A polyester fiber and its preparation method

By introducing modified copolyester, modified polyurethane, grafted nanocrystals and core-shell microcapsules into polyester fibers, and utilizing core-shell composite spinning and multi-stage stretching processes, the problem of balancing the mechanical properties and biodegradability of polyester fibers has been solved, achieving high strength, high toughness and rapid biodegradability.

CN123108779APending Publication Date: 2026-11-17JIANGSU SOUTHWEST INTELLIGENT TEXTILE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611627266.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-21
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing technologies struggle to achieve rapid biodegradation while maintaining the mechanical properties of polyester fibers, limiting their application in packaging and manufacturing.

Method used

By introducing modified copolyester, modified polyurethane, grafted nanocrystals and core-shell microcapsules into polyester fibers, and utilizing skin-core composite spinning technology and multi-stage stretching process, a structure in which the skin layer wraps the core layer is formed, which synergistically improves biodegradability and mechanical properties.

Benefits of technology

This technology enables polyester fibers to maintain high strength and high toughness while significantly improving biodegradability and gas barrier properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108779A_ABST
    Figure CN123108779A_ABST
Patent Text Reader

Abstract

This invention relates to the field of polyester fiber technology, specifically to a polyester fiber and its preparation method. This invention overcomes the problem in existing technologies where the mechanical properties and biodegradability of polyester fibers cannot be simultaneously achieved. This invention obtains grafted nanocrystals by grafting cellulose nanocrystals with 4,4'-diphenylmethane diisocyanate; core-shell microcapsules are obtained using citric acid as the core layer and PVA crosslinking products as the shell layer; modified polyurethane is obtained by end-capping with epoxy resin E51; adipic acid and caprolactone are used as the matrix material for copolymer modification; and a core-sheath composite spinning technology is used to melt-blend modified copolyester chips, modified polyurethane, and grafted nanocrystals to form the sheath layer, and melt-blend polycaprolactone and core-shell microcapsules to form the core layer. The resulting polyester fiber exhibits excellent mechanical properties while also possessing significantly improved biodegradability and gas barrier properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of polyester fiber technology, specifically to a polyester fiber and its preparation method. Background Technology

[0002] Polyester fiber is the largest category of synthetic fibers. It is a fiber-forming polymer obtained from purified terephthalic acid or dimethyl terephthalate and ethylene glycol through esterification or transesterification and polycondensation reactions, and then spun and post-processed into fibers. As a semi-crystalline polymer, it is widely used in various fields such as clothing, packaging, biology, and manufacturing due to its good thermoplasticity, excellent mechanical properties, thermal stability, and chemical stability.

[0003] However, PET's inherent drawback lies in its difficulty in degradation, causing increasingly serious environmental problems. Existing technologies are also dedicated to developing polyester materials with good biodegradability. Common strategies include introducing easily degradable comonomers, adding biodegradable components, or designing multi-component composite structures. However, while improving biodegradability, the introduction of flexible segments or easily degradable components can disrupt the regularity of polymer molecular chains, reduce crystallinity, or create regions with weak mechanical properties, often resulting in a significant decrease in mechanical properties.

[0004] Therefore, achieving a balance between the mechanical and biodegradability properties of polyester fibers while maintaining other key performance characteristics is a significant challenge facing the field of polymer materials. Existing technologies often focus on improving a single property, making it difficult to achieve a balance across multiple properties, especially rapid biodegradation while maintaining high strength and toughness. The current technology for polyester fibers still suffers from the inability to simultaneously achieve both mechanical and biodegradability, limiting their further application in packaging and manufacturing.

[0005] To this end, a polyester fiber and its preparation method are proposed. Summary of the Invention

[0006] The purpose of this invention is to provide a polyester fiber and its preparation method. This invention involves grafting cellulose nanocrystals with 4,4'-diphenylmethane diisocyanate to obtain grafted nanocrystals; using citric acid as the core layer and PVA crosslinking product as the shell layer to obtain core-shell microcapsules; using epoxy resin E51 for end-capping to obtain modified polyurethane; using adipic acid and caprolactone copolymerization modification as the matrix material; and employing a core-sheath composite spinning technology, melt-blending modified copolyester chips, modified polyurethane, and grafted nanocrystals to form the sheath layer, and melt-blending polycaprolactone and core-shell microcapsules to form the core layer, followed by core-sheath composite spinning, multi-stage stretching, and heat treatment to obtain polyester fiber. The resulting polyester fiber exhibits excellent mechanical properties, while also possessing significantly improved biodegradability and gas barrier properties.

[0007] To achieve the above objectives, the present invention provides the following technical solution: This invention provides a method for preparing polyester fibers, comprising the following preparation steps: By weight, 90-100 parts of modified copolyester chips, 8-15 parts of modified polyurethane, 3-5 parts of grafted nanocrystals, 0.5 parts of antioxidant 1010, and 5 parts of dispersant are fed into a twin-screw extruder for the skin layer. The temperatures of each zone of the extruder are 190℃, 200℃, 210℃, 210℃, and 205℃, respectively, and melt-blended to obtain the skin layer melt. 70-80 parts of polycaprolactone and 20-30 parts of core-shell microcapsules are fed into a twin-screw extruder for the core layer. The temperatures of each zone of the extruder are 150℃, 160℃, 165℃, 170℃, and 160℃, respectively, and melt-blended to obtain the core layer melt. The skin layer melt and the core layer melt are then combined according to their weight... The composite fiber is fed to a sheath-core composite spinneret at a ratio of 80-90:10-20. After forming a concentric circle structure of sheath covering core within the spinneret orifice, it is extruded to obtain composite fiber. The composite fiber is then laterally cooled by an annular airflow at a temperature of 20℃ and a wind speed of 0.8m / s, and then subjected to multi-stage stretching to obtain stretched fiber. The stretched fiber is then oiled, crimped, and heat-treated at a temperature of 120-140℃ for 20-30 minutes. Finally, it is cooled and wound to obtain polyester fiber. In the multi-stage stretching process, the first stage of hot stretching is at 85℃ with a stretching ratio of 1.5 times; the second stage of hot stretching is at 115℃ with a stretching ratio of 2 times, and the total stretching ratio is 3 times. The modified copolyester is obtained by esterification polycondensation reaction of terephthalic acid, adipic acid, ethylene glycol and caprolactone. Modified polyurethane is obtained by polymerization of polycaprolactone diol and hexamethylene diisocyanate, chain extension reaction of 1,4-butanediol, and end-capping with epoxy resin. The grafted nanocrystals were prepared by grafting cellulose nanocrystals with 4,4'-diphenylmethane diisocyanate. The core-shell microcapsules were prepared by cross-linking and curing PVA to obtain the core layer from citric acid and the shell layer from PVA.

[0008] Preferably, the preparation of the modified copolyester includes the following steps: By mass fraction, terephthalic acid, adipic acid, and ethylene glycol are added to an esterification reactor in a specific ratio. Antimony acetate is added, and under nitrogen protection, the temperature is gradually raised to 240-260℃, and the reaction is carried out at atmospheric pressure for 2-3 hours to obtain the esterification product. The esterification product is then transferred to a polycondensation reactor, where triphenyl phosphate and caprolactone are added. The temperature is raised to 270-285℃, and the system is evacuated to below 50 Pa. The polycondensation reaction is carried out for 4-6 hours. When the intrinsic viscosity of the melt reaches 0.6-0.8 dL / g, the reaction is stopped, and the mixture is cooled to room temperature to obtain modified copolyester chips.

[0009] Preferably, the mass ratio of terephthalic acid to adipic acid is 50-55:35-40; the molar ratio of total acid moles to ethylene glycol is 1:1.2-1.4; the molar amount of caprolactone accounts for 3%-8% of the total acid moles; antimony acetate accounts for 0.03% of the total mass; and triphenyl phosphate accounts for 0.01% of the mass.

[0010] Preferably, the preparation of grafted nanocrystals includes the following steps: By mass fraction, cellulose nanocrystals were added to a vacuum drying oven and dried at 100℃ for 4 hours to obtain dried raw material. 10 parts of the dried raw material were added to 300 parts of N,N-dimethylformamide and sonicated for 30 minutes. Subsequently, the mixture was gradually transferred to anhydrous toluene by solvent displacement to obtain a suspension. The sonication frequency was 40-60 kHz and the sonication power was 300-500 W. 25 parts of 4,4'-diphenylmethane diisocyanate were added to anhydrous toluene and stirred to obtain a mixed solution. The suspension was transferred to a reaction vessel and heated to 50℃ under nitrogen protection. The mixed solution was slowly added dropwise to the suspension, and 0.03 parts of dibutyltin dilaurate were added. The temperature was raised to 70-80℃ for grafting reaction for 4-6 hours to obtain the reaction system. The reaction system was cooled to room temperature, centrifuged at 5000-8000 rpm for 5-10 minutes, washed 3-5 times with toluene and 3-5 times with deionized water, and dried under vacuum at 60℃ for 12 hours to obtain grafted nanocrystals.

[0011] Preferably, the preparation of core-shell microcapsules includes the following steps: Citric acid was dissolved in deionized water to prepare a 10-30% acid solution. 10 parts of PVA were added and stirred to obtain an aqueous phase. 3-5 parts of Span 80 emulsifier were added to 100 parts of liquid paraffin and stirred at 500-1500 rpm to obtain an oil phase solution. The aqueous phase was slowly added dropwise to the oil phase and stirred at high speed to obtain an emulsion. The mass ratio of the aqueous phase to the oil phase was controlled at 1:3-5. 5-10 parts of 25% glutaraldehyde aqueous solution were added to the emulsion, and the pH was adjusted to 3-4 using 10% dilute hydrochloric acid. The mixture was heated to 40-60℃ for a crosslinking reaction for 2-4 hours to obtain the reactant. The reactant was demulsified with n-hexane, washed three times with anhydrous ethanol, filtered, and vacuum dried at 40℃ for 10 hours to obtain core-shell microcapsules. The shell thickness of the microcapsules was 100-150 nm. The molar ratio of glutaraldehyde to the hydroxyl groups in PVA was 0.05-0.1:1.

[0012] Preferably, the preparation of modified polyurethane includes the following steps: By mass, polycaprolactone diol and hexamethylene diisocyanate were added to a vacuum drying oven and dried at 100°C for 4 hours. 100 parts of polycaprolactone diol (number average molecular weight 2000) and 18 parts of hexamethylene diisocyanate were added to a reaction vessel, and the temperature was raised to 80-90°C under nitrogen protection. Stannous octoate was added, accounting for 0.1% of the total mass of the reactants, and the polymerization reaction was maintained at this temperature for 2-3 hours to obtain a polyurethane prepolymer. The -NCO content was determined by titration to ensure the reaction reached the predetermined degree. The prepolymer was then cooled to... At 60-70℃, 4.1 parts of 1,4-butanediol were slowly added dropwise to the polyurethane prepolymer, and the chain extension reaction was carried out for 1-1.5 hours to obtain the reaction system; wherein the molar ratio of -NCO groups in the prepolymer to -OH groups in 1,4-butanediol was 1:0.8; 4.3 parts of epoxy resin E51 were added to the reaction system, and the temperature was raised to 90-100℃, and the end-capping reaction was carried out for 1-2 hours to obtain the modified polyurethane; wherein the molar ratio of epoxy resin E51 to the remaining -NCO was 1:1; and the molar ratio of -NCO to -OH was 2.0:1.

[0013] The present invention also provides a polyester fiber comprising a sheath melt and a core melt; the sheath melt comprises modified copolyester chips, modified polyurethane, grafted nanocrystals and additives; the core melt comprises polycaprolactone and core-shell microcapsules.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: 1. Existing technologies introduce aliphatic segments to achieve degradation, which disrupts the regularity of the polymer chain and reduces the crystallinity of the material. This invention achieves dual micro-control of regularity and flexibility by co-polymerizing adipate and caprolactone in the main chain. At the same time, modified polyurethane with alternating soft and hard segments is introduced into the skin matrix as a continuous toughening phase, and MDI-grafted cellulose nanocrystals serve as rigid reinforcing nodes. By controlling the parameters of the multi-stage hot stretching process, the composite system undergoes deformation and orientation, effectively dispersing the fracture load and achieving a simultaneous leap in strength and impact toughness.

[0015] 2. Existing technologies, when directly blending water-soluble degradation initiators, are prone to phase separation and deterioration of initial strength during spinning. Furthermore, in the early stages of composting, the rapid dissolution of hydrophilic components causes a burst release effect, resulting in the breakage of large pores in the fibers. In the middle and later stages, the catalytic process stagnates due to the loss of initiator. This invention uses microcapsules with citric acid as the core and cross-linked PVA as the shell, which are incorporated into the polycaprolactone core layer to physically block the macroscopic phase separation between the polar catalyst and the matrix. By utilizing the moisture penetration and slow dissolution mechanism of the PVA shell in the composting environment, the long-term and continuous release of citric acid is achieved, thus realizing a dual improvement in degradation efficiency and material structure disintegration uniformity.

[0016] 3. In existing technologies, to impart biodegradability to polyester, the free volume of polymer chains is increased or multi-components that are prone to phase separation are introduced, resulting in amorphous regions and interfacial micropores inside the material, shortening the gas permeation path, and reducing the oxygen and water vapor barrier performance. This invention utilizes epoxy resin E51 to end-cap modified polyurethane, causing it to crosslink in the skin layer to form a three-dimensional network structure, strongly binding the slippage of molecular chains and repairing phase interface defects. At the same time, hydrophobically modified grafted nanocrystals are uniformly dispersed in the skin layer with a high aspect ratio, increasing the diffusion path length of gas molecules inside the fiber and effectively improving the barrier performance of polyester fibers. Attached Figure Description

[0017] Figure 1 The graph shows the degradation rate of Examples 1, 5, Comparative Examples 1-3, and Comparative Examples 10-11 of the present invention over time. Detailed Implementation

[0018] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0019] Please see Figure 1 This invention provides a polyester fiber and its preparation method, the technical solution of which is as follows: Example 1 Cellulose nanocrystals were added to a vacuum drying oven and dried at 100°C for 4 hours by mass fraction to obtain dried raw material. Ten parts of the dried raw material were added to 300 parts of N,N-dimethylformamide and sonicated for 30 minutes. The mixture was then gradually transferred to anhydrous toluene via solvent displacement to obtain a suspension. The sonication frequency was 50 kHz and the sonication power was 400 W. 25 parts of 4,4'-diphenylmethane diisocyanate were added to anhydrous toluene and stirred to obtain a mixed solution. The suspension was transferred to a reaction vessel and heated to 50°C under nitrogen protection. The mixed solution was slowly added dropwise to the suspension, and 0.03 parts of dibutyltin dilaurate were added. The mixture was heated to 80°C and grafted for 5 hours to obtain a reaction system. The reaction system was cooled to room temperature, centrifuged at 6000 rpm for 10 minutes, washed three times with toluene, washed five times with deionized water, and dried under vacuum at 60°C for 12 hours to obtain grafted nanocrystals. 20 parts of citric acid were dissolved in 100 parts of deionized water to prepare a 20% acid solution. 10 parts of PVA were added and stirred to dissolve, resulting in an aqueous phase. 4 parts of Span 80 emulsifier were added to 100 parts of liquid paraffin and stirred at 800 rpm to obtain an oil phase solution. The aqueous phase was slowly added dropwise to the oil phase and stirred at high speed to obtain an emulsion. The mass ratio of the aqueous phase to the oil phase was controlled at 1:4. 8 parts of 25% glutaraldehyde aqueous solution were added to the emulsion, and the pH was adjusted to 3 using 10% dilute hydrochloric acid. The mixture was heated to 50℃ and crosslinked for 3 hours to obtain the reactant. The reactant was demulsified with n-hexane, washed three times with anhydrous ethanol, filtered, and vacuum dried at 40℃ for 10 hours to obtain core-shell microcapsules.

[0020] Polycaprolactone diol and hexamethylene diisocyanate were added to a vacuum drying oven and dried at 100°C for 4 hours. 100 parts of polycaprolactone diol (number average molecular weight 2000) and 18 parts of hexamethylene diisocyanate were added to a reaction vessel, and the mixture was heated to 80°C under nitrogen protection. Stannous octoate (0.1% of the total mass of the reactants) was added, and the polymerization reaction was maintained at this temperature for 3 hours to obtain a polyurethane prepolymer. The -NCO content was determined by titration to ensure the reaction reached the predetermined extent. The prepolymer was cooled to 60°C, and 4.1 parts of 1,4-butanediol were slowly added dropwise to the polyurethane prepolymer. The chain extension reaction was carried out for 1.5 hours to obtain the reaction system. 4.3 parts of epoxy resin E51 were added to the reaction system, and the mixture was heated to 100°C for end-capping reaction for 1 hour. The 2270 cm⁻¹ value was measured using an infrared spectrometer. -1 The characteristic absorption peak of -NCO completely disappeared, resulting in modified polyurethane.

[0021] 55 parts of terephthalic acid, 40 parts of adipic acid, and 50 parts of ethylene glycol were added to an esterification reactor in a certain proportion. 0.05 parts of antimony acetate were added. Under nitrogen protection, the temperature was gradually raised to 250°C and the reaction was carried out at normal pressure for 3 hours to obtain the esterification product. The esterification product was transferred to a polycondensation reactor, 0.02 parts of triphenyl phosphate and 3.5 parts of caprolactone were added, and the temperature was raised to 280°C. The system was evacuated to below 50 Pa and the polycondensation reaction was carried out for 5 hours. The mixture was then cooled to room temperature to obtain modified copolyester chips.

[0022] By weight, 100 parts of modified copolyester chips, 10 parts of modified polyurethane, 5 parts of grafted nanocrystals, 0.5 parts of antioxidant 1010, and 5 parts of stearic acid were fed into a twin-screw extruder for the skin layer. The temperatures of each zone of the extruder were 190℃, 200℃, 210℃, 210℃, and 205℃, respectively, for melt blending to prepare a skin layer melt. 80 parts of polycaprolactone and 20 parts of core-shell microcapsules were fed into a twin-screw extruder for the core layer. The temperatures of each zone of the extruder were 150℃, 160℃, 165℃, 170℃, and 160℃, respectively, for melt blending to prepare a core layer melt. The skin layer melt and the core layer melt were then fed into a skin layer extruder at a weight ratio of 80:20. A core-composite spinneret is used to form a concentric circle structure in the spinneret holes, which encapsulates the core layer to obtain composite fibers. The composite fibers are then laterally cooled by an annular airflow at a temperature of 20°C and a wind speed of 0.8 m / s, and then subjected to multi-stage stretching, with the first stage hot stretching temperature at 85°C, the second stage hot stretching temperature at 115°C, and a total stretching ratio of 3 times to obtain stretched fibers. The stretched fibers are then oiled, crimped, and heat-treated at 130°C for 30 minutes. Finally, they are cooled and wound to form polyester fibers.

[0023] Examples 2-4 follow the same preparation method and parameter conditions as Example 1, with differences shown in Table 1.

[0024] Table 1. Parameter variations in Examples 1-4 Example Modified copolyester chips, mass dosage / part Modified polyurethane mass dosage / part Grafted nanocrystal mass dosage / part Polycaprolactone mass dosage / part Core-shell microcapsule mass dosage / part Mass ratio of skin melt to core melt Example 1 100 10 5 80 20 80:20 Example 2 90 15 3 70 30 90:10 Example 3 100 8 4 75 25 85:15 Example 4 90 12 4 80 20 80:20 Comparative Example 1: Refer to Example 1, except that adipic acid and caprolactone were not added for modification, and conventional PET chips were used.

[0025] Comparative Example 2 is the same as Example 1, except that only adipic acid was added to modify the copolyester chips.

[0026] Comparative Example 3 is the same as Example 1, except that only caprolactone was added to modify the copolyester chips.

[0027] Comparative Example 4 is the same as Example 1, except that no modified polyurethane is added.

[0028] Comparative Example 5 is the same as Example 1, except that epoxy resin E51 is not added to the polyurethane for end-capping treatment.

[0029] Comparative Example 6 is the same as Example 1, except that no grafted nanocrystals are added.

[0030] Comparative Example 7 is the same as Example 1, except that 4,4'-diphenylmethane diisocyanate grafting modification is not used.

[0031] Comparative Example 8 is the same as Example 1, except that it does not undergo multi-stage stretching treatment, and the second-stage hot stretching temperature is directly used for stretching.

[0032] Comparative Example 9 is the same as Example 1, except that it does not undergo heat treatment.

[0033] Experimental Example 1: Mechanical Property Testing The polyester fibers prepared in Examples 1-4 and Comparative Examples 1-9 were subjected to mechanical property tests. The tensile strength and elongation at break were tested according to GB / T14344-2022. The prepared polyester fiber samples were cut into 50 mm pieces and placed under standard temperature and humidity conditions for 24 hours. The tests were then conducted using an electronic universal testing machine at a speed of 10 mm / min. The test results are shown in Table 2.

[0034] Table 2 Mechanical Performance Test Results Example Tensile strength / MPa Elongation at break / % Example 1 90.5 38.6 Example 2 90.2 38.5 Example 3 90.4 38.2 Example 4 90.1 38.4 Comparative Example 1 62.5 16.8 Comparative Example 2 75.8 22.6 Comparative Example 3 82.6 26.5 Comparative Example 4 81.8 23.2 Comparative Example 5 72.4 20.6 Comparative Example 6 68.8 37.8 Comparative Example 7 60.5 26.5 Comparative Example 8 70.2 28.4 Comparative Example 9 74.6 36.5 As shown in Table 2, the polyester fibers obtained in the comparative examples, through changes in components and processes, exhibited significantly reduced strength and toughness compared to the examples. In Comparative Examples 1-3, without the addition of adipic acid and caprolactone modification, conventional PET chips were used. The high regularity and crystallinity of the molecular chains resulted in strong intermolecular forces and difficulty in chain segment movement. Under stress, the fibers were unable to slip and extend, leading to a significant decrease in strength and toughness. The lack of flexible methylene segments introduced by caprolactone limited the overall improvement in fiber flexibility. The weak intermolecular interactions resulted in poor resistance to deformation and damage, leading to reduced mechanical properties. The absence of adipic acid prevented sufficient disruption of the original molecular chain regularity, hindering effective crystallinity control. During stretching, localized stress concentration easily occurred in the molecular chains, further reducing overall mechanical properties. In Comparative Example 4, without modified polyurethane, the fiber system lacked a phase that could effectively disperse stress and absorb impact energy. Under external force, stress could not be effectively dispersed, easily leading to cracks that propagated rapidly, resulting in reduced strength and toughness. In Example 5, the lack of reaction between epoxy resin E51 and polyurethane prepolymer to form a cross-linked structure resulted in polyurethane existing mainly in a linear structure with weak intermolecular forces, leading to reduced mechanical properties. Comparative Examples 6-7 show that grafted nanocrystals possess high specific surface area and good mechanical properties, forming a good interfacial bond with the polyester matrix and providing reinforcement. Without grafted nanocrystals, the fiber lacks a reinforcing phase, failing to effectively share stress and resulting in decreased tensile strength. Without grafting modification, the polar groups on the nanocrystal surface have poor compatibility with the polyester matrix, easily leading to agglomeration. These agglomerates become internal defects, acting as stress concentration points under stress, thus reducing mechanical properties. In Comparative Examples 8-9, the process change significantly impacted mechanical properties. Direct stretching at the second-stage hot stretching temperature forced the molecular chains to stretch before they could arrange themselves in an orderly manner, resulting in uneven molecular chain orientation, imperfect crystal structure, and numerous internal defects within the fiber. Furthermore, without heat treatment, the residual internal stress within the fiber becomes a crack source under stress, reducing the fiber's strength and toughness.

[0035] In summary, by introducing adipic acid copolymerization and caprolactone copolymerization, the crystallization behavior and chain segment flexibility of polyester are adjusted. The addition of adipic acid can disrupt the regularity of the molecular chain, while caprolactone introduces flexible chain segments. The synergistic effect of the two can improve the strength and toughness of polyester. At the same time, the introduction of modified polyurethane utilizes the soft and hard segment structures. The soft segments provide flexibility, while the hard segments provide rigidity and strength, forming a reinforcing and toughening phase in polyester fibers, thereby improving the mechanical properties of the fibers. Cellulose nanocrystals have the characteristics of high strength, high modulus, and high specific surface area, which can provide a large number of stress transfer points and effectively disperse the load. Furthermore, MDI grafting modification can improve compatibility with the polymer matrix, reduce agglomeration, and be introduced into the skin layer as a nano-reinforcing filler, which can significantly improve the mechanical properties of the fibers. During the preparation process, multi-stage stretching helps the polymer molecular chain orientation and crystallization, improving the strength and modulus of the fibers. Heat treatment stabilizes the fiber structure, eliminates internal stress, improves dimensional stability, and promotes perfect crystallization. Through the synergy of multiple components and processes, the overall mechanical properties of the fibers are further improved.

[0036] Examples 5-8 follow the same preparation method and parameter conditions as Example 1, with differences shown in Table 3.

[0037] Table 3 Parameter changes in Examples 1 and 5-8 Example Citric acid solution mass concentration / % 80 parts by weight / serving Mass parts of glutaraldehyde aqueous solution Mass ratio of aqueous phase to oil phase Crosslinking reaction temperature / ℃ Crosslinking reaction time / h Example 1 20 4 8 1:4 50 3 Example 5 10 3 5 1:5 40 4 Example 6 30 5 10 1:5 60 2 Example 7 20 3 5 1:4 40 4 Example 8 20 5 10 1:4 60 3 Comparative Example 10 is the same as Example 1, except that no core-shell microcapsules were added, while the other components remained unchanged.

[0038] Comparative Example 11 is the same as Example 1, except that no core-shell microcapsules are introduced, and citric acid and polycaprolactone are used directly as the core layer.

[0039] Comparative Example 12 is the same as Example 1, except that the core-shell microcapsule is used as the core layer and polycaprolactone is not used in the blend.

[0040] Comparative Example 13 is the same as Example 1, except that a core-sheath structure is not introduced, and polyester fibers are obtained by direct melt blending and spinning.

[0041] Experiment Example 2: Biodegradability Test The polyester fibers prepared in Examples 1, 5-8, Comparative Examples 1-3, and Comparative Examples 10-13 were subjected to biodegradability tests. Following the test method of GB / T 19277.1-2011, the samples were placed in a composting environment with a temperature of 58℃ and a humidity of 50-55% to test the biodegradability rate. The degradation rates were tested at 30d, 60d, 120d, and 180d, respectively. The test results are shown in Table 4. The degradation rate of Examples 1, 5, Comparative Examples 1-3, and Comparative Examples 10-11 over time is shown in the graph. Figure 1 As shown.

[0042] Table 4 Biodegradability Test

[0043] Through Table 4, Figure 1 The results show that, compared to the examples, the polyester fibers obtained by changing the components and processes in the comparative examples exhibit a significantly lower biodegradability rate. Comparative Examples 1-3 show that the terephthalic acid and ethylene glycol structural units in conventional PET are regularly arranged, with high crystallinity, making it difficult for microorganisms to adhere to and decompose them. The branched structure of adipic acid can disrupt the regularity of the molecular chain, and the flexible segments of caprolactone can reduce crystallinity. The carboxyl groups of adipic acid and the ester groups of caprolactone can serve as action sites for microbial enzymes, improving the biodegradation of the matrix material by microorganisms and increasing the degradation rate. The absence of methylene segments in caprolactone increases the number of chain segments. The material's flexibility makes it difficult for molecular chain movement to expose more ester sites in a composting environment, hindering microbial degradation. The lack of adipic acid to regulate the carboxyl group ratio in the esterification reaction leads to a wider molecular weight distribution in the copolyester. The high molecular weight portion, due to its tight chain entanglement, makes it difficult for microorganisms to penetrate the fiber matrix, reducing the degradation rate. Comparative Examples 10-11 show that both the PVA shell and polycaprolactone dispersion in the core-shell microcapsules are easily degradable components. The released citric acid promotes microbial metabolism, and the aliphatic ester bonds of polycaprolactone are easily attacked by lipases. Without the core layer, which consists only of polycaprolactone, the degradation rate depends on a single component. Without the catalytic properties of citric acid, the degradation rate decreases. Furthermore, the shell of the core-shell microcapsule can delay the release of citric acid from the core layer. However, in direct blending, the high melting temperature causes a large amount of citric acid to decompose during melt spinning, resulting in a lack of effective catalytic degradation during biodegradation and a lower degradation rate. Simultaneously, citric acid without a shell protection easily separates from polycaprolactone, forming pores and defects. While this accelerates moisture penetration, it leads to premature loss of material mechanical properties, uneven degradation, and affects the overall performance of the fiber. In Comparative Examples 12-13, only microcapsules are used as the core layer, lacking polycaprolactone... Esters improve compatibility and provide protection, but microcapsules tend to form aggregates with high internal porosity but small effective degradation area, making it difficult for microorganisms to penetrate and affecting degradation performance. When directly blended, easily degradable components are randomly dispersed in the melt, forming local enrichment zones, leading to inconsistent degradation rates. In addition, in direct melt blending, citric acid molecules are highly polar and tend to aggregate, causing phase separation in the polycaprolactone melt, which reduces its effective catalytic contact area. Furthermore, the lack of a shell coating leads to rapid loss of moisture in the early stages of degradation, causing subsequent catalytic degradation to stagnate, reducing catalytic efficiency, and further affecting overall degradation performance.

[0044] In summary, firstly, the introduction of adipic acid and caprolactone units into the fiber matrix facilitates hydrolysis or enzymatic degradation of ester bonds in a biological environment. Furthermore, in a composting environment, molecular chain movement exposes more ester sites and microbial attachment sites, improving the biodegradability of polyester fibers. Secondly, the introduction of core-shell microcapsules, mixed with polycaprolactone to form a core layer, serves two purposes. Firstly, the synergistic effect of the shell layer and polycaprolactone delays the release of citric acid from the core layer, preventing rapid dissolution and reduced catalytic effect. Secondly, the protective effect of the shell layer and polycaprolactone improves the compatibility between citric acid and the matrix, preventing poor interfacial compatibility that could lead to core-sheath separation and affect the overall fiber performance. Finally, the introduction of the core-sheath structure, through layered spinning, achieves a gradient design with a degradation-resistant outer layer and a degradation-friendly inner layer, avoiding inconsistent degradation rates. Additionally, the formation of an amorphous, interlocking crystalline structure further enhances the fiber's mechanical properties. Through the synergistic effect of multiple components and the coordination of the processing procedures, the overall performance of the fiber is improved.

[0045] Examples 9-11 follow the preparation method and parameter conditions of Example 1, with differences shown in Table 5.

[0046] Table 5 Parameter changes in Examples 1 and 9-11 Example Grafting reaction temperature / ℃ Grafting reaction time / h Polymerization reaction temperature / °C Polymerization reaction time / h End-capping reaction temperature / ℃ End capping reaction time / h Example 1 80 5 80 3 100 1 Example 9 70 6 90 2 90 2 Example 10 80 4 80 2 100 1 Example 11 80 6 90 3 100 2 Experiment Example 3 Barrier Performance Test The polyester fibers prepared in Examples 1, 9-11, Comparative Examples 1, 4-7, and 13 were subjected to barrier performance tests. The oxygen permeability was tested according to GB / T 1038-2022, and the water vapor permeability was tested according to GB / T 1037-2021. The test results are shown in Table 6.

[0047] Table 6 Barrier performance test results Example Oxygen permeability / cm³ / (m²・d) Water vapor transmission rate / g / (m²・d) Example 1 12.6 6.8 Example 9 12.5 6.2 Example 10 12.4 6.5 Example 11 12.2 6.3 Comparative Example 1 25.4 18.2 Comparative Example 4 20.8 12.5 Comparative Example 5 24.6 13.6 Comparative Example 6 25.8 14.5 Comparative Example 7 32.6 21.6 Comparative Example 13 21.2 12.2 As shown in Table 6, the polyester fibers obtained in the comparative examples, through changes in components and processes, exhibited significantly reduced barrier properties compared to the examples. Comparative Example 1 shows that conventional PET molecular chains are highly regular and crystallinity-rich, inherently hindering molecular permeation. The addition of adipic acid and caprolactone utilizes the hydrogen bonds formed by the carboxyl groups of adipic acid and the ester groups of caprolactone with water molecules, slowing water vapor diffusion and reducing the fiber's water vapor permeability. In Comparative Examples 4-5, the lack of modified polyurethane resulted in increased gaps between copolyester molecular chains in the cortex, straightening the gas permeation path and facilitating gas molecules' entry into the fiber structure. Furthermore, the absence of hydrogen bonding between polyurethane and the copolyester matrix increased the number of phase interfaces within the cortex, creating weak points for gas permeation. Simultaneously, without epoxy resin end-capping, an effective cross-linked three-dimensional network structure could not be formed, restricting molecular chain movement. The uncapped polyurethane exhibited a predominantly linear structure, with inter-chain... In a large free volume, gases easily diffuse; unreacted -NCO groups readily react with moisture in the environment to generate carbon dioxide bubbles, forming micron-sized pores in the cortex, which become rapid permeation channels for oxygen and water vapor, reducing overall barrier performance; in Comparative Examples 6-7, after being modified with isocyanate, the grafted nanocrystals are uniformly dispersed in the cortex in a lamellar form, creating a tortuous path effect. Without isocyanate, the cortex is a homogeneous copolyester, with a short and direct gas diffusion path, making it easier for gas molecules to enter the fiber interior; the hydroxyl groups on the surface of the ungrafted nanocrystals have poor compatibility with the copolyester matrix, easily agglomerating to form porous structures, becoming permeation defects, which facilitate gas permeation and reduce barrier performance; in Comparative Example 13, during direct blending, easily degradable components are randomly dispersed, resulting in polycaprolactone-rich areas in the fiber. Its low crystallinity and large interstitial molecular chains easily become weak areas for oxygen and water vapor permeation, facilitating gas entry and thus reducing barrier performance.

[0048] In summary, by modifying the polyester matrix, which inherently possesses good barrier properties, the introduction of adipic acid branched structures disrupts the regularity of the molecular chains, reduces crystallinity, and decreases the occurrence of permeation channels caused by crystalline defects. The flexible segments of caprolactone fill the voids in the amorphous regions, resulting in tighter molecular chain packing, extended gas diffusion paths, and improved barrier performance. Furthermore, modified polyurethane, as the skin layer component, allows its hard segments to fill the gaps between copolyester molecular chains, while its soft segments enhance intermolecular forces through flexible winding, forming a dense barrier layer. Finally, the epoxy resin end-capping creates a three-dimensional network structure that improves the overall mechanical properties of the fiber. While increasing the number of hydrogen bonding sites, reducing interfacial compatibility within the cortex, and improving overall barrier performance, 4,4'-diphenylmethane diisocyanate grafting can coat the nanocrystal surface with hydrophobic phenyl groups, reducing surface energy and improving dispersion uniformity in the melt, avoiding agglomeration that leads to increased internal porosity. After grafting, the nanocrystals and copolyester form a molecular-level composite, and the layered structure can hinder the diffusion of gas molecules, further improving gas barrier performance. Through the synergistic effect of multiple components and multiple mechanisms, the mechanical properties of the fiber material are improved while maintaining good gas barrier performance.

[0049] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A method for preparing polyester fiber, characterized in that, The preparation process includes the following steps: melt extrusion of modified copolyester chips, modified polyurethane, grafted nanocrystals, and additives to obtain a skin melt; melt extrusion of polycaprolactone and core-shell microcapsules to obtain a core melt; spin extrusion of the skin melt and the core melt to obtain composite fibers; cooling by blowing and multi-stage stretching to obtain stretched fibers; oiling, heat treatment, cooling, and winding of the stretched fibers to obtain the polyester fibers; the modified copolyester chips are obtained from terephthalic acid, adipic acid, ethylene glycol, and caprolactone through an esterification polycondensation reaction. The modified polyurethane is obtained by polymerizing and extending the chain of polycaprolactone diol and hexamethylene diisocyanate, followed by epoxy resin end capping; the grafted nanocrystals are prepared by grafting cellulose nanocrystals with 4,4'-diphenylmethane diisocyanate; and the core-shell microcapsules are prepared by cross-linking and curing citric acid as the core layer and PVA as the shell layer.

2. The method for preparing polyester fiber according to claim 1, characterized in that, The preparation of the modified copolyester chips includes the following steps: The terephthalic acid, adipic acid, and ethylene glycol were added to an esterification reactor, and antimony acetate was added. Under nitrogen protection, the esterification reaction was carried out at atmospheric pressure to obtain the esterification product. The esterification product was transferred to a polycondensation reactor, and triphenyl phosphate and caprolactone were added. The polycondensation reaction was carried out under vacuum, and the product was cooled to obtain the modified copolyester chips.

3. The method for preparing polyester fiber according to claim 1, characterized in that, The preparation of the grafted nanocrystals includes the following steps: vacuum drying the cellulose nanocrystals to obtain a dried raw material; adding the dried raw material to anhydrous toluene and ultrasonically treating it to obtain a suspension; adding the 4,4'-diphenylmethane diisocyanate to anhydrous toluene and stirring to obtain a mixed solution; transferring the suspension to a reaction vessel, adding the mixed solution dropwise to the suspension under nitrogen protection, adding dibutyltin dilaurate, and performing a grafting reaction to obtain a reaction system; cooling the reaction system to room temperature, separating and centrifuging, washing with toluene and deionized water alternately, and vacuum drying to obtain the grafted nanocrystals.

4. The method for preparing polyester fiber according to claim 1, characterized in that, The preparation of the core-shell microcapsules includes the following steps: dissolving citric acid in deionized water to prepare an acid solution with a mass concentration of 10-30%, then adding the PVA and stirring to dissolve it to obtain an aqueous phase; adding 3-5 parts of emulsifier Span 80 to liquid paraffin and stirring at high speed to obtain an oil phase; slowly adding the aqueous phase dropwise to the oil phase and stirring at high speed to obtain an emulsion; adding 5-10 parts of glutaraldehyde aqueous solution to the emulsion, adjusting the pH to acidic using dilute hydrochloric acid, and performing a crosslinking reaction to obtain a reactant; demulsifying the reactant, washing it with anhydrous ethanol, filtering and vacuum drying to obtain the core-shell microcapsules.

5. The method for preparing polyester fiber according to claim 1, characterized in that, The preparation of the modified polyurethane includes the following steps: The polycaprolactone diol and hexamethylene diisocyanate were added to a reaction vessel, heated under nitrogen protection, and stannous octoate was added to polymerize and obtain a polyurethane prepolymer. 1,4-Butanediol was added to the polyurethane prepolymer to conduct a chain extension reaction to obtain a reaction system. The epoxy resin was added to the reaction system to conduct an end-capping reaction to obtain the modified polyurethane.

6. The method for preparing polyester fiber according to claim 1, characterized in that, The preparation of the skin melt and the core melt includes the following steps: feeding 90-100 parts of the modified copolyester chips, 8-15 parts of the modified polyurethane, 3-5 parts of the grafted nanocrystals, antioxidant 1010 and stearic acid into a twin-screw extruder for skin layering, and performing melt blending to obtain the skin melt; feeding 70-80 parts of the polycaprolactone and 20-30 parts of the core-shell microcapsules into a twin-screw extruder for core layering, and performing melt blending to obtain the core melt.

7. A polyester fiber, characterized in that: The polyester fiber comprises a sheath melt and a core melt; the sheath melt comprises modified copolyester chips, modified polyurethane, grafted nanocrystals, and additives; the core melt comprises polycaprolactone and core-shell microcapsules; the polyester fiber is prepared by the preparation method according to any one of claims 1-6.