An antistatic agent for high-speed spinning of spandex, its preparation method and application

By combining a phosphate-based anionic silicone antistatic agent with a nonionic surfactant, the problem of poor antistatic performance of spandex spinning oil in high and low humidity environments was solved, the storage stability of the oil and the conductivity of the fiber were enhanced, and it is suitable for the industrial production of spandex spinning.

CN123108783APending Publication Date: 2026-11-17SHANDONG DAYI CHEM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611609855.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-19
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing spandex spinning oils have shortcomings in antistatic properties, making it difficult to maintain good performance in both high and low humidity environments. Furthermore, the oil film is prone to migration, resulting in poor storage stability, and they lack synergistic effects with other oil components.

Method used

A phosphate-type anionic organosilicon antistatic agent is compounded with a nonionic surfactant. Long-chain alkyl and epoxy groups are introduced into the polysiloxane backbone through hydrosilylation and ring-opening esterification reactions to form a phosphate structure, which enhances affinity and compatibility. Combined with the nonionic surfactant, a dense conductive layer is formed.

Benefits of technology

It achieves the durability and stability of antistatic agents under different humidity environments, reduces the coefficient of friction, improves the feel of fibers, and has a simple preparation method, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108783A_ABST
    Figure CN123108783A_ABST
Patent Text Reader

Abstract

This invention belongs to the field of organosilicon technology, specifically relating to an antistatic agent for high-speed spandex spinning, its preparation method, and its application. To address the lack of existing antistatic agents that simultaneously achieve durable antistatic performance, excellent system compatibility, simple dispersion processes, and synergistic compatibility with other components of the oiling agent, this invention provides an antistatic agent for high-speed spandex spinning, comprising a phosphate-type anionic organosilicon antistatic agent and a nonionic surfactant. The phosphate-type anionic organosilicon antistatic agent has a polysiloxane backbone, to which long-chain alkyl side chains and epoxy-containing side chains are connected via hydrosilylation. The epoxy groups in the epoxy-containing side chains undergo ring-opening esterification with a phosphorylating agent to form phosphate ester groups, which are then salted to form a phosphate structure. The antistatic agent of this invention exhibits excellent thermal stability, good system compatibility, and a controllable failure mode, making it suitable for high-speed spandex spinning processes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to an antistatic agent for high-speed spinning of spandex, its preparation method and application, belonging to the field of organosilicon technology. Background Technology

[0002] Spandex, with its excellent elastic recovery rate, is widely used in various elastic textiles such as underwear, sportswear, bodybuilding wear, swimwear, high-elastic stockings, and compression garments. In the spinning and processing of spandex, spinning oils play a crucial role in comprehensive regulation. Their main functions include reducing the fiber surface friction coefficient to minimize mechanical damage, preventing fuzzing and tangling caused by static electricity accumulation, and improving fiber bundle properties for efficient winding and subsequent textile processing. In recent years, with the continuous upgrading of consumer market requirements for the functionality and quality of textiles, spandex spinning oils have also faced higher performance requirements.

[0003] Antistatic agents are the core functional components in spandex spinning oils used to eliminate static electricity hazards. Their function is to inhibit the accumulation of static electricity caused by high-speed friction during spinning and weaving, preventing fibers from repelling each other due to like charges or adsorbing environmental dust, thereby ensuring spinnability and the stability of the final product quality. Based on the type of ion, existing antistatic agents can be divided into four main categories: cationic, anionic, amphoteric, and nonionic. However, although commercially available spandex oils have made some breakthroughs in lubrication, shaping, and unwinding properties, they generally suffer from insufficient antistatic performance, making it difficult to effectively solve static interference in subsequent weaving processes.

[0004] To address the aforementioned issues, researchers have attempted various improvement solutions. For example, oiling agents formulated with mineral oil, silicone oil, and amino-modified silicone oil can maintain the smooth feel of spandex yarn, but these systems lack highly efficient antistatic components, resulting in poor actual antistatic effects. Other solutions utilize quaternary ammonium salt cationic surfactants as antistatic agents, which offer some improvement but still cannot fully meet the rapid static dissipation requirements of weaving operations. Furthermore, existing oiling agents reveal another significant problem in practical applications: when spandex yarn cakes are stored for more than three months, the oil film gradually migrates from the bottom to the surface, leading to a significant difference in unwinding performance between the surface and interior of the yarn cake, and a substantial decrease in antistatic effect with storage time.

[0005] Among various antistatic agents, anionic antistatic agents have unique advantages: they maintain good static dissipation ability under low-temperature and dry conditions, remain stable in high-humidity environments, and possess excellent electrolyte compatibility. They can maintain long-term stable dispersion in complex oil-based systems, making them a relatively balanced formulation choice. However, existing anionic antistatic agent solutions still have many shortcomings. For example, while some anionic antistatic oil-based formulations can meet basic antistatic indicators, the components such as higher fatty acid metal salts contained in these formulations require relatively stringent dispersion conditions, and their antistatic performance easily degrades with prolonged use and storage. Some studies have also directly added a mixture of polydimethylsiloxane and phosphate as an antistatic component to the spinning solution. Although this method imparts antistatic properties to the finished fiber, it requires large quantities of raw materials, involves complex processes, and has high overall costs, hindering industrial adoption. It should be noted that most antistatic agents currently only have a single antistatic function and lack synergistic design with other necessary components in the oil (such as smoothers, clustering agents, and release agents). It is difficult to achieve antistatic properties while ensuring the stability and long-lasting effect of the overall oil formulation.

[0006] With the industry trend of spandex oil agents accelerating towards functionalization and differentiation, the market urgently needs an antistatic agent solution that can take into account long-lasting antistatic performance, excellent system compatibility, simple dispersion process, and synergistic matching ability with other components of the oil agent, in order to break through existing technical bottlenecks and meet the manufacturing requirements of high-end spandex products. Summary of the Invention

[0007] To address the aforementioned deficiencies in the prior art, this invention provides an antistatic agent for high-speed spinning of spandex, its preparation method, and its application.

[0008] The technical solution of the present invention to solve the above-mentioned technical problems is as follows: One of the objectives of this invention is to provide an antistatic agent for high-speed spinning of spandex, which comprises a phosphate-type anionic organosilicon antistatic agent and a nonionic surfactant. The phosphate-type anionic organosilicon antistatic agent has a polysiloxane backbone, on which long-chain alkyl side chains and epoxy-containing side chains are connected by hydrosilylation reaction. The epoxy group in the side chain containing the epoxy group is ring-opening esterified by a phosphorylating agent to form a phosphate ester group, and the phosphate ester group is then salted to form a phosphate structure.

[0009] Furthermore, the long-chain alkyl side chain originates from the hydrosilylation reaction of the long-chain olefin with the silane-hydrogen bond on the polysiloxane backbone; the epoxy-containing side chain originates from the hydrosilylation reaction of the epoxy compound with double bond with the silane-hydrogen bond on the polysiloxane backbone.

[0010] Furthermore, the nonionic surfactant is selected from one or more of fatty alcohol polyoxyethylene ether, cashew phenol polyoxyethylene ether, and isomeric tridecyl alcohol polyoxyethylene ether.

[0011] Furthermore, the mass ratio of the phosphate-type anionic organosilicon antistatic agent to the nonionic surfactant is 1-10:1-10.

[0012] The second objective of this invention is to provide a method for preparing the antistatic agent for high-speed spinning of spandex as described above, comprising the following steps: S1. Hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane are subjected to a ring-opening copolymerization reaction in the presence of a catalyst to obtain hydrogen-containing silicone oil. S2. The hydrogen-containing silicone oil obtained in step S1 is subjected to a hydrosilylation reaction with long-chain olefins and epoxy compounds with double bonds in the presence of a platinum catalyst to obtain a long-chain alkane and epoxy co-modified silicone oil. S3. The long-chain alkane obtained in step S2 is subjected to ring-opening esterification reaction with epoxy co-modified silicone oil and phosphorylation reagent, and then washed with water to obtain phosphate ester modified silicone oil. S4. The phosphate-modified silicone oil obtained in step S3 is neutralized with an alkaline solution and dehydrated to obtain a phosphate-type anionic organosilicon antistatic agent. S5. Mix the phosphate-type anionic organosilicon antistatic agent obtained in step S4 with a nonionic surfactant until homogeneous to obtain the antistatic agent for high-speed spinning of spandex.

[0013] Furthermore, in step S1: The mass ratio of hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane is 1-8:1-100:1-200. The catalyst is selected from any one or more of trifluoromethanesulfonic acid, acidic cation exchange resin, sulfuric acid, sulfonic acid, and acidic clay, and the amount of the catalyst used is 0.1% to 20% of the total mass of hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane. The reaction temperature in step S1 is 20℃~100℃, and the reaction time is 2 hours~10 hours.

[0014] Furthermore, in step S2: The mass ratio of the hydrogen-containing silicone oil to the long-chain olefin and the epoxy compound with double bonds is 1-7:1-20:1-40; the long-chain olefin is a C3-C30 straight-chain olefin. The epoxy compound with double bonds is any one of allyl epoxy polyether, allyl glycidyl ether, glycidyl methacrylate, and 1,2-epoxy-4-vinylcyclohexane. The platinum-based catalyst is selected from any one or more of Karstedt catalysts, Speier catalysts, and supported platinum catalysts. The amount of platinum-based catalyst added is 1 ppm to 10 ppm of the total mass of hydrogen-containing silicone oil, long-chain olefins, and epoxy compounds with double bonds. The reaction temperature in step S2 is 50℃~130℃, and the reaction time is 2 hours~10 hours.

[0015] Furthermore, in step S3: The mass ratio of the long-chain alkane and epoxy co-modified silicone oil to the phosphorylation reagent is 1-50:1; The phosphorylation reagent is one or more of phosphoric acid, phosphorus pentoxide, and polyphosphoric acid; The reaction temperature in step S3 is 10℃~120℃, and the reaction time is 1 hour~10 hours; The water washing is repeated 1 to 2 times until the pH value of the washing solution is 4 to 5.

[0016] Furthermore, in step S4: The alkaline solution is any one of potassium hydroxide aqueous solution, sodium hydroxide aqueous solution, or triethylamine solution, with a concentration of 5wt% to 20wt%. Neutralize to pH 6-7, then dehydrate under vacuum at a vacuum level of -0.1MPa to -0.01MPa and a dehydration temperature of 80℃ to 120℃. In step S5: the mixing temperature is 40℃~80℃, the mixing and stirring time is 30min~120min, until the system is a homogeneous and transparent liquid, then stop heating, continue stirring and cooling until the temperature is ≤40℃.

[0017] A third objective of this invention is to provide a spandex spinning oil, which comprises the antistatic agent for high-speed spandex spinning as described above, or comprises the antistatic agent for high-speed spandex spinning prepared by the preparation method described above.

[0018] Compared with the prior art, the present invention has the following beneficial effects: This invention covalently links long-chain alkyl groups to the polysiloxane backbone. The introduction of long-chain alkyl groups significantly enhances the affinity between the antistatic agent and components such as mineral oil and white oil in the oiling agent, enabling the antistatic agent to achieve uniform dispersion at the molecular level in the oiling agent system. This avoids common problems of layering, oil drift, and precipitation in traditional antistatic agents, thereby giving the spandex oiling agent excellent long-term storage stability.

[0019] This invention covalently links phosphate groups to the polysiloxane backbone via an epoxy ring-opening esterification reaction, solving the problems of poor compatibility, easy migration, and insufficient durability of antistatic agents. At the same time, the newly generated hydroxyl groups in the ring-opening reaction can further enhance hydrophilicity, which is beneficial to forming a continuous conductive film on the fiber surface and improving the durability of the antistatic effect.

[0020] This invention employs a phosphate-based anionic silicone antistatic agent combined with a nonionic surfactant. The anionic antistatic agent maintains good antistatic performance even in low-temperature, dry environments, overcoming the high humidity dependence of amphoteric antistatic agents. Furthermore, the anionic agent is compatible with the anionic emulsifier system commonly found in spandex oils, and unlike cationic antistatic agents, it does not undergo charge neutralization and precipitation reactions. The combination of anionic and nonionic agents forms a denser conductive surface layer, significantly reducing the surface resistance of the material. The anionic component enhances the hygroscopicity of the nonionic component, allowing the system to maintain good performance even in low-humidity environments, making it insensitive to humidity changes and adaptable to various processing environments. In addition, the two components synergistically reduce the coefficient of friction and improve fiber hand feel.

[0021] The antistatic agent of this invention exhibits excellent stability under high-temperature thermal storage conditions. Furthermore, the antistatic agent remains clear and transparent after 20 repeated freeze-thaw cycles, demonstrating significantly superior freeze-thaw stability compared to existing cationic products.

[0022] The preparation method of the antistatic agent for high-speed spinning of spandex of the present invention is simple, the reaction conditions of each step are mild, no complicated post-processing is required, the raw materials are widely available and inexpensive, and while ensuring product performance, it achieves low-cost and high-efficiency production, which is suitable for large-scale industrial application. Attached Figure Description

[0023] Figure 1 The infrared spectrum of the product obtained in Example 1 is shown below. Detailed Implementation

[0024] The principles and features of the present invention are described below. The examples given are only for explaining the present invention and are not intended to limit the scope of the present invention.

[0025] Unless otherwise specified, the methods used in this invention are conventional methods; the raw materials and apparatus used are conventional commercially available products unless otherwise specified.

[0026] This invention provides an antistatic agent for high-speed spinning of spandex, which comprises a phosphate-type anionic organosilicon antistatic agent and a nonionic surfactant, wherein the mass ratio of the phosphate-type anionic organosilicon antistatic agent to the nonionic surfactant is 1-10:1-10. The phosphate-type anionic organosilicon antistatic agent has a polysiloxane backbone, on which long-chain alkyl side chains and side chains containing epoxy groups are covalently connected by hydrosilylation reaction. The epoxy group undergoes a ring-opening esterification reaction and reacts with a phosphorylation reagent to form a phosphate monoester group or a phosphate diester group; the phosphate monoester group or the phosphate diester group further forms a salt to form a phosphate structure.

[0027] The long-chain alkyl side chain originates from the hydrosilylation reaction of the long-chain olefin with the silane-hydrogen bond on the polysiloxane backbone; the side chain containing the epoxy group originates from the hydrosilylation reaction of the epoxy compound with the double bond with the silane-hydrogen bond on the polysiloxane backbone.

[0028] Its preparation method includes the following steps: S1. Preparation of hydrogen-containing silicone oil: Hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane are added to a reactor in a mass ratio of 1–8:1–100:1–200. Under nitrogen protection, stirring is started, and a catalyst is added. The mass of the catalyst is 0.1%–20% of the total mass of hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane. Heating is started to raise the temperature of the liquid in the reactor to 20°C–100°C, and the reaction is continued with stirring for 2–10 hours to carry out ring-opening copolymerization, thus obtaining hydrogen-containing silicone oil.

[0029] S2. Preparation of long-chain alkanes and epoxy co-modified silicone oil: The hydrogen-containing silicone oil, long-chain olefins, and epoxy compounds with double bonds obtained in step S1 are added to a reaction vessel. The mass ratio of hydrogen-containing silicone oil to long-chain olefins and epoxy compounds with double bonds is 1-7:1-20:1-40. A vacuum is drawn and replaced with nitrogen to a vacuum level of -0.1 MPa to -0.01 MPa. Stirring and heating are started to raise the liquid temperature in the reaction vessel to 20℃-100℃. A platinum-based catalyst is added at a rate of 1 ppm to 10 ppm of the total amount of hydrogen-containing silicone oil, long-chain olefins, and epoxy compounds with double bonds. The temperature is raised to 50℃-130℃, and the reaction is continuously stirred for 2-10 hours until no residual hydrogen-containing silicone oil remains. Vacuum dehydration is performed and replaced with nitrogen gas at a vacuum level of -0.1 MPa to -0.01 MPa. Stirring and heating are then started to raise the temperature of the liquid in the reactor to 80°C to 120°C. Water is removed until no more droplets fall back. After cooling, anhydrous long-chain alkane and epoxy co-modified silicone oil is obtained.

[0030] S3. Preparation of Phosphate-Modified Silicone Oil: The long-chain alkane and epoxy co-modified silicone oil obtained in step S2 is added to a reaction vessel, and a phosphorylation reagent is slowly added. The mass ratio of the long-chain alkane and epoxy co-modified silicone oil to the phosphorylation reagent is 1–50:1. The reaction is carried out at a controlled temperature of 10℃–120℃ for 1–10 hours. Afterward, the reaction solution is slowly poured into ice water, and the mixture is stirred thoroughly to hydrolyze and dissolve the unreacted phosphorylation reagent into the aqueous phase. After standing and separating the layers, the lower wastewater layer is separated. The washing is repeated 1–2 times until the pH of the washing solution is 4–5, yielding the organic phase phosphate-modified silicone oil.

[0031] S4. Preparation of phosphate-type anionic organosilicon antistatic agent: A base solution with a concentration of 5 wt%–20 wt% is slowly added dropwise to the organic phase from step S3, and the pH is adjusted to 6–7. Vacuum dehydration is performed, followed by nitrogen purging to a vacuum degree of -0.1 MPa to -0.01 MPa. Stirring and heating are then started to raise the liquid temperature in the reactor to 80℃–120℃. Water is removed until no more droplets fall back, and the mixture is cooled to obtain the phosphate-type anionic organosilicon antistatic agent.

[0032] S5. Preparation of antistatic agent for high-speed spinning of spandex: Add the phosphate-type anionic silicone antistatic agent and nonionic surfactant from step S4 to the reaction vessel, start stirring and heating, and raise the temperature of the liquid in the reaction vessel to 40℃~80℃. Mix and stir for 30min~120min until the system is a homogeneous and transparent liquid. Stop heating, continue stirring and cooling until the temperature is ≤40℃ to obtain the antistatic agent for high-speed spinning of spandex. The mass ratio of phosphate-type anionic silicone antistatic agent to nonionic surfactant is 1~50:1~50.

[0033] The structural formula of the hydrogen-containing silicone oil obtained in step S1 is shown in formula (Ⅰ):

[0034] (I); In equation (Ⅰ), 3≤n≤200, and the value of n includes but is not limited to positive integers; 0<m≤60, and the value of m includes but is not limited to positive integers.

[0035] The double-bonded epoxy compound added in step S2 is any one of allyl epoxy polyether, allyl glycidyl ether, glycidyl methacrylate, and 1,2-epoxy-4-vinylcyclohexane. The structural formula of the allyl epoxy polyether is shown in formula (II) below:

[0036] (II); In equation (II), 0 ≤ a ≤ 20, and the value of a includes but is not limited to positive integers; 0 ≤ b ≤ 20, and the value of b includes but is not limited to positive integers.

[0037] The long-chain olefin added in step S2 is a C3-C30 straight-chain olefin; the structural formula of the long-chain olefin is shown in formula (Ⅲ) below:

[0038] (III); In equation (Ⅲ), 0 < c < 30, and the value of c is an odd number.

[0039] The phosphorylation reagent mentioned in step S3 is one or more of phosphoric acid, phosphorus pentoxide, and polyphosphoric acid; wherein, the structural formula of polyphosphoric acid is shown in formula (Ⅳ) below:

[0040] (Ⅳ); In equation (Ⅳ), 0 ≤ d ≤ 100, and the value of d is a positive integer.

[0041] The alkaline solution mentioned in step S4 is any one of potassium hydroxide aqueous solution, sodium hydroxide aqueous solution, or triethylamine solution.

[0042] The nonionic surfactant in step S5 is selected from one or more of fatty alcohol polyoxyethylene ether, cashew phenol polyoxyethylene ether, and isomeric tridecyl alcohol polyoxyethylene ether.

[0043] Example 1 A method for preparing an antistatic agent for high-speed spinning of spandex includes the following steps: (1) Preparation of hydrogen-containing silicone oil: 13.88g of hexamethyldisiloxane, 63g of tetramethyltetrahydrocyclotetrasiloxane, and 223.12g of octamethylcyclotetrasiloxane were added to the reactor. Under nitrogen protection, stirring was started, and 9g of sulfonic acid macroporous acidic cation exchange resin with a styrene-divinylbenzene copolymer backbone (crosslinking degree 8%, wet apparent density 0.75g / mL~0.85g / mL, total exchange capacity ≥4.2mmol / g, soaked in 1mol / L hydrochloric acid for 4h, washed with deionized water until neutral, and vacuum dried at 60℃ for 12h) was added. Heating was started to raise the temperature of the liquid in the reactor to 60℃, and the reaction was stirred continuously for 10 hours to carry out ring-opening copolymerization and obtain hydrogen-containing silicone oil.

[0044] (2) Preparation of long-chain alkanes and epoxy co-modified silicone oil: 100g of hydrogen-containing silicone oil obtained in step (1), 68.9g of hexadecene and 147.2g of allyl epoxy polyether (molecular weight of 1000) were added to the reactor, vacuumed and replaced with nitrogen gas, the vacuum degree was -0.08MPa, stirring and heating were turned on, and the liquid temperature in the reactor was raised to 30℃. 4ppm of Karstedt catalyst (CAS: 68478-92-2, i.e. platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex) was added, the temperature was raised to 90℃ and stirring was continued for 7 hours until there was no residual hydrogen-containing silicone oil (confirmed by the disappearance of the Si-H characteristic absorption peak by infrared spectroscopy). Vacuum dehydration was performed and replaced with nitrogen gas at a vacuum level of -0.09 MPa. Stirring and heating were then started to raise the temperature of the liquid in the reactor to 110°C. Water was removed until no more droplets fell back. After cooling, anhydrous long-chain alkane and epoxy co-modified silicone oil was obtained.

[0045] (3) Preparation of phosphate-modified silicone oil: 230g of the long-chain alkane and epoxy co-modified silicone oil obtained in step (2) was added to a reaction vessel, and 24.13g of tetrapolyphosphoric acid was slowly added. The reaction was carried out at 75℃ for 4 hours. Afterward, the reaction solution was slowly poured into ice water and stirred thoroughly to hydrolyze and dissolve the unreacted phosphorylation reagent into the aqueous phase. After standing and separating the layers, the lower wastewater was separated. The washing was repeated twice until the pH of the washing solution was 5, and the crude product of organic phase phosphate-modified silicone oil was obtained.

[0046] (4) Preparation of phosphate-type anionic organosilicon antistatic agent: Slowly add 5wt% sodium hydroxide aqueous solution to the organic phase in step (3) and adjust the pH to 7. Vacuum dehydration is carried out and replaced with nitrogen gas at a vacuum degree of -0.09MPa. Stirring and heating are started to raise the temperature of the liquid in the reactor to 110℃. Water is removed until no liquid droplets fall back. Cooling is performed to obtain phosphate-type anionic organosilicon antistatic agent.

[0047] (5) Preparation of antistatic agent for high-speed spandex spinning: The phosphate-type anionic silicone antistatic agent from step (4) and cashew phenol polyoxyethylene ether BGF-3 were added to the reactor. Stirring and heating were started to raise the liquid temperature in the reactor to 50°C. Stirring was carried out for 120 minutes until the system became a homogeneous and transparent liquid. Heating was stopped, and stirring was continued to cool to 35°C to obtain the antistatic agent for high-speed spandex spinning. The mass ratio of phosphate-type anionic silicone antistatic agent to nonionic surfactant was 1:1.

[0048] The infrared spectrum of the product is shown below. Figure 1 ,from Figure 1 It can be known that: 3500cm -1 The broad absorption peak is enhanced, which is attributed to the stretching vibration of -OH, originating from the hydroxyl group formed by ring opening of the epoxy group and the phosphate ester P-OH.

[0049] 2954cm -1 2924cm -1 2856cm -1 All three peaks are strong absorption peaks, which are attributed to the asymmetric stretching vibration of -CH3 and the asymmetric and symmetric stretching vibrations of -CH2- in the alkyl chain, respectively, indicating the presence of long-chain alkyl groups and aliphatic structures in the connecting chains in the product.

[0050] 1467cm -1 1408cm -1 The absorption peaks mainly originate from the shear bending vibration of -CH2 and the asymmetric bending vibration of -CH3.

[0051] 1350cm -1 The -CH2- is an out-of-plane rocking vibration, a characteristic absorption of long-chain alkyl or polyether segments.

[0052] 1260cm -1 The strong absorption peak at 1200 cm⁻¹ is characteristically attributed to the symmetric bending vibration of Si-CH₂ in siloxanes; simultaneously, the P=O stretching vibration of phosphate esters also appears at 1200 cm⁻¹. -1 -1300cm -1 The interval is such that the signals of Si-CH3 and P=O at this location may overlap.

[0053] 1000cm -1 -1100cm -1 The region is a strong and broad absorption band, mainly corresponding to the asymmetric stretching vibration of Si-O-Si, which is a typical feature of the polysiloxane backbone. This region may also contain stretching vibrations of COC (ether bond) and POC, but due to the extremely high signal intensity of Si-O-Si, the other absorption peaks are masked by it.

[0054] 909cm -1 The characteristic peak at 953 cm⁻¹ disappears, and at the same time... -1 The presence of stretching vibrations at the point of origin, which are attributed to POC, indicates that the epoxy underwent ring opening and formed a POC structure.

[0055] 842cm -1 The absorption peak at that point may originate from the rocking vibration of Si-CH or the bending vibration of Si-O-Si.

[0056] 803cm -1 The strong absorption peak is usually attributed to the symmetric stretching vibration of Si-O-Si or the stretching vibration of Si-C.

[0057] Example 2 A method for preparing an antistatic agent for high-speed spinning of spandex includes the following steps: (1) Preparation of hydrogen-containing silicone oil: 19.44g of hexamethyldisiloxane, 45g of tetramethyltetrahydrocyclotetrasiloxane, and 235.56g of octamethylcyclotetrasiloxane were added to a reaction vessel. Under nitrogen protection, stirring was started, and 7.5g of acid clay (the acid clay is bentonite activated with sulfuric acid, with an activity ≥180, free acid ≤0.20%, and moisture ≤8.0%, and dried and activated at 105℃ for 4h before use) was added. Heating was started to raise the temperature of the liquid in the reaction vessel to 80℃, and the reaction was stirred continuously for 9 hours to carry out ring-opening copolymerization and obtain hydrogen-containing silicone oil.

[0058] (2) Preparation of long-chain alkane and epoxy co-modified silicone oil: 100g of hydrogen-containing silicone oil obtained in step (1), 45g of dodecene and 85.71g of allyl epoxy polyether (molecular weight 800) were added to the reactor. Vacuum was drawn and replaced with nitrogen to a vacuum degree of -0.09MPa. Stirring and heating were started to raise the liquid temperature in the reactor to 30℃. 5ppm of Karstedt catalyst (CAS: 68478-92-2, i.e., platinum(0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex) was added. The temperature was raised to 95℃ and the reaction was stirred continuously for 5 hours until no residual hydrogen-containing silicone oil was found. Vacuum was drawn to remove water and replaced with nitrogen to a vacuum degree of -0.08MPa. Stirring and heating were started to raise the liquid temperature in the reactor to 110℃. Water was removed until no droplets fell back. The mixture was cooled to obtain anhydrous long-chain alkane and epoxy co-modified silicone oil.

[0059] (3) Preparation of phosphate-modified silicone oil: 200g of the long-chain alkane and epoxy co-modified silicone oil obtained in step (2) was added to a reaction vessel, and 11g of phosphorus pentoxide was slowly added. The reaction was carried out at 65℃ for 3 hours. After that, the reaction solution was slowly poured into ice water and stirred thoroughly to hydrolyze and dissolve the unreacted phosphorus pentoxide into the aqueous phase. After standing and separating the layers, the lower wastewater was separated. The washing was repeated twice until the pH of the washing solution was 4, and the crude product of organic phase phosphate-modified silicone oil was obtained.

[0060] (4) Preparation of phosphate-type anionic organosilicon antistatic agent: Slowly add 10wt% sodium hydroxide aqueous solution to the organic phase in step (3) and adjust the pH to 7. Vacuum dehydration is carried out and replaced with nitrogen gas at a vacuum degree of -0.08MPa. Stirring and heating are started to raise the temperature of the liquid in the reactor to 110℃. Water is removed until no liquid droplets fall back. Cooling is performed to obtain phosphate-type anionic organosilicon antistatic agent.

[0061] (5) Preparation of antistatic agent for high-speed spandex spinning: The phosphate-type anionic silicone antistatic agent from step (4) and isomeric tridecyl alcohol polyoxyethylene ether 1304 were added to a reaction vessel. Stirring and heating were started to raise the liquid temperature in the reaction vessel to 65°C. Stirring was continued for 40 minutes until the system became a homogeneous and transparent liquid. Heating was stopped, and stirring was continued to cool to 40°C to obtain the antistatic agent for high-speed spandex spinning. The mass ratio of phosphate-type anionic silicone antistatic agent to nonionic surfactant was 4:1.

[0062] Example 3 A method for preparing an antistatic agent for high-speed spinning of spandex includes the following steps: (1) Preparation of hydrogen-containing silicone oil: 12.15g of hexamethyldisiloxane, 90g of tetramethyltetrahydrocyclotetrasiloxane, and 197.85g of octamethylcyclotetrasiloxane were added to a reaction vessel. Under nitrogen protection, stirring was started, 5.4g of sulfuric acid was added, and heating was started to raise the temperature of the liquid in the reaction vessel to 50°C. The reaction was carried out by stirring for 7 hours to carry out ring-opening copolymerization and obtain hydrogen-containing silicone oil.

[0063] (2) Preparation of long-chain alkanes and epoxy co-modified silicone oil: 100g of hydrogen-containing silicone oil obtained in step (1), 68.6g of tetradecene and 210g of allyl epoxy polyether (molecular weight 600) were added to the reactor, vacuumed and replaced with nitrogen to a vacuum degree of -0.08MPa, stirring and heating were started to raise the temperature of the liquid in the reactor to 40℃, 3ppm of Karstedt catalyst (CAS: 68478-92-2, i.e. platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex) was added, the temperature was raised to 100℃, and the reaction was stirred continuously for 5 hours until there was no residual hydrogen-containing silicone oil. Vacuum dehydration was performed, followed by nitrogen purging to a vacuum level of -0.08 MPa. Stirring and heating were then initiated to raise the temperature of the liquid in the reactor to 110°C. Water was removed until no more droplets fell back down. After cooling, anhydrous long-chain alkane and epoxy co-modified silicone oil was obtained.

[0064] (3) Preparation of phosphate-modified silicone oil: 250g of the long-chain alkane and epoxy co-modified silicone oil obtained in step (2) was added to a reaction vessel, and 22.65g of phosphoric acid was slowly added. The reaction was carried out at 55℃ for 6 hours. Afterward, the reaction solution was slowly poured into ice water and stirred thoroughly to hydrolyze and dissolve the unreacted phosphoric acid into the aqueous phase. After standing and separating the layers, the lower wastewater was separated. The washing was repeated twice until the pH of the washing solution was 4, and the crude product of organic phase phosphate-modified silicone oil was obtained.

[0065] (4) Preparation of phosphate-type anionic organosilicon antistatic agent: Slowly add 8wt% sodium hydroxide aqueous solution to the organic phase in step (3) and adjust the pH to 7. Vacuum dehydration is carried out and replaced with nitrogen gas at a vacuum degree of -0.08MPa. Stirring and heating are started to raise the temperature of the liquid in the reactor to 110℃. Water is removed until no liquid droplets fall back. Cooling is performed to obtain phosphate-type anionic organosilicon antistatic agent.

[0066] (5) Preparation of antistatic agent for high-speed spandex spinning: The phosphate-type anionic silicone antistatic agent from step (4) and fatty alcohol polyoxyethylene ether AEO-3 were added to a reaction vessel. Stirring and heating were started to raise the liquid temperature in the reaction vessel to 60°C. Stirring was continued for 60 min until the system became a homogeneous and transparent liquid. Heating was stopped, and stirring was continued to cool to 40°C to obtain the antistatic agent for high-speed spandex spinning. The mass ratio of phosphate-type anionic silicone antistatic agent to nonionic surfactant was 2:1.

[0067] Example 4 A method for preparing an antistatic agent for high-speed spinning of spandex includes the following steps: (1) Preparation of hydrogen-containing silicone oil: 48.6g of hexamethyldisiloxane, 54g of tetramethyltetrahydrocyclotetrasiloxane, and 197.4g of octamethylcyclotetrasiloxane were added to a reaction vessel. Under nitrogen protection, stirring was started, 2.4g of trifluoromethanesulfonic acid was added, and heating was started to raise the temperature of the liquid in the reaction vessel to 60°C. The reaction was carried out by stirring for 8 hours to carry out ring-opening copolymerization and obtain hydrogen-containing silicone oil.

[0068] (2) Preparation of long-chain alkane and epoxy co-modified silicone oil: 100g of hydrogen-containing silicone oil obtained in step (1), 65g of hexadecene and 80g of allyl epoxy polyether (molecular weight 800) were added to the reactor. The reactor was evacuated and replaced with nitrogen to a vacuum degree of -0.07MPa. Stirring and heating were started to raise the liquid temperature in the reactor to 40℃. 6ppm of Karstedt catalyst (CAS: 68478-92-2, i.e., platinum (0)-1,3-diethylene-1,1,3,3-tetramethyldisiloxane complex) was added. The temperature was raised to 80℃ and the reaction was stirred continuously for 7 hours until no residual hydrogen-containing silicone oil was found. The reactor was then dehydrated under vacuum and replaced with nitrogen to a vacuum degree of -0.07MPa. Stirring and heating were started to raise the liquid temperature in the reactor to 110℃. Water was removed until no droplets fell back. The reactor was then cooled to obtain anhydrous long-chain alkane and epoxy co-modified silicone oil.

[0069] (3) Preparation of phosphate-modified silicone oil: 200g of the long-chain alkane and epoxy co-modified silicone oil obtained in step (2) was added to a reaction vessel, and 12g of phosphorus pentoxide was slowly added. The reaction was carried out at 50℃ for 6 hours. After that, the reaction solution was slowly poured into ice water and stirred thoroughly to hydrolyze and dissolve the unreacted phosphorylation reagent into the aqueous phase. After standing and separating the layers, the lower wastewater was separated. The washing was repeated twice until the pH of the washing solution was 5, and the crude product of organic phase phosphate-modified silicone oil was obtained.

[0070] (4) Preparation of phosphate-type anionic organosilicon antistatic agent: Slowly add 6wt% sodium hydroxide aqueous solution to the organic phase in step (3) and adjust the pH to 7. Vacuum dehydration is carried out and replaced with nitrogen gas at a vacuum degree of -0.07MPa. Stirring and heating are started to raise the temperature of the liquid in the reactor to 110℃. Water is removed until no liquid droplets fall back. Cooling is performed to obtain phosphate-type anionic organosilicon antistatic agent.

[0071] (5) Preparation of antistatic agent for high-speed spandex spinning: The phosphate-type anionic silicone antistatic agent from step (4) and fatty alcohol polyoxyethylene ether AEO-9 were added to a reaction vessel. Stirring and heating were started to raise the liquid temperature in the reaction vessel to 55°C. Stirring was continued for 90 min until the system became a homogeneous and transparent liquid. Heating was stopped, and stirring was continued to cool to 35°C to obtain the antistatic agent for high-speed spandex spinning. The mass ratio of phosphate-type anionic silicone antistatic agent to nonionic surfactant was 3:1.

[0072] Comparative Example 1 This comparative example provides a method for preparing a sulfonate betaine-type organosilicon zwitterionic antistatic agent, comprising the following steps: (1) Preparation of polymethylhydrosiloxane: 30.6g of tetramethyltetrahydrocyclotetrasiloxane, 103.2g of octamethylcyclotetrasiloxane and 16.2g of hexamethyldisiloxane were added to the reactor. Under nitrogen protection, stirring and heating were started to raise the temperature of the liquid in the reactor to 50°C. 3g of trifluoromethanesulfonic acid was added and the reaction was stirred continuously for 8 hours to carry out ring-opening copolymerization to obtain polymethylhydrosiloxane. (2) Preparation of long-chain alkane and epoxy co-modified silicone oil: 100g of polymethylhydrosiloxane obtained in step (1), 80g of allyl epoxy polyether (molecular weight of 1000) and 60g of n-hexadecene were added to the reactor, vacuumed and dehydrated, and replaced with nitrogen gas with a vacuum degree of -0.08MPa. Stirring and heating were started to raise the liquid temperature in the reactor to 50°C. 3ppm of platinum tetrachloride catalyst was added and the temperature was raised to 100°C. The reaction was stirred for 3 hours until there was no residual polymethylhydrosiloxane, and long-chain alkane and epoxy co-modified silicone oil was obtained. (3) Preparation of amino-modified silicone oil: 210g of long-chain alkane and epoxy co-modified silicone oil obtained in step (2) and 21g of N-methyl-D-glucosamine were added into the reaction vessel, and then 25g of toluene was added. Under nitrogen protection, the liquid temperature in the reaction vessel was raised to 50°C, and stirring was started at the same time. The reaction was kept at the temperature for 6 hours to carry out the ring-opening reaction and obtain amino-modified silicone oil. (4) Add 231g of amino-modified silicone oil and 17.7g of 1,4-butylsulfonate lactone obtained in step (3) into the reactor. Under nitrogen protection, turn on the stirring and heating to raise the temperature of the liquid in the reactor to 60°C. Stir and keep the reaction for 10 hours. After cooling, the crude antistatic agent for high-speed spinning of spandex is obtained. (5) Distillation to remove impurities: The crude product obtained in step (4) is subjected to vacuum distillation at a temperature of 150°C and a vacuum of -0.09 MPa to remove unreacted raw materials and solvents until no droplets fall back. After cooling, orange-red transparent organosilicon zwitterionic antistatic agent is obtained.

[0073] Comparative Example 2 The difference between this comparative example and Example 2 is as follows: In this comparative example, step (2) is changed to prepare epoxy-modified silicone oil, that is, dodecylene is not added, and the amount of allyl epoxy polyether (molecular weight of 800) added is adjusted to 280g. In step (3) of this comparative example, the amount of phosphorus pentoxide added was adjusted to 21.8g.

[0074] The remaining operations are the same as in Example 2, and will not be repeated here.

[0075] Comparative Example 3 This comparative example provides a quaternary ammonium salt cationic antistatic agent, which includes the following steps: (1) Preparation of epoxy siloxane polymer: 400g of hydrogen-containing siloxane polymer (0.25% hydrogen content) and 228g of allyl epoxy polyether (m=0) were added to the reactor. The nitrogen gas was purged three times and stirred and heated to raise the liquid temperature in the reactor to 85°C. Pt catalyst (2ppm based on Pt) was added and the temperature was raised to 100°C. The reaction was stirred for 2 hours until there was no residual hydrogen-containing siloxane polymer. (2) Distillation to remove impurities: The mixture obtained in step (1) is subjected to vacuum distillation at a temperature of 140°C and a pressure of 65 mmHg to remove unreacted raw materials and impurities until no droplets fall back. After cooling, a light yellow and transparent epoxy siloxane polymer is obtained. (3) Preparation of organic acid quaternary ammonium salt solution: 200g of lauric acid was added to the reaction vessel, and then 413g of ethylene glycol butyl ether was added. Under the protection of nitrogen, the temperature of the liquid in the reaction vessel was raised to 50°C. At the same time, stirring was started to completely dissolve and mix the liquid in the reaction vessel. The stirring time was 1 hour. The temperature was further increased to control the temperature of the liquid in the reaction vessel to 60°C. 213g of dodecyl dimethyl tertiary amine was added dropwise to the reaction vessel. The dropwise addition time was 1.5 hours. After the dropwise addition was completed, the mixture was stirred and kept warm for 1 hour. (4) Add 514g of the epoxy siloxane polymer obtained in step (2) into a reactor containing 826g of the organic acid quaternary ammonium salt solution obtained in step (3). Under the protection of nitrogen, start stirring and heating to raise the temperature of the liquid in the reactor to 100°C. Stir and keep the reaction at the temperature for 10 hours until there is no residual epoxy siloxane polymer. After cooling, the quaternary ammonium salt cationic antistatic agent is finally obtained.

[0076] Performance testing The antistatic agents prepared in Examples 1-4 and Comparative Examples 1-3 were added at a mass ratio of 1% to the basic formulation of spandex oil (a mixture of white oil and dimethicone oil in a mass ratio of 1:1) without antistatic agents, and the following performance tests were performed.

[0077] I. Long-term storage stability test Equal amounts of the spandex oil agents from Examples 1-4 and Comparative Examples 1-3 were placed under the same conditions for 60 days, 120 days, and 180 days. The appearance changes of the spandex oil agents and whether there were any precipitates were observed. The results are shown in Table 1. Table 1. Long-term storage stability results of each embodiment and comparative example group.

[0078] Comparing the test results in Table 1, it can be seen that Examples 1-4 remained transparent and showed no precipitation after 180 days of standing, while Comparative Example 2 (without added long-chain olefins) showed precipitation after 60 days of standing. This demonstrates that long-chain alkyl groups play a crucial role in improving the compatibility and dispersion stability of the antistatic agent with mineral oil. Comparative Example 3 (cationic type) showed precipitation after 120 days, indicating that the anionic antistatic agent prepared in this invention has better long-term storage stability than the cationic type, is well compatible with white oil and silicone oil, and can be uniformly and stably dispersed in oil-based systems.

[0079] II. Thermal Storage Stability and Failure Mode Testing To test the thermal storage stability and failure mode of the antistatic agent for high-speed spinning of spandex prepared in this invention under different working conditions, the following four sets of parallel accelerated aging experiments were designed.

[0080] Group A (Conventional Heat Storage Conditions): Equal amounts of spandex oil from Examples 1-4 and Comparative Examples 1-3 were placed in glass bottles. The bottle caps were tightened and then turned back 1 / 3 turn (to prevent gas expansion). The bottles were then sealed with sealing film and placed in a constant temperature oven at 50℃±0.5℃, away from the air vents. The sample spacing was ≥3cm. The bottles were continuously heat-stored for 7 days without adding any additional water or acid / alkali adjusters. These conditions were used to simulate the conventional aging process of spandex oil under anhydrous, constant temperature storage conditions.

[0081] Group B (Damp Heat Fluctuation): Take equal amounts of spandex oil agents from Examples 1-4 and Comparative Examples 1-3, add 0.5% deionized water (by total mass of the oil agent) to each, stir thoroughly until evenly dispersed, then place in glass bottles. Tighten the caps and turn them back 1 / 3 turn (to prevent gas expansion), wrap with sealing film, and place in a constant temperature oven at 50℃±0.5℃, avoiding the air outlet, with a sample spacing ≥3cm, for continuous heat storage for 7 days. This condition is used to simulate the aging process of circulating oil agents after being exposed to trace amounts of moisture due to environmental humidity or spinning moisture regain during use.

[0082] Group C (Acid Fluctuation): Take equal amounts of spandex oils from Examples 1-4 and Comparative Examples 1-3, add 0.3% of the total oil mass of deionized water to each, and add glacial acetic acid dropwise to adjust the pH of the system to 5.0±0.1. Stir thoroughly until evenly dispersed, then place in a glass bottle, tighten the cap and turn it 1 / 3 turn (to prevent gas expansion), wrap with sealing film, and place in a constant temperature oven at 50℃±0.5℃, avoiding the air outlet, with a sample spacing ≥3cm, for continuous heat storage for 7 days. This condition is used to simulate the extreme working conditions of acidic aging of the oil due to oxidative decomposition or the introduction of external contaminants during long-term cyclic use.

[0083] Group D (Alkaline Fluctuation): Take equal amounts of spandex oiling agents from Examples 1-4 and Comparative Examples 1-3, add 0.3% deionized water (by total oiling agent mass) to each, and add triethanolamine dropwise to adjust the pH of the system to 9.0±0.1. Stir thoroughly until evenly dispersed, then place in a glass bottle, tighten the cap and turn it 1 / 3 turn (to prevent gas expansion), wrap with sealing film, and place in a constant temperature oven at 50℃±0.5℃, avoiding the air outlet, with a sample spacing ≥3cm, for continuous heat storage for 7 days. This condition is used to simulate the alkalization of circulating oiling agents caused by alkaline degreasing agent residue in the downstream processing of spandex fibers.

[0084] Starting from day 0, samples were taken once a day at a set time. After sampling, the samples were allowed to cool naturally to 25℃±0.5℃, and the following tests were conducted immediately.

[0085] Appearance record: Observe and record the appearance of the sample on day 7, including whether there is turbidity, flocculation, layering or sticking to the wall.

[0086] Oil phase conductivity determination: Samples were taken at each time point, and the conductivity of each sample was measured using a conductivity meter under constant temperature conditions of 25℃±0.5℃. The conductivity was recorded as K(t). The conductivity retention rate η(t) was calculated based on the value of day 0 K(0) = [K(t) / K(0)]×100%. Judgment criteria: η(t)≥90% indicates excellent antistatic performance; η(t)<70% is judged as significant performance degradation.

[0087] Centrifugal sedimentation (V, vol%) determination: Take 10 mL of sample at each time point, place it in a graduated centrifuge tube, centrifuge at 3000 r / min for 15 min, and read the volume fraction of the precipitate or stratified matter at the bottom, recording it as V(t). Judgment criterion: When the centrifugal sedimentation V(t) first exceeds 2.0 vol%, it indicates that irreversible macroscopic phase separation has occurred in the oil system, and the effective concentration of the antistatic agent has dropped to a level that cannot guarantee processing quality.

[0088] Sedimentation Mutation Index (SMI): SMI(t) = |V(t) - V(t-1)| / V(t-1), representing the rate of change in sedimentation volume between two consecutive days, i.e., the increase in the volume of centrifuged sediment on day t and day t-1. Judgment Criteria: When SMI(t) > 1.5, the system is considered to have experienced a sudden phase separation mutation at that time point, corresponding to the failure mode: sudden drop type; if SMI(t) ≤ 1.5 throughout the process, the system's sedimentation process is considered to have a gradual and controllable increase, corresponding to the failure mode: progressively controllable type. It should be noted that when V(t) approaches 0, the calculated value of SMI(t) may be abnormally amplified. This situation only occurs in the initial stage when the system has almost no sedimentation. Therefore, this test stipulates that SMI(t) is only included in the statistics when V(t) ≥ 0.2 vol% and V(t-1) ≥ 0.2 vol%; otherwise, it is assigned a value of 0, considered as baseline fluctuation.

[0089] Failure warning criteria: During the 7-day damp heat fluctuation aging test, if a sample exhibits any of the following conditions, it is deemed to have experienced a sudden failure warning: (a) The conductivity retention rate η(t) first falls below 75%; (b) The centrifugal sedimentation volume V(t) exceeds 2.0% (volume fraction) for the first time; (c) Precipitation mutation index SMI(t) > 1.5.

[0090] If none of the three conditions are triggered within the 7-day thermal storage period, the failure mode of the sample is determined to be: progressively controllable; if any one condition is triggered within 7 days, it is determined to be: sudden drop failure mode.

[0091] The test results are shown in Table 2: Table 2. Thermal storage stability results of each embodiment and comparative example group

[0092] As shown in Table 2, under the conditions of groups A, B, C, and D in Examples 1-4 of the present invention, the 7-day centrifugal sedimentation amount V(7) was ≤0.5 vol%, the conductivity retention rate η(7) was ≥90.9%, the maximum sedimentation change rate SMI(max) between adjacent days was ≤0.3, and the appearance remained uniform and transparent. None of the three indicators triggered a failure warning, and it was determined to be a progressively controllable failure mode. In contrast, under the conditions of group B, Comparative Example 1 (zwitterion) had V(7) of 4.4 vol% and η(7) of 69.3%. Under acid / alkaline conditions, it further deteriorated to V(7) of 5.6 vol% to 6.6 vol% and η(7) of 53.6% to 57.9%, with SMI(max) reaching 1.54, and a large number of defects appeared on the appearance. Flocculent suspended matter and bottom sediment were observed. Comparative Example 2 showed V(7) of 6.7 vol% and η(7) of 56.4% under Group B conditions, and further deteriorated to V(7) of 7.2 vol%–7.9 vol% and η(7) of 49.5%–52.5% under acid / alkaline conditions, with an SMI(max) of 1.46. The appearance showed obvious turbidity and a bottom sediment layer. Comparative Example 3 (cation) showed V(7) of 9.1 vol% and η(7) of 45.1% under Group B conditions, and further deteriorated to V(7) of 9.5 vol%–10.5 vol% and η(7) of 39.3%–42.9% under acid / alkaline conditions, with an SMI(max) of 2.26. The appearance showed severe stratification and blocky sediment. Each comparative example triggered at least one failure warning under both Group B and acid / alkaline conditions, and was judged to be a sudden drop type failure mode. The above results demonstrate that the anionic-nonionic composite system of this invention, through the formation of a thermodynamically stable mixed micelle structure, exhibits excellent tolerance to trace moisture, acidic and alkaline pH fluctuations, and its failure mode is progressively controllable, significantly superior to existing ionic antistatic agent systems. However, not all organosilicon anionic antistatic agents with arbitrary structures can achieve the technical effects of this invention. Comparative Example 2, without the addition of dodecene, showed significantly deteriorated thermal storage stability and system compatibility compared to Example 2.

[0093] III. Freeze-thaw stability test Equal amounts of spandex oil agents from Examples 1-4 and Comparative Examples 1-3 were placed in a sealed container and frozen at -20°C for 20 hours. After freezing, they were allowed to thaw naturally at a constant temperature of 25°C for 4 hours. This constitutes one freeze-thaw cycle. The above operation was repeated 20 times. The sample condition was observed at room temperature after the 0th, 10th, and 20th freeze-thaw cycles, and the results are shown in Table 3. Table 3 Freeze-thaw stability results of each embodiment and comparative example group

[0094] As shown in Table 3, Examples 1-4 and Comparative Example 1 exhibit excellent freeze-thaw stability, remaining clear and transparent after 20 freeze-thaw cycles. This demonstrates that the oil agent of the present invention possesses excellent freeze-thaw resistance and can adapt to long-term storage and transportation under extreme climates. In contrast, Comparative Example 2 (without added long-chain olefins) shows poor compatibility in the spandex oil agent system, resulting in a significant imbalance in freeze-thaw stability. Comparative Example 3 (cationic type) also exhibits slightly worse freeze-thaw stability compared to the present invention, becoming cloudy after 20 freeze-thaw cycles, indicating that the antistatic agent prepared by the present invention has better freeze-thaw stability.

[0095] IV. Performance Testing of Spandex Spinning Applications Application experiments were conducted on the spandex oils (containing different antistatic agents) of Examples 1-4 and Comparative Examples 1-3, with the spandex yarn denier fixed at 40D and the oil adhesion amount at 4.0%. The specific experimental testing methods are as follows: Determination of the static friction coefficient of fibers: Referring to the fixed yarn winch method in ASTM D3412 / D3412M-13 (2020) "Standard Test Method for Coefficient of Friction of Yarn to Yarn", after equilibrating the sample under standard atmospheric conditions (temperature 20℃±2℃, relative humidity 65%±5%), the spandex yarn to be tested was wound around the surface of a yarn tube with a diameter of 50±5mm at a tension of 11±1mN / tex as a fixed yarn body. A single strand of the same yarn was wrapped around the yarn tube at a wrap angle of 180°. The input tension was set to 10.0±0.5mN / tex and the running speed was 100mm / min. After the speed stabilized, the static friction coefficient was directly read by the tester. Each sample was tested 5 times and the arithmetic mean was taken.

[0096] Determination of the coefficient of friction between metals: Refer to ASTM D3108 / D3108M-13 (2020), "Standard Test Method for Coefficient of Friction of Yarn to Solid Material". Test conditions: wrap angle 180°, running speed 100 m / min, input tension 9.8 mN / tex, and the friction surface is a 12.7 mm diameter chrome-faced cylindrical pin. The yarn was conditioned in standard atmosphere before testing, and the coefficient of friction value was read directly from the instrument.

[0097] Resistance (×10) 9 Ω): The test was conducted in accordance with FZ / T 50035-2016 "Test Method for Resistance of Synthetic Fiber Filaments". A high resistance meter was used, and the resistance value was read after equilibration under the conditions of temperature (20±2)℃ and humidity (65±5)%.

[0098] Elastic elongation determination: Referring to the test principle of FZ / T 50007-2012 "Test Method for Elasticity of Spandex Filament", under the conditions of temperature 20℃±2℃ and relative humidity 65%±5%, the spandex filament sample is placed on a constant speed elongation type tensile tester with a clamping distance of 50mm and a pre-tension of (0.01±0.001)cN / tex. The sample is stretched at a speed of 500mm / min until it breaks. The elongation at the time of break is recorded as the elastic elongation. Each sample is tested 5 times and the arithmetic mean is taken.

[0099] Static electricity generation (V): Referring to the principle of the triboelectric voltage method in GB / T 12703.2-2021, the sample is rubbed against the standard cloth at a speed of 50 m / min, and the maximum voltage value is measured at a distance of 1 cm from the sample using an electrostatic potentiometer.

[0100] Surface unwinding: Spandex bobbins were unwinded under standard atmospheric conditions (temperature 20±2℃, relative humidity 65±5% RH); samples were conditioned for 24 hours before testing. An axial passive external unwinding method was used, with the traction roller set to an unwinding speed of 600 m / min; a continuous unwinding sampling length of 3000 m (surface section) was taken from the outer surface of the bobbin; a tension sensor was placed between the bobbin and the traction roller, with a signal sampling frequency of 50 Hz. Five bobbins were tested in parallel for each group, and the average unwinding tension variation coefficient was calculated to evaluate the smoothness of surface unwinding. Smaller unwinding tension fluctuations indicate better high-speed unwinding stability.

[0101] The test data is shown in Table 4: Table 4. Spandex spinning test results of each example and comparative example group

[0102] By comparing the test data in Table 4, we can see that: (1) Coefficient of friction: The static friction coefficients of Examples 1-4 and Comparative Example 1 were 0.210-0.219 for fibers and 0.233-0.236 for metals, all close to the ideal state, indicating that the yarn has good smoothness and is easy to process. However, the friction coefficients of Comparative Examples 2-3 were significantly higher (0.275-0.310 for fibers and 0.303-0.369 for metals), which easily led to yarn entanglement and breakage, causing processing difficulties.

[0103] (2) Electrostatic performance: The static electricity generated in Examples 1-4 was 3-4V, and in Comparative Example 1 it was 4V, both at ideal levels. However, Comparative Example 2 reached as high as 30V, indicating severe static electricity accumulation, and Comparative Example 3 was 8V, higher than that of this invention. Resistance test results also showed that the resistance of Examples 1-4 was 6.9 × 10⁻⁶. 8 Ω~7.3×10 8 Ω is superior to that of Comparative Example 1 (8.2 × 10⁻⁶). 8Ω), Comparative Example 2 (15.0 × 10 8 Ω) and Comparative Example 3 (11.1 × 10 8 Ω).

[0104] (3) Elastic elongation: The elastic elongation of Examples 1 to 4 was 577% to 586%, which was significantly better than that of Comparative Example 1 (551%), Comparative Example 2 (534%) and Comparative Example 3 (545%), indicating that the antistatic agent of the present invention has a positive contribution to the elastic recovery performance of spandex fiber.

[0105] (4) Unwinding performance: The unwinding tension (1.10g to 1.12g) and unwinding tension variation coefficient (3.4% to 3.6%) of Examples 1 to 4 are better than those of Comparative Examples 1 to 3 (unwinding tension 1.25g to 1.31g, unwinding tension variation coefficient 5.3% to 11.9%), indicating that the antistatic agent of the present invention has good unwinding smoothness.

[0106] During the spinning process, spandex fibers often carry a negative charge on their surface. According to the principle of opposite charges attract, cationic antistatic agents (Comparative Example 3) are more easily adsorbed onto the fiber surface, but they are also more prone to over-adsorption, leading to uneven distribution of the oil agent, resulting in an excessively high coefficient of friction and affecting unwinding smoothness. In contrast, anionic antistatic agents repel the fibers due to their similar charge, resulting in a moderate and uniform adsorption amount and the formation of a smoother oil film. Comparative Example 2 (without long-chain alkyl groups) lacks the solubilizing effect of long-chain alkyl groups, leading to poor compatibility with the mineral oil components in the oil agent, causing system instability and precipitation, and a significant decrease in both smoothness and antistatic properties.

[0107] In summary, the most significant advantages of adding the antistatic agent prepared according to this invention to spandex oiling agents compared to cationic and amphoteric types are its superior thermal stability, broad system compatibility, and highly controllable failure modes. This antistatic agent does not suffer from the precipitous performance drop caused by isoelectric point drift or molecular coiling at high temperatures, as seen in amphoteric types. It also does not undergo neutralization and precipitation reactions with anionic emulsifiers in spandex oiling agents (a drawback of cationic antistatic agents). It is perfectly compatible with existing oiling systems primarily composed of anionic / nonionic agents, allowing ample room for process adjustments. Furthermore, it remains stable over a wide pH range (4–10) and does not precipitate due to acid-base fluctuations caused by trace amounts of hydrolysis in the oiling agent. Its overall reliability is significantly superior to both amphoteric and cationic types, making it a more mature and reliable choice for industrial spandex oiling agents.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. An antistatic agent for high-speed spinning of spandex, characterized in that, It contains phosphate-type anionic organosilicon antistatic agents and nonionic surfactants; The phosphate-type anionic organosilicon antistatic agent has a polysiloxane backbone, on which long-chain alkyl side chains and epoxy-containing side chains are connected by hydrosilylation reaction. The epoxy group in the side chain containing the epoxy group is ring-opening esterified by a phosphorylating agent to form a phosphate ester group, and the phosphate ester group is then salted to form a phosphate structure.

2. The antistatic agent for high-speed spinning of spandex according to claim 1, characterized in that, The long-chain alkyl side chain originates from the hydrosilylation reaction of the long-chain olefin with the silane-hydrogen bond on the polysiloxane backbone; the epoxy-containing side chain originates from the hydrosilylation reaction of the epoxy compound with double bond with the silane-hydrogen bond on the polysiloxane backbone.

3. The antistatic agent for high-speed spinning of spandex according to claim 1, characterized in that, The nonionic surfactant is selected from one or more of fatty alcohol polyoxyethylene ether, cashew phenol polyoxyethylene ether, and isomeric tridecyl alcohol polyoxyethylene ether.

4. The antistatic agent for high-speed spinning of spandex according to claim 1, characterized in that, The mass ratio of the phosphate-type anionic organosilicon antistatic agent to the nonionic surfactant is 1-10:1-10.

5. A method for preparing an antistatic agent for high-speed spinning of spandex as described in any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane are subjected to a ring-opening copolymerization reaction in the presence of a catalyst to obtain hydrogen-containing silicone oil. S2. The hydrogen-containing silicone oil obtained in step S1 is subjected to a hydrosilylation reaction with long-chain olefins and epoxy compounds with double bonds in the presence of a platinum catalyst to obtain a long-chain alkane and epoxy co-modified silicone oil. S3. The long-chain alkane obtained in step S2 is subjected to ring-opening esterification reaction with epoxy co-modified silicone oil and phosphorylation reagent, and then washed with water to obtain phosphate ester modified silicone oil. S4. The phosphate-modified silicone oil obtained in step S3 is neutralized with an alkaline solution and dehydrated to obtain a phosphate-type anionic organosilicon antistatic agent. S5. Mix the phosphate-type anionic organosilicon antistatic agent obtained in step S4 with a nonionic surfactant until homogeneous to obtain the antistatic agent for high-speed spinning of spandex.

6. The method for preparing the antistatic agent for high-speed spinning of spandex according to claim 5, characterized in that, In step S1: the mass ratio of hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane is 1-8:1-100:1-200; the catalyst is selected from any one or more of trifluoromethanesulfonic acid, acidic cation exchange resin, sulfuric acid, sulfonic acid, and acidic clay; the amount of catalyst used is 0.1%-20% of the total mass of hexamethyldisiloxane, tetramethyltetrahydrocyclotetrasiloxane, and octamethylcyclotetrasiloxane; the reaction temperature in step S1 is 20℃-100℃, and the reaction time is 2 hours-10 hours.

7. The method for preparing the antistatic agent for high-speed spinning of spandex according to claim 5, characterized in that, In step S2: the mass ratio of the hydrogen-containing silicone oil, long-chain olefin, and epoxy compound with double bonds is 1-7:1-20:1-40; the long-chain olefin is a C3-C30 straight-chain olefin; the epoxy compound with double bonds is any one of allyl epoxy polyether, allyl glycidyl ether, glycidyl methacrylate, and 1,2-epoxy-4-vinylcyclohexane; the platinum catalyst is selected from any one or more of Karstedt catalyst, Speier catalyst, and supported platinum catalyst, and the amount of platinum catalyst added is 1 ppm to 10 ppm of the total mass of the hydrogen-containing silicone oil, long-chain olefin, and epoxy compound with double bonds; the reaction temperature in step S2 is 50℃ to 130℃, and the reaction time is 2 hours to 10 hours.

8. The method for preparing the antistatic agent for high-speed spinning of spandex according to claim 5, characterized in that, In step S3: the mass ratio of the long-chain alkane and epoxy co-modified silicone oil to the phosphorylation reagent is 1-50:1; the phosphorylation reagent is one or more of phosphoric acid, phosphorus pentoxide, and polyphosphoric acid; the reaction temperature of step S3 is 10℃-120℃, and the reaction time is 1 hour-10 hours; the water washing is repeated 1-2 times until the pH of the washing solution is 4-5.

9. The method for preparing the antistatic agent for high-speed spinning of spandex according to claim 5, characterized in that, In step S4: the alkaline solution is any one of potassium hydroxide aqueous solution, sodium hydroxide aqueous solution or triethylamine solution, with a concentration of 5wt% to 20wt%; neutralized to pH 6 to 7, and then dehydrated under vacuum with a vacuum degree of -0.1MPa to -0.01MPa and a dehydration temperature of 80℃ to 120℃; In step S5: the mixing temperature is 40℃~80℃, the mixing and stirring time is 30min~120min, until the system is a homogeneous and transparent liquid, then stop heating, continue stirring and cooling until the temperature is ≤40℃.

10. A spandex spinning oil, characterized in that, It contains an antistatic agent for high-speed spinning of spandex as described in any one of claims 1 to 4, or contains an antistatic agent for high-speed spinning of spandex prepared by the preparation method described in any one of claims 5 to 9.