Magnetic field control methods and devices, Czochralski single crystal furnace, single crystal silicon rod

By applying a horizontal magnetic field to the silicon melt and controlling the periodic fluctuations in its intensity, the problem of asymmetric mass and heat transfer in the silicon melt during Czochralski growth was solved, thereby improving the uniformity of the radial resistance and oxygen content of the crystal and enhancing the quality and yield of single-crystal silicon rods.

CN123108744APending Publication Date: 2026-11-17ZING SEMICON CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611452109.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-17
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

During the Czochralski process for growing large-diameter single-crystal silicon, the horizontal magnetic field causes asymmetry in mass and heat transfer in the silicon melt, forming mass transfer dead zones and thermal dead zones. This affects the uniformity of the radial resistance and oxygen content distribution of the crystal, and consequently leads to crystal defects.

Method used

By applying a horizontal magnetic field to the silicon melt and controlling the magnetic field strength to produce periodic fluctuations based on a set reference strength, periodic Lorentz force changes are formed, which induces periodic relaxation of melt convection to form a weak stirring effect and improve heat and mass transfer conditions.

Benefits of technology

It effectively reduces the generation of thermal dead zones and mass transfer dead zones, prevents impurity accumulation, improves the uniformity of crystal radial resistance and oxygen content distribution, and enhances the quality and yield of single crystal silicon rods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108744A_ABST
    Figure CN123108744A_ABST
Patent Text Reader

Abstract

A magnetic field control method and apparatus, a Czochralski single crystal furnace, and a single crystal silicon rod are disclosed. The magnetic field control method includes applying a horizontal magnetic field to a silicon melt and controlling the magnetic field strength to periodically fluctuate based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse, which has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, during which the magnetic field strength remains at the reference strength. This application can improve the heat and mass transfer conditions of the silicon melt, reduce and avoid the generation of thermal dead zones and mass transfer dead zones, prevent the local accumulation of impurities, improve the uniformity of the radial resistance and oxygen content distribution of the crystal, and improve the quality and yield of the single crystal silicon rod.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of semiconductor technology, and more specifically to a magnetic field control method and apparatus, a Czochralski single crystal furnace, and a single crystal silicon rod. Background Technology

[0002] Single-crystal silicon is a core material for semiconductor integrated circuit manufacturing, and its quality determines the performance and yield of devices. Currently, the Czochralski (CZ) method is the mainstream process for preparing large-diameter single-crystal silicon. Its basic process includes: placing high-purity polycrystalline silicon raw material in a quartz crucible, heating and melting it under an inert gas atmosphere to form a silicon melt; then, bringing a seed crystal into contact with the surface of the silicon melt and slowly pulling it up, sequentially going through the stages of crystal introduction, shoulder formation, constant-diameter growth, and finalization, ultimately obtaining a single-crystal silicon rod. As the diameter of single-crystal silicon increases to 300 mm (12 inches), the volume of the silicon melt increases significantly, intensifying natural and thermal convection within the silicon melt, and causing significant temperature fluctuations near the solid-liquid interface, which adversely affects crystal quality.

[0003] To suppress excessive convection of the silicon melt during the growth of large-diameter single-crystal silicon, the Magnetic Czochralski (MCZ) method was developed. Among them, the Horizontal Magnetic Czochralski (HMCZ) method applies a horizontal magnetic field (the magnetic field strength is usually a fixed value or varies linearly with time) to the silicon melt during crystal pulling. This utilizes the Lorentz force to suppress convection of the silicon melt parallel to the magnetic field direction, reducing temperature fluctuations near the solid-liquid interface and thus improving the stability of crystal growth to some extent.

[0004] However, in the HMCZ process, due to the inherent directionality of the horizontal magnetic field, the convection of the silicon melt parallel to the magnetic field direction is strongly suppressed by the Lorentz force, while the convection of the silicon melt perpendicular to the magnetic field direction is almost unrestrained, resulting in a severe asymmetry in mass and heat transfer of the silicon melt in the circumferential direction. Especially under higher magnetic field strengths above 3,000 Gauss (Gs), mass transfer dead zones or thermal dead zones are easily formed in the silicon melt, which in turn causes uneven distribution of the radial resistance and oxygen content of the crystal and induces crystal defects. Summary of the Invention

[0005] The summary section introduces a series of simplified concepts, which will be further explained in detail in the detailed description section. This summary section is not intended to limit the key and essential technical features of the claimed technical solution, nor is it intended to determine the scope of protection of the claimed technical solution.

[0006] To address the existing problems, this application provides a magnetic field control method for growing single-crystal silicon using the Czochralski method, the magnetic field control method comprising: A horizontal magnetic field is applied to the silicon melt, and the magnetic field strength is controlled to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. The single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, and the magnetic field strength remains at the reference strength during the pulse interval.

[0007] In some embodiments of this application, the Czochralski method for growing single-crystal silicon sequentially undergoes a seeding stage, a shoulder formation stage, a constant diameter growth stage, and a finishing stage. The step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength is performed during the entire growth process of at least one of the following stages: the crystal pulling stage, the shoulder forming stage, the constant diameter growth stage, and the finishing stage, or within a preset crystal length range in at least one stage.

[0008] In some embodiments of this application, the frequency of the periodic fluctuation is 0.003 Hz to 0.5 Hz.

[0009] In some embodiments of this application, the absolute value of the pulse amplitude of the single pulse is 0.1% to 25% of the reference intensity.

[0010] In some embodiments of this application, the magnetic field strength is lower than the reference strength within the pulse width of the single pulse.

[0011] In some embodiments of this application, the pulse width of a single pulse is 1 second to 120 seconds, and the pulse interval is 1 second to 120 seconds.

[0012] In some embodiments of this application, the waveform of the single pulse is at least one of a rectangular wave, a trapezoidal wave, a triangular wave, and a sine wave.

[0013] According to another aspect of this application, a magnetic field control device is provided for growing single-crystal silicon using the Czochralski method, the magnetic field control device comprising: Magnetic field generating component; The controller is communicatively connected to the magnetic field generating component; The controller is configured to control the magnetic field generating component to apply a horizontal magnetic field to the silicon melt, and to control the magnetic field strength to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. The single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, and the magnetic field strength remains at the reference strength during the pulse interval.

[0014] According to another aspect of this application, a Czochralski single crystal furnace is provided, the Czochralski single crystal furnace comprising: Furnace body; A crucible disposed within the furnace body is used to contain molten silicon. The magnetic field control device described above has its magnetic field generating component disposed on the outer periphery of the crucible.

[0015] According to another aspect of this application, a single-crystal silicon rod is provided, which is grown using the magnetic field control method described in any one of the above-mentioned methods.

[0016] The magnetic field control method and apparatus, Czochralski single crystal furnace, and single crystal silicon rod of this application apply a horizontal magnetic field to the silicon melt and control the magnetic field strength to generate periodic fluctuations based on a set reference strength. This causes periodic changes in the Lorentz force on the silicon melt, which in turn induces periodic relaxation of melt convection to form a weak stirring effect. This effectively improves the heat and mass transfer conditions of the silicon melt, reduces and avoids the generation of thermal dead zones and mass transfer dead zones, prevents the local accumulation of impurities, and significantly improves the uniformity of the radial resistance and oxygen content distribution of the crystal, thereby improving the quality and yield of the single crystal silicon rod. Attached Figure Description

[0017] The following drawings, which are incorporated herein by reference and are used to understand this application, illustrate embodiments of the invention and their descriptions to explain the principles of the invention.

[0018] In the attached image: Figure 1 This is a top view schematic diagram showing the state of silicon melt and magnetic field applied during Czochralski crystal growth according to a specific embodiment of this application.

[0019] Figure 2 The diagram shows the waveform timing of the magnetic field strength acting on the silicon melt after superimposed periodic pulsed magnetic field according to a specific embodiment of this application. Detailed Implementation

[0020] The following description provides numerous specific details to offer a more thorough understanding of this application. However, it will be apparent to those skilled in the art that this application can be practiced without one or more of these details. In other instances, certain technical features well-known in the art have not been described to avoid confusion with this application.

[0021] It should be understood that this application can be implemented in various forms and should not be construed as limited to the embodiments set forth herein. Rather, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of this application to those skilled in the art. In the drawings, for clarity, the dimensions and relative dimensions of layers and regions may be exaggerated. The same reference numerals denote the same elements throughout.

[0022] It should be understood that when an element or layer is referred to as "on," "adjacent to," "connected to," or "coupled to" other elements or layers, it may be directly on, adjacent to, connected to, or coupled to other elements or layers, or there may be intervening elements or layers. Conversely, when an element is referred to as "directly on," "directly adjacent to," "directly connected to," or "directly coupled to" other elements or layers, there are no intervening elements or layers. It should be understood that although the terms first, second, third, etc., may be used to describe various elements, components, areas, layers, and / or portions, these elements, components, areas, layers, and / or portions should not be limited by these terms. These terms are only used to distinguish one element, component, area, layer, or portion from another element, component, area, layer, or portion. Therefore, without departing from the teachings of this application, the first element, component, area, layer, or portion discussed below may be referred to as the second element, component, area, layer, or portion.

[0023] Spatial relation terms such as “below,” “under,” “below,” “below,” “above,” “above,” etc., are used herein for convenience of description to describe the relationship between one element or feature shown in the figure and other elements or features. It should be understood that, in addition to the orientation shown in the figure, spatial relation terms are intended to also include different orientations of the device in use and operation. For example, if the device in the figure is flipped, then the element or feature described as “below” or “below” other elements or features will be oriented “above” other elements or features. Therefore, the exemplary terms “below” and “under” can include both above and below orientations. The device may be otherwise oriented (rotated 90 degrees or otherwise) and the spatial descriptive terms used herein will be interpreted accordingly.

[0024] The terminology used herein is for the purpose of describing particular embodiments only and is not intended to limit the scope of this application. When used herein, the singular forms “a,” “an,” and “the” are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the terms “comprising” and / or “including,” when used in this specification, identify the presence of the stated features, integers, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components, and / or groups. When used herein, the term “and / or” includes any and all combinations of the associated listed items.

[0025] To fully understand this application, detailed steps and structures will be presented in the following description to illustrate the technical solutions proposed in this application. Preferred embodiments of this application are described in detail below; however, in addition to these detailed descriptions, this application may have other implementation methods.

[0026] Example 1 The following describes a magnetic field control method according to an embodiment of this application. This magnetic field control method is used for Czochralski growth of single-crystal silicon and includes: applying a horizontal magnetic field to a silicon melt and controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. Each single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. A pulse interval is spaced between two adjacent single pulses, and the magnetic field strength remains at the reference strength during the pulse interval.

[0027] In related technologies, the magnetic field applied to the silicon melt is usually a fixed value or varies linearly with time, which can easily form mass transfer dead zones or thermal dead zones inside the silicon melt, thereby affecting the uniformity of the radial resistivity and oxygen content distribution of the crystal and inducing crystal defects.

[0028] To address the aforementioned issues, this application applies a horizontal magnetic field to the silicon melt, controlling the magnetic field strength to exhibit periodic fluctuations based on a predetermined baseline strength. This causes periodic fluctuations in the Lorentz force within the silicon melt, resulting in periodic relaxation of melt convection. This periodic relaxation effectively increases the weak stirring effect of melt mass transfer without causing destructive structural changes to the melt's own convection. Through these effects, the heat and mass transfer conditions of the silicon melt under a horizontal magnetic field are effectively improved, reducing and avoiding the formation of thermal and mass transfer dead zones, preventing localized impurity accumulation, and significantly improving the uniformity of crystal radial resistivity and oxygen content distribution. Furthermore, this periodic fluctuation of the magnetic field strength also generates micron- or nanometer-scale periodic shape oscillations at the solid-liquid interface. The weak temperature oscillations accompanying these oscillations in the high-temperature regions of the crystal do not lead to crystal defects but rather effectively suppress them, thereby significantly expanding the range of the perfect crystal processing window for single-crystal silicon and ultimately greatly improving the quality and yield of single-crystal silicon rods.

[0029] For example, Figure 1 This is a top view schematic diagram illustrating the silicon melt and magnetic field applied during Czochralski crystal growth according to a specific embodiment of this application. The outer solid circles represent the crucible used to contain the silicon melt, and the inner small solid circles represent the single-crystal silicon crystal being pulled and grown. During crystal growth, the crucible rotates in a predetermined direction (clockwise, as shown by arrow CR in the diagram), and simultaneously, the single-crystal silicon crystal growing above the melt also rotates in a predetermined direction (counterclockwise, as shown by arrow SR in the diagram). This counter-rotation of the crucible and crystal helps improve the convection state of the melt. Outside the thermal field, a horizontal magnetic field is applied to the silicon melt, such as... Figure 1 As indicated by the thick arrow at the top, the magnetic field direction B passes horizontally through the silicon melt. Due to the strong electromagnetic braking effect of a horizontal magnetic field on conductive fluids, its inherent directionality leads to a severe asymmetry in mass and heat transfer in the circumferential direction of the silicon melt. This is especially true under the influence of high-intensity magnetic fields, such as... Figure 1 As shown by the dashed ellipse in the figure, the convection zone inside the silicon melt exhibits a distinct elliptical distribution; while at both ends parallel to the magnetic field direction, the flow of the melt is strongly suppressed, thus forming a mass transfer dead zone. Within this dead zone, due to the extremely small flow of the melt and low heat exchange efficiency, the local temperature is relatively high.

[0030] To completely overcome the "dead zone" limitation caused by the reference magnetic field strength, this application does not apply a fixed or linearly varying magnetic field to the silicon melt, but rather controls the applied horizontal magnetic field (such as...). Figure 1 The magnetic field strength (as indicated by direction B in the diagram) fluctuates periodically. Specifically, combined with... Figure 1The lower right diagram, used as a parameter illustration, shows how the magnetic field strength in the horizontal direction is controlled to fluctuate periodically based on a set reference strength S, and the amplitude of this fluctuation corresponds to... Figure 1 The pulse amplitude fS is marked in the figure. Through this periodic fluctuation, the magnetic field strength acting on the silicon melt fluctuates periodically, which in turn causes periodic changes in the Lorentz force on the silicon melt. This induces periodic relaxation of melt convection, resulting in a periodic weak stirring effect in the silicon melt. This effectively improves the heat and mass transfer conditions of the silicon melt in the circumferential direction, reduces and avoids the high-temperature mass transfer dead zone at both ends of the parallel magnetic field direction, prevents the local accumulation of impurities, and thus significantly improves the uniformity of the radial resistance and oxygen content distribution of the crystal, thereby improving the quality and yield of single crystal silicon rods.

[0031] In practical implementation, the periodic fluctuation of the magnetic field strength is achieved by controlling the excitation current input to the magnetic field generating component. Specifically, the controller is communicatively connected to the magnetic field generating component located around the crucible. During crystal growth, a set reference current is input to the magnetic field generating component to excite and form a horizontal magnetic field of corresponding reference strength. To generate periodic fluctuations in the magnetic field strength in the form of pulses, the controller periodically adjusts the magnitude of the excitation current input to the magnetic field generating component according to set parameters such as pulse width, pulse interval time, and pulse amplitude. In the specific control logic, during the pulse interval time, the controller maintains the set reference current input to the magnetic field generating component, keeping the magnetic field strength at the reference strength. When entering the pulse width of a single pulse, the controller changes the magnitude of the excitation current, causing the magnetic field strength generated by the changed excitation current to deviate from the reference strength. The difference between the two values ​​corresponds to the set pulse amplitude, thereby achieving periodic fluctuations in the magnetic field strength acting on the silicon melt based on the set reference strength.

[0032] In some embodiments, the Czochralski method for growing single-crystal silicon includes heating and melting polycrystalline silicon raw material in a crucible to form a silicon melt, contacting a seed crystal with the surface of the silicon melt, and sequentially performing a seeding stage, a shoulder formation stage, a constant-diameter growth stage, and a finishing stage. The step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength, as described in this application, can be performed throughout the entire growth process of at least one of the seeding stage, shoulder formation stage, constant-diameter growth stage, and finishing stage, or within a preset crystal length range within that at least one stage.

[0033] Specifically, the magnetic field strength can be controlled to fluctuate periodically within a set baseline strength throughout the entire growth process of the four stages: seeding, shoulder formation, constant diameter growth, and finishing. Alternatively, depending on the specific needs for improving crystal quality, this periodic fluctuation can be implemented only during the entire growth process of one or more of these stages. Furthermore, more precise local growth range control is possible; that is, within at least one selected stage, the periodic fluctuation of the magnetic field strength is implemented only within a preset crystal length range.

[0034] Preferably, the step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength is mainly performed during the shoulder formation stage and the constant-diameter growth stage. This is because the shoulder formation stage involves rapid changes in the crystal diameter, resulting in severe fluctuations in the melt's thermal and flow fields, which easily lead to defects. The constant-diameter growth stage is the critical period for the formation of the single-crystal silicon rod, and it has the most stringent requirements for radial uniformity of oxygen content, radial uniformity of electrical resistance, and micro-defect control. Therefore, performing the step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength in these two stages can most effectively utilize the periodic weak stirring effect, improve the heat and mass transfer conditions of the melt, suppress the formation of thermal dead zones and mass transfer dead zones, thereby significantly improving crystal quality and yield.

[0035] In some embodiments, the periodic fluctuations are low-frequency fluctuations. The reason for using low-frequency fluctuations is twofold: firstly, it is necessary to control the rate of change of the magnetic field strength to ensure that the magnetic field generating component does not experience magnetic field quench failure; secondly, low-frequency periodic fluctuations allow the Lorentz force within the silicon melt to gradually shift, promoting periodic relaxation of melt convection, thereby generating a moderate and effective weak stirring effect without causing destructive structural changes to the melt's own convection. For example, the frequency of the periodic fluctuations can be set in the low-frequency range of 0.003 Hz to 0.5 Hz. Preferably, the frequency of the periodic fluctuations is set to approximately 0.01 Hz.

[0036] In some embodiments, the absolute value of the pulse amplitude of a single pulse is 0.1% to 25% of the reference intensity. This range ensures that the periodic fluctuations in the magnetic field intensity produce an effective weak stirring effect on the flow of the silicon melt, while avoiding the disruption of crystal growth stability caused by drastic fluctuations in the magnetic field intensity acting on the silicon melt due to excessively large pulse amplitudes.

[0037] In some embodiments, the magnetic field strength is preferably set to be lower than the reference strength within the pulse width of a single pulse, so that the magnetic field strength decreases periodically from the base strength. This periodic decrease in magnetic field strength can gradually weaken the Lorentz force resisting convection in the silicon melt, induce periodic relaxation of melt convection, effectively increase the weak stirring effect of melt mass transfer, and improve heat and mass transfer conditions.

[0038] In some embodiments, the pulse width of a single pulse is set between 1 second and 120 seconds, and the pulse interval between two adjacent single pulses is set between 1 second and 120 seconds. Limiting the pulse width and pulse interval serves to reasonably control the magnetic field change rate and prevent the magnetic field generating component from quenching due to excessively fast excitation speed. Preferably, the pulse width of a single pulse is set to 60 seconds, and the pulse interval is set to 60 seconds.

[0039] In some embodiments, the waveform of a single pulse is at least one of a rectangular wave, a trapezoidal wave, a triangular wave, and a sine wave.

[0040] This concludes the description of the key steps of the magnetic field control method of this application. A complete magnetic field control method may also include other steps, which will not be elaborated here.

[0041] In summary, the magnetic field control method of this application applies a horizontal magnetic field to the silicon melt and controls the magnetic field strength to fluctuate periodically based on a set reference strength. This causes periodic changes in the Lorentz force on the silicon melt, which in turn induces periodic relaxation of melt convection to form a weak stirring effect. This effectively improves the heat and mass transfer conditions of the silicon melt, reduces and avoids the generation of thermal dead zones and mass transfer dead zones, prevents the local accumulation of impurities, and significantly improves the uniformity of the radial resistance and oxygen content distribution of the crystal, thereby improving the quality and yield of single crystal silicon rods.

[0042] Example 2 This application also provides a magnetic field control device. The magnetic field control device is used for Czochralski growth of single-crystal silicon and includes: a magnetic field generating component and a controller communicatively connected to the magnetic field generating component. The controller is configured to control the magnetic field generating component to apply a horizontal magnetic field to the silicon melt, and to control the magnetic field strength to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. Each single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, during which the magnetic field strength remains at the reference strength.

[0043] The magnetic field control device in this embodiment applies a horizontal magnetic field to the silicon melt by controlling the magnetic field generating component, and controls the magnetic field strength to fluctuate periodically based on a set reference strength. This causes periodic changes in the Lorentz force on the silicon melt, thereby inducing periodic relaxation of melt convection to form a weak stirring effect. This effectively improves the heat and mass transfer conditions of the silicon melt, reduces and avoids the generation of thermal dead zones and mass transfer dead zones, prevents the local accumulation of impurities, and significantly improves the uniformity of the crystal radial resistance and oxygen content distribution, thereby improving the quality and yield of single crystal silicon rods.

[0044] In some embodiments, the magnetic field generating component may be at least one of a superconducting magnet, a conventional electromagnet, or an array of permanent magnets to generate the desired magnetic field.

[0045] In some embodiments, the controller may be a programmable logic controller, an industrial control computer, a digital signal processor, or a field-programmable gate array, etc., and execute a preset control algorithm to achieve precise timing and amplitude control of the magnetic field generating component.

[0046] In some embodiments, the magnetic field generating components are typically symmetrically arranged around the vacuum chamber of a single crystal furnace or around the crucible containing the molten silicon. Control signals can be transmitted between the controller and the magnetic field generating components via wired cable, or command interaction can be performed using a wireless communication module.

[0047] In practical implementation, the periodic fluctuation of the magnetic field strength is achieved by controlling the excitation current input to the magnetic field generating component. Specifically, during crystal growth, a set reference current is input to the magnetic field generating component to excite and form a horizontal magnetic field of corresponding reference strength. To generate periodic fluctuations in the magnetic field strength in the form of pulses, the controller periodically adjusts the magnitude of the excitation current input to the magnetic field generating component according to set parameters such as pulse width, pulse interval time, and pulse amplitude. In the specific control logic, during the pulse interval time, the controller maintains the set reference current input to the magnetic field generating component, keeping the magnetic field strength at the reference strength; when entering the pulse width of a single pulse, the controller changes the magnitude of the excitation current, causing the magnetic field strength generated by the changed excitation current to deviate from the reference strength. The difference between the two values ​​corresponds to the set pulse amplitude, thereby achieving periodic fluctuations in the magnetic field strength acting on the silicon melt based on the set reference strength.

[0048] In some embodiments, the Czochralski method grows single-crystal silicon sequentially through a seeding stage, a shoulder formation stage, a constant diameter growth stage, and a finishing stage; the step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength is performed during the entire growth process of at least one of the seeding stage, the shoulder formation stage, the constant diameter growth stage, and the finishing stage, or is performed within a preset crystal length range in at least one stage.

[0049] In some embodiments, the frequency of the periodic fluctuation is from 0.003 Hz to 0.5 Hz.

[0050] In some embodiments, the absolute value of the pulse amplitude of a single pulse is 0.1% to 25% of the reference intensity.

[0051] In some embodiments, the magnetic field strength is lower than the reference strength within the pulse width of a single pulse.

[0052] In some embodiments, the pulse width of a single pulse is 1 to 120 seconds, and the pulse interval is 1 to 120 seconds.

[0053] In some embodiments, the waveform of a single pulse is at least one of a rectangular wave, a trapezoidal wave, a triangular wave, and a sine wave.

[0054] For a detailed description of the magnetic field control device, please refer to the description of the magnetic field control method in Example 1, which will not be repeated here.

[0055] Example 3 This application also provides a Czochralski single crystal furnace. The Czochralski single crystal furnace includes a furnace body, a crucible disposed within the furnace body, and a magnetic field control device. The crucible is used to contain molten silicon; the magnetic field generating component of the magnetic field control device is disposed on the outer periphery of the crucible.

[0056] The magnetic field control device can be the same as the one described in Embodiment 2, as detailed above, and will not be repeated here.

[0057] Example 4 In another aspect, this application provides a single-crystal silicon rod, which is grown using the magnetic field control method described in Example 1.

[0058] For example, in this embodiment, the diameter of the single-crystal silicon rod is 300mm, the radial resistance uniformity RRG of the single-crystal silicon rod is <8%, and the radial oxygen content uniformity ORG is <8%.

[0059] Example 5 To make the technical solutions and effects of this application clearer, the following detailed description is provided in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.

[0060] Comparative example A single-crystal silicon rod with a diameter of 300 mm was drawn using a single-crystal furnace equipped with a horizontal magnetic field. In this comparative example, a constant horizontal magnetic field with a strength of 3500 Gauss was applied to the silicon melt, and the fluctuation of the crystal diameter was controlled within ±1.0 mm during the constant diameter growth stage.

[0061] After the monocrystalline silicon rods grown from the comparative example were processed into silicon wafers, their oxygen content and electrical resistance were tested. The test results showed that up to 20% of the silicon wafers exceeded the product specification limits (e.g., product specification requirement: RRG or ORG < 8%) in terms of radial uniformity of oxygen content (ORG) or radial uniformity of electrical resistance (RRG), resulting in a low overall product yield.

[0062] Test case A single crystal silicon rod with a diameter of 300 mm was pulled using the same single crystal furnace with a horizontal magnetic field as in the comparative example. Unlike the comparative example, this test example used the magnetic field control method, magnetic field control device or Czochralski single crystal furnace provided in this application, that is, a horizontal magnetic field was applied to the silicon melt, and the magnetic field strength was controlled to produce periodic fluctuations based on a set reference strength.

[0063] In this test case, the baseline strength was set at 3500 Gauss, and based on this, the magnetic field strength produced periodic fluctuations. Each fluctuation in the periodic fluctuation corresponds to a single pulse, and the pulse amplitude of a single pulse is set to -100 Gauss, that is, the difference between the magnetic field strength and the baseline strength within the pulse width is -100 Gauss; the pulse width of a single pulse is set to 60 seconds, and the pulse interval time is set to 60 seconds.

[0064] The waveform of the magnetic field strength acting on the silicon melt is as follows Figure 2 As shown. Among them, Figure 2The horizontal axis represents time, in seconds (s); the vertical axis represents the magnetic field strength acting on the molten silicon, in gauss (GS). The horizontal dashed line in the figure represents the set reference strength, specifically 3500 gauss. The solid waveform represents the actual applied magnetic field that produces periodic fluctuations. Because the pulse amplitude is negative, the magnetic field strength appears as a periodic downward rectangular abrupt change in the macroscopic waveform. Specifically, within each fluctuation, the pulse amplitude of a single pulse is -100 gauss, causing the magnetic field strength acting on the molten silicon to decrease from 3500 gauss to 3400 gauss within the pulse width; the pulse width of a single pulse is set to 60 seconds, meaning the weakened magnetic field state of 3400 gauss is maintained for 60 seconds; then the single pulse ends, the magnetic field strength returns to the reference strength of 3500 gauss, and a pulse interval of 60 seconds begins. Each fluctuation cycle is 120 seconds, and this 120-second cycle repeats continuously, causing the magnetic field strength to periodically switch between 3500 gauss and 3400 gauss. This periodic magnetic field fluctuation causes the Lorentz force on the silicon melt to change alternately, thereby inducing a periodic weak stirring effect inside the silicon melt, which improves the radial uniformity of oxygen content and radial uniformity of electrical resistance of the grown single crystal silicon.

[0065] Furthermore, during the constant diameter growth stage, the fluctuation of the crystal diameter is also stably controlled within ±1.0 mm.

[0066] After the monocrystalline silicon rods grown from this test example were processed into silicon wafers, the same oxygen content and resistance tests were performed. The test results showed that only 2% of the silicon wafers exceeded the product specification limits (e.g., product specification requirement: RRG or ORG < 8%) in terms of radial uniformity of oxygen content or radial uniformity of resistance.

[0067] Experimental conclusions The comparison between the comparative examples and the test examples shows that, under the same crystal growth size and stringent diameter fluctuation control standards, this application significantly improves the radial uniformity of oxygen content and radial uniformity of resistance of silicon wafers by applying a horizontal magnetic field to the silicon melt and controlling the magnetic field strength to produce periodic fluctuations based on the set reference strength. This reduces the defect rate of silicon wafers from 20% to 2%, and the overall yield of the product is greatly improved.

[0068] Although exemplary embodiments have been described herein with reference to the accompanying drawings, it should be understood that the above exemplary embodiments are merely illustrative and are not intended to limit the scope of this application. Various changes and modifications can be made therein by those skilled in the art without departing from the scope and spirit of this application. All such changes and modifications are intended to be included within the scope of this application as claimed in the appended claims.

[0069] Similarly, it should be understood that, in order to simplify this application and aid in understanding one or more aspects of the application, various features of this application may sometimes be grouped together in a single embodiment, figure, or description thereof in the description of exemplary embodiments of this application. However, this approach should not be construed as reflecting an intention that the claimed application requires more features than are expressly recited in each claim. Rather, as reflected in the corresponding claims, the point of application is that the corresponding technical problem can be solved with fewer features than all of a single disclosed embodiment. Therefore, the claims following the detailed description are hereby expressly incorporated into that detailed description, wherein each claim itself is a separate embodiment of this application.

[0070] Furthermore, those skilled in the art will understand that although some embodiments described herein include certain features but not others included in other embodiments, combinations of features from different embodiments are intended to be within the scope of this application and form different embodiments. For example, in the claims, any one of the claimed embodiments can be used in any combination.

[0071] It should be noted that the above embodiments are illustrative of this application and not limiting of it, and that those skilled in the art can devise alternative embodiments without departing from the scope of the appended claims. In the claims, any reference signs placed between parentheses should not be construed as limiting the claims. The use of the words first, second, and third, etc., does not indicate any order. These words can be interpreted as names.

Claims

1. A magnetic field control method for Czochralski growth of single crystal silicon, characterized by, The magnetic field control method includes: A horizontal magnetic field is applied to the silicon melt, and the magnetic field strength is controlled to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. The single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, and the magnetic field strength remains at the reference strength during the pulse interval.

2. The magnetic field control method of claim 1, wherein, The Czochralski method for growing single-crystal silicon sequentially involves the crystal pulling stage, the shoulder formation stage, the constant diameter growth stage, and the finishing stage. The step of controlling the magnetic field strength to generate periodic fluctuations based on a set reference strength is performed during the entire growth process of at least one of the following stages: the crystal pulling stage, the shoulder forming stage, the constant diameter growth stage, and the finishing stage, or within a preset crystal length range in at least one stage.

3. The magnetic field control method of claim 1, wherein, The frequency of the periodic fluctuation is from 0.003 Hz to 0.5 Hz.

4. The magnetic field control method of claim 1, wherein, The absolute value of the pulse amplitude of the single pulse is 0.1% to 25% of the reference intensity.

5. The magnetic field control method of claim 1, wherein, Within the pulse width of the single pulse, the magnetic field strength is lower than the reference strength.

6. The magnetic field control method of claim 1, wherein, The pulse width of a single pulse is from 1 second to 120 seconds, and the pulse interval is from 1 second to 120 seconds.

7. The magnetic field control method of claim 1, wherein, The waveform of the single pulse is at least one of a rectangular wave, a trapezoidal wave, a triangular wave, and a sine wave.

8. A magnetic field control apparatus for use in the Czochralski growth of single crystal silicon, characterized by The magnetic field control device includes: Magnetic field generating component; The controller is communicatively connected to the magnetic field generating component; The controller is configured to control the magnetic field generating component to apply a horizontal magnetic field to the silicon melt, and to control the magnetic field strength to generate periodic fluctuations based on a set reference strength. The reference strength is a fixed value or varies linearly with time. Each fluctuation in the periodic fluctuation corresponds to a single pulse. The single pulse has a set pulse amplitude and a set pulse width. The pulse amplitude is the difference between the magnetic field strength and the reference strength within the pulse width. There is a pulse interval between two adjacent single pulses, and the magnetic field strength remains at the reference strength during the pulse interval.

9. A Czochralski single crystal pulling furnace characterized by comprising: The Czochralski single crystal furnace includes: Furnace body; A crucible disposed within the furnace body is used to contain molten silicon. The magnetic field control device as described in claim 8, wherein the magnetic field generating component of the magnetic field control device is disposed on the outer periphery of the crucible.

10. A single crystal silicon ingot, characterized by, The single-crystal silicon rod is grown using the magnetic field control method as described in any one of claims 1 to 7.