 100, multiple occupancy zones are formed. When silicon carbide powder is manually added to the crucible 100, the silicon carbide powder cannot fill each occupancy zone. For example, the sealed crucible 100 can be transferred to a resistance furnace for high-temperature sintering, thereby forming columnar sintering raw materials from the loose silicon carbide powder. Then, the occupancy rods 200 are removed, and the final raw material is honeycomb-shaped. The original occupancy zones become vapor-phase sublimation channels in the subsequent crystal growth process, which can improve the sublimation rate during silicon carbide crystal growth.

[0028] In some embodiments, S400 and the placer rod 200 are made of a material capable of generating gaseous products under an oxidizing atmosphere. Removing the sintering raw material and the placer rod 200 to form the final honeycomb-like raw material includes: partially crushing the placer rod 200 along its length to create a fluid channel; placing the sintering raw material in an oxidation furnace and heating it to oxidize the placer rod 200 to form the final raw material. Exemplarily, the placer rod 200 can be made of graphite or a carbon-carbon composite material. It is understood that by partially crushing the placer rod 200 along its length, a fluid channel can be formed for oxygen flow in subsequent processes. The crushing method can be mechanical impact or laser projection. After crushing, the sintering raw material is placed in an oxidation furnace, which provides a high-temperature environment with sufficient oxygen to oxidize and remove the placer rod 200 from the sintering raw material.

[0029] In some embodiments, step S400, removing the sintering raw material and removing the placer rod 200 to form the final honeycomb-shaped raw material, includes: using laser projection processing to project a laser onto the placer area to remove the placer rod 200. It is understood that, as an alternative, the placer rod 200 may also be made of other materials, but this requires laser projection to remove the entire placer rod 200.

[0030] See Figure 2 and Figure 3 In some embodiments, multiple placeholder rods 200 are installed inside the crucible 100. Each placeholder rod 200 occupies a place to form a placeholder area. This includes: multiple recessed mounting holes 110 pre-set on the bottom surface of the crucible 100, with each placeholder rod 200 inserted into one of the mounting holes 110. It is understood that the mounting holes 110 are recessed relative to the bottom surface of the crucible 100, facilitating the insertion and positioning of the placeholder rod 200. Furthermore, the inner diameter of the mounting hole 110 matches the outer diameter of the placeholder rod 200, ensuring that the outer periphery of the bottom of the placeholder rod 200 is substantially in contact with the inner peripheral wall of the mounting hole 110.

[0031] In some embodiments, the distribution density of the plurality of mounting holes 110 on the inner bottom surface of the crucible 100 gradually decreases from near the outer peripheral wall of the crucible 100 to near the center of the crucible 100. It is understood that, since the temperature near the center of the crucible 100 is relatively low, at high temperatures, the sublimated gases Si, Si2C, and SiC2 are prone to blockage in the central region of the crucible 100. Therefore, by increasing the distribution density of graphite pillars near the center of the crucible 100, the sublimation rate during subsequent crystal growth in various regions of the raw material is ensured to remain relatively uniform.

[0032] In some embodiments, the placeholder 200 is hollow, and its two ends along its length are an open end (not shown) and a closed end 210 (see reference). Figure 4During installation, the open end is inserted into the mounting hole 110 to complete the connection, and the thickness of the closed end 210 is configured to be less than or equal to 10 mm. It is understood that dust particles are easily generated inside the crucible 100 during subsequent material feeding. Therefore, positioning the closed end 210 away from the bottom of the crucible 100 can prevent dust particles from entering the placer rod 200 and causing blockages in subsequent processes. By making the placer rod 200 hollow and setting an open end and a closed end 210 at both ends along its length, and configuring the thickness of the closed end 210 to be less than or equal to 10 mm, the closed end 210 can be easily broken after the raw material is sintered, thus achieving a through-flow along the length of the placer rod 200, facilitating the subsequent flow of oxygen for rapid oxidation.

[0033] In some embodiments, adding silicon carbide powder into the crucible 100 to fill the non-occupied area of ​​the crucible 100 includes controlling the height of the upper surface of the silicon carbide powder in the crucible 100 to be lower than the top tip of the placer rod 200. It is understood that by controlling the height of the upper surface of the silicon carbide powder in the crucible 100 to be lower than the top tip of the placer rod 200, it is ensured that after the placer rod 200 is subsequently oxidized and removed, the sintering material is penetrated along its length, thereby facilitating the sublimation of the gas phase from the penetrated region and increasing the crystal growth rate.

[0034] In some embodiments, in the step of adding silicon carbide powder into the crucible 100 to fill the non-occupied area within the crucible 100, the particle size of the added silicon carbide powder is configured to be less than 0.25 mm. It is understood that because large-particle-size SiC powder has a low density, the raw materials are not tightly packed together, and the morphology of large-particle-size raw materials varies greatly, thus the thermal field inside the crucible 100 is difficult to control. Conversely, small-particle-size SiC powder has a high density, the raw materials are tightly packed together, and the thermal field uniformity is good. Therefore, adding silicon carbide powder with a particle size of less than 0.25 mm is preferred.

[0035] In some embodiments, before adding silicon carbide powder into the crucible 100 to fill a portion of the non-occupied area within the crucible 100, a layer of graphite paper is circumferentially arranged on the inner peripheral wall of the crucible 100, with a thickness of not less than 1.5 mm. It is understood that circumferentially arranging a layer of graphite paper on the inner peripheral wall of the crucible 100 prevents the graphite crucible 100 and SiC powder from adhering together during subsequent high-temperature sintering processes, which could prevent the sintered raw materials from being poured out and affect subsequent high-temperature oxidation processes.

[0036] In some embodiments, sealing the crucible 100 and transferring it to a resistance furnace for high-temperature sintering to form a sintering raw material includes: covering the crucible 100 with a lid to seal it, and transferring the entire crucible 100 to the resistance furnace; filling the crucible 100 with high-purity argon gas and performing three gas purging operations to remove air from inside the crucible 100; controlling the bottom temperature of the crucible 100 to 2000℃~2200℃, for example, the bottom temperature can be 2000℃, 2020℃, 2040℃, 2060℃, 2080℃, 2100℃, 2120℃, 2140℃, 2160℃, 2180℃, and 2200℃, while simultaneously introducing hydrogen gas to remove nitrogen gas adsorbed on the surface of the silicon carbide powder; controlling the bottom temperature of the crucible 100 to 2200℃~2400℃, for example, the bottom temperature can be 2200℃, 2220℃, and 2200℃. 40℃, 2260℃, 2280℃, 2300℃, 2320℃, 2340℃, 2360℃, 2380℃, and 2400℃, controlling the top temperature of crucible 100 to 2000℃~2100℃. For example, the top temperature could be 2000℃, 2020℃, 2040℃, 2060℃, 2080℃, 2100℃, 2120℃, 2140℃, or 2160℃. The synthesis temperature is 2180℃ and 2200℃, and the synthesis pressure is controlled to 5000 Pa to 10000 Pa. For example, the synthesis pressure can be controlled to be 5000 Pa, 5500 Pa, 6000 Pa, 6500 Pa, 7000 Pa, 7500 Pa, 8000 Pa, 8500 Pa, 9000 Pa, 9500 Pa, or 10000 Pa, and the synthesis time is 20 h to 45 h. It can be understood that by heating the crucible bottom temperature to 2000℃ to 2200℃ at a heating rate of 1℃ to 5℃, controlling the flow rate of hydrogen gas to 200 sccm to 800 sccm, after synthesizing and sintering the raw materials, it is naturally cooled to room temperature and then transferred to the next process.

[0037] In some embodiments, placing the sintering raw material into an oxidation furnace and heating it to oxidize the placer bars 200 to form the final raw material includes: placing the sintering raw material in the oxidation furnace, heating it to 900°C, and maintaining it for 12 hours to form a honeycomb-like final raw material. It is understood that the 12-hour high-temperature oxidation effectively removes any remaining placer bars 200 from the sintering raw material, thereby forming multiple through-holes 310 within the sintering raw material (see reference). Figure 5 The sintering raw materials are generally honeycomb shaped.

[0038] The SiC raw material 300 of this application is prepared using the SiC raw material preparation method of this application. It is understood that the SiC raw material 300 prepared using the SiC raw material preparation method of this application can significantly improve the gas phase transport rate and improve the crystal quality during the subsequent crystal growth stage.

[0039] Experimental procedure: Example 1: Oxidized honeycomb-shaped SiC raw material 300 was placed in crystal growth crucible 100 for the growth of 4H-SiC single crystals. Growth method: PVT; Seed crystal information: 4° off the C-axis in the <11-20> direction; Growth template: C-plane; Growth temperature: 2100℃~2200℃ at the seed crystal location, 2250℃~2350℃ at the raw material source location; Axial gradient: 20℃~70℃ / cm; Growth pressure: 5mbar~50mbar. The final product is as follows. Figure 6 As shown.

[0040] Example 2: The operation method is basically the same as that of Example 1. The difference is that when preparing SiC raw material 300, the distribution spacing of the mounting holes 110 in the raw material crucible 100 is equidistant. That is, the distribution density of the placer rods 200 is basically the same in each region of the crucible 100 cross section. Thus, the SiC raw material 300 obtained is different from that of Example 1. The SiC raw material 300 of Example 2 is used for crystal growth using the same process.

[0041] Example 3: The operation method is basically the same as that of Example 1. The difference is that when preparing SiC raw material 300, the distribution spacing of the mounting holes 110 in the raw material crucible 100 is randomly distributed. That is, the distribution density of the placer rods 200 is random in each region on the cross section of the crucible 100. Thus, the SiC raw material 300 obtained is different from that of Example 1 and Example 2. The SiC raw material 300 of Example 3 is used for crystal growth using the same process.

[0042] Comparative Example 1: The operation method is basically the same as that of Example 1, except that when preparing SiC raw material 300, no mounting hole 110 is provided in the raw material crucible 100, and no placeholder rod 200 is installed. The conventional crucible 100 is used for preparation. As a result, the SiC raw material 300 obtained is different from that of Example 1, Example 2 and Example 3. The SiC raw material 300 of Comparative Example 1 is used to grow crystals using the same process.

[0043] The crystals formed from the crystal growth in Examples 1, 2, 3, and Comparative Example 1 were subjected to various performance tests, and the following data table was obtained:

[0044] In summary, the honeycomb-shaped SiC raw material 300 effectively solves the problem of gas phase transport, allowing crystals to grow to thicknesses of 25mm, 21mm, and 10mm. During high-temperature crystal growth, the temperature at the center of crucible 100 is consistently lower than the outer edge, resulting in slower volatilization at the center. This necessitates more voids to ensure the transport of silicon-rich vapor. Experiments in Examples 2 and 3 show that the temperature difference at the center is a crucial factor affecting silicon carbide crystal growth. Therefore, it is necessary to control the distribution of voids in the occupant rods 200 near the outer periphery to the center of crucible 100 to ensure the uniformity of upward transport of silicon-rich vapor. Conversely, referring to Comparative Example 1, the crystal thickness is only 4mm. This is because during gas transport, the silicon-rich gas lacks an effective mass transfer path (no channel), resulting in high resistance to upward gas transport. This leads to localized gas oversaturation within the powder, causing condensation between powder particles. Because gas blockage in Comparative Example 1 prevents normal transport, the Si / C molar ratio cannot remain stable, resulting in higher screw dislocation, edge dislocation, and basal plane dislocation densities in the grown crystal compared to Examples 1. Because small-particle-size SiC powders are more densely packed, the thermal field of the raw material is easier to control, resulting in fewer defects in the grown crystals.

[0045] Beneficial effects: This application creates multiple occupant regions by installing multiple occupant rods 200 inside a crucible 100. When silicon carbide powder is manually added to the crucible 100, the powder cannot fill the occupant regions. The sealed crucible 100 is then transferred to a resistance furnace for high-temperature sintering, causing the loose silicon carbide powder to form columnar sintering raw materials. By breaking the occupant rods 200 along their length, fluid channels can be formed for oxygen flow in subsequent processes. After breaking, the sintering raw materials are placed in an oxidation furnace. The oxidation furnace provides a high-temperature environment with sufficient oxygen to oxidize and remove the occupant rods 200 from the sintering raw materials. The final sintering raw materials are honeycomb-shaped, and the original occupant regions become vapor-phase sublimation channels for subsequent crystal growth processes, significantly improving the sublimation rate during silicon carbide crystal growth.

[0046] The specific embodiments described herein are merely illustrative examples of the spirit of this application. Those skilled in the art to which this application pertains may make various modifications or additions to the described specific embodiments or use similar methods to substitute them, without departing from the spirit of this application or exceeding the scope defined by the appended claims.

Claims

1. A method for preparing SiC raw materials, characterized in that, include: Multiple spacer rods (200) are set inside the crucible (100), and each spacer rod (200) occupies a space to form a spacer area; Silicon carbide powder is added into the crucible (100) to fill the non-occupied area of ​​the crucible (100), and the height of the upper surface of the silicon carbide powder is controlled to be lower than the top of the occupied rod (200). A sealed crucible (100) is used to sinter the silicon carbide powder inside the crucible (100) at high temperature to form a sintered raw material; Remove the sintering raw material and remove the placer rod (200) to form the final raw material in the shape of honeycomb briquettes.

2. The method for preparing SiC raw materials according to claim 1, characterized in that, The placer rod (200) is made of a material that can generate gaseous products under an oxidizing atmosphere. The removal of the sintering raw material and the removal of the placer rod (200) to form the final raw material in a honeycomb briquette shape includes: Partially break the spacer bar (200) along its length to allow it to pass through and form a fluid channel; The sintering raw material is placed in an oxidation furnace, and the temperature is raised to oxidize the placer rod (200) to form the final raw material.

3. The method for preparing SiC raw materials according to claim 1, characterized in that, The process of removing the sintering raw material and removing the placer rod (200) to form the final honeycomb briquette includes: Laser projection is used to project a laser beam onto the occupant area to remove the occupant rod.

4. The method for preparing SiC raw materials according to claim 1, characterized in that, The installation of multiple spacer rods (200) inside the crucible (100), with each spacer rod (200) occupying a spacer area, includes: multiple recessed mounting holes (110) pre-set on the bottom surface of the crucible (100), with each spacer rod (200) inserted into each mounting hole (110).

5. The method for preparing SiC raw materials according to claim 4, characterized in that, The distribution density of the multiple mounting holes (110) on the bottom surface of the crucible (100) gradually decreases from near the outer peripheral wall of the crucible (100) to near the center of the crucible (100).

6. The method for preparing SiC raw materials according to claim 4, characterized in that, The placeholder (200) is hollow, and the two ends of the placeholder (200) in the length direction are an open end and a closed end (210) respectively. During installation, the open end is inserted into the mounting hole (110) to complete the insertion. The thickness of the closed end (210) is configured to be less than or equal to 10mm.

7. The method for preparing SiC raw materials according to claim 1, characterized in that, In the step of adding silicon carbide powder into the crucible (100) to fill the non-occupied area of ​​the crucible (100), the particle size of the added silicon carbide powder is configured to be less than 0.25 mm.

8. The method for preparing SiC raw materials according to claim 1, characterized in that, Before the step of adding silicon carbide powder into the crucible (100) to fill the non-occupied area of ​​the crucible (100), a layer of graphite paper is arranged circumferentially on the inner peripheral wall of the crucible (100), and the thickness of the graphite paper is configured to be not less than 1.5 mm.

9. The method for preparing SiC raw materials according to claim 1, characterized in that, The sealed crucible (100) is transferred to a resistance furnace for high-temperature sintering to form sintered raw materials, including: Cover the crucible (100) with the lid and transfer the entire crucible (100) to the resistance furnace; High-purity argon gas is introduced into the crucible (100), and three gas washing operations are performed to remove the air inside the crucible (100); Control the bottom temperature of the crucible (100) to 2000℃~2200℃, and at the same time introduce hydrogen gas to remove nitrogen gas adsorbed on the surface of silicon carbide powder; Control the bottom temperature of crucible (100) to 2200℃~2400℃, control the top temperature of crucible (100) to 2000℃~2100℃, control the synthesis pressure to 5000pa~10000pa, and the synthesis time to 20h~45h.

10. A SiC raw material, prepared by the SiC raw material preparation method as described in any one of claims 1-9.