Liquid crystal polymer fibers and their surface treatment methods, tire cord fabric
By introducing grooves and polar functional groups on the surface of liquid crystal polymer fibers and combining them with surface treatment agents, a stable interfacial bonding layer is formed, which solves the adhesion problem between LCP fibers and rubber matrix, achieving a balance between high strength and high adhesion performance, and is suitable for high-performance tire cord fabric.
Patent Information
- Application Number
- CN202611496511.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-23
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to achieve high adhesion to rubber matrices while maintaining the high strength of liquid crystal polymer fibers (LCP fibers), and surface activity is prone to degradation, resulting in unstable adhesion in industrial continuous production.
By employing dry surface activation treatment combined with surface treatment agents, grooves and polar functional groups are introduced on the surface of LCP fibers, and reactive compounds and film-forming components are coated to form physical anchoring points and chemical bonds, thus constructing a stable interfacial bonding layer.
While maintaining the high strength of the fiber itself, it significantly improves the interfacial adhesion performance with the rubber matrix and inhibits the decline of surface activity, thus meeting the high-performance requirements of tire cord fabric.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of high-performance fiber technology, and in particular to liquid crystal polymer fibers and their surface treatment methods, as well as tire cord fabric. Background Technology
[0002] Tire cord fabric is the skeleton material of a tire, primarily bearing the internal inflation pressure, external loads, and dynamic stresses during driving. It has a decisive impact on the tire's load-bearing capacity, dimensional stability, driving safety, and service life. As the automotive industry develops towards high-speed, energy-saving, safe, and new energy vehicle specialization, the performance requirements for tire cord fabric are increasingly stringent. An ideal next-generation cord should simultaneously possess high strength, high modulus, low heat shrinkage, excellent dimensional stability, and high adhesion to the rubber matrix. Currently, mainstream cord fabric fibers include polyester fiber, nylon 66, and aramid fiber. Among these, while aramid fiber has high strength and modulus, its resistance to damp heat aging is insufficient, and its cost is relatively high.
[0003] Liquid crystal polymer (LCP) fibers consist of rigid or semi-rigid rod-shaped molecular chains that can form anisotropic liquid crystal states in the molten or solution state. After spinning, their highly oriented structure is frozen within the solid fiber, thus endowing the fiber with excellent comprehensive properties. LCP fibers have tensile strengths exceeding 3.0 GPa, moduli often exceeding 70 GPa, low density, near-zero moisture absorption, extremely low coefficient of thermal expansion, excellent dimensional stability, a wide operating temperature range, and inherent flame retardancy and outstanding chemical corrosion resistance. In terms of specific strength and specific modulus, LCP fibers outperform traditional organic fibers such as nylon, polyester, and rayon, and are comparable to inorganic fibers such as carbon fiber and glass fiber, while overcoming the latter's brittleness and easy breakage. Therefore, LCP fibers are considered an ideal candidate material for next-generation high-performance tire cord fabrics.
[0004] However, LCP molecular chains are highly oriented axially, resulting in a smooth fiber surface primarily composed of rigid aromatic rings and ester groups. This structure endows the fiber with ultra-high strength and modulus, but also makes its surface exhibit extremely high chemical inertness. XPS analysis shows that the oxygen content on the surface of untreated LCP fibers is typically only around 5%, with few polar groups and a lack of active functional groups such as -OH, -COOH, and -NH2 that can chemically bond with rubber. This results in a surface energy as low as 20-40 mN / m, making it difficult for conventional rubber adhesives to effectively wet and spread on its surface. Therefore, LCP fibers struggle to form effective chemical bonds and physical adsorption with polar rubbers such as natural rubber and styrene-butadiene rubber, resulting in extremely low interfacial adhesion. If used directly, under dynamic tire loads, the cords are prone to peeling off from the rubber, leading to damage to the tire's internal structure and failure.
[0005] In addition, the bonding treatment of tire cord fibers currently typically employs a resorcinol-formaldehyde-latex (RFL) impregnation system. This impregnation system works well for fibers containing polar groups, such as polyester and nylon, because the polar groups on the fiber surface can chemically react with the RFL resin, thereby forming a strong interfacial bonding layer between the fiber and the rubber. However, due to the extremely strong chemical inertness of LCP fiber surfaces, there is a lack of active sites that can chemically react with RFL resin. Even with a two-bath impregnation process, the adhesion of the RFL film to the LCP fiber surface is extremely weak. The conventional RFL process reported in CN1533453A can increase the pull-out force of aramid fibers to 80-100 N / fiber after treatment, but the direct impregnation effect on LCP fibers is far lower, with an adhesion rate typically less than 40%, and the interface failure mode is mainly debonding. Even with a one-bath activation pretreatment such as D417, it is difficult to introduce a sufficient density of active sites on the LCP fiber surface, resulting in poor subsequent adhesion to the rubber matrix.
[0006] Therefore, to improve the surface activity of LCP fibers and their adhesion to the rubber matrix, existing technologies have attempted surface treatment methods such as chemical etching and plasma activation, but all have shortcomings. While chemical etching of the fiber surface using strong acids such as concentrated sulfuric acid or mixed acids, or strong oxidants such as potassium permanganate solution, can introduce polar groups or form a rough structure, the strength of LCP fibers mainly depends on the physical interactions between molecular chains rather than chemical cross-linking. Its bulk strength is highly dependent on the physical entanglement and orientation of the molecular chains. Chemical etching, while introducing polar groups or a rough structure, inevitably erodes the surface molecular chains of the fiber, leading to peeling or chain breakage. Experimental data shows that after conventional chemical etching, the tensile strength retention rate of LCP fibers is typically only 70%-80%, far below the minimum requirement of over 85% for tire cord fabric applications, making it difficult to establish a balance between "introducing sufficient active sites" and "maintaining the bulk strength of the fiber." While plasma activation treatment can introduce polar groups and increase surface energy on the surface of LCP fibers, these introduced polar groups are time-sensitive. Studies have shown that after plasma activation, the surface contact angle of LCP surfaces gradually recovers and the concentration of active groups decreases, typically within 24-72 hours, as storage time increases. This is because LCP molecular chains still possess a certain degree of mobility at room temperature, allowing the introduced polar groups to migrate into the bulk, while the surface free energy tends towards its thermodynamic minimum. Current technologies have not provided an effective solution to this activity degradation problem, making it difficult to guarantee stable bonding performance of plasma-treated LCP fibers in continuous industrial production.
[0007] In summary, existing technologies exhibit poor compatibility between conventional RFL impregnation systems and LCP fibers, chemical etching can damage the fiber's bulk strength, and plasma activation methods suffer from easy degradation of surface activity. Therefore, existing technologies struggle to simultaneously meet the requirements of maintaining high strength in LCP fibers, achieving high adhesion to both the RFL impregnation system and the rubber matrix, ensuring long-term surface activity stability, and maintaining stability for continuous industrial production. Summary of the Invention
[0008] Based on this, it is necessary to provide a liquid crystal polymer fiber and its surface treatment method, as well as a tire cord fabric, to address the above problems. The surface treatment method introduces high-density active functional groups on the surface of the LCP fiber and coats it with a surface treatment agent, which significantly improves the interfacial adhesion performance between the LCP fiber and the impregnation system and the rubber matrix while maintaining the high strength of the fiber body and inhibiting the decline of surface activity.
[0009] A surface treatment method for liquid crystal polymer fibers includes the following steps:
[0010] Dry surface activation treatment of liquid crystal polymer fibers;
[0011] A surface treatment agent is coated onto the surface of a liquid crystal polymer fiber after dry surface activation treatment and then dried. The surface treatment agent contains a reactive compound and / or a film-forming component. The reactive compound is selected from one or more of epoxy resin, blocked isocyanate, and polyurethane prepolymer. The film-forming component is selected from fatty acid ester smoothing agents and / or terpene resins.
[0012] In one embodiment, the surface treatment agent comprises, by mass fraction, 12%-18% water-soluble epoxy resin, 6%-9% blocked isocyanate, 2%-5% coupling agent, 1%-2% wetting agent, and the balance being deionized water.
[0013] In one embodiment, the surface treatment agent comprises, by mass fraction, 30%-50% of a fatty acid ester smoother, 10%-30% of a terpene resin, 10%-30% of an antistatic agent, 10%-30% of an emulsifier, and the balance being deionized water.
[0014] In one embodiment, the surface treatment agent comprises, by mass fraction, 20%-50% polyurethane prepolymer, 2%-6% epoxy silane coupling agent, 5%-15% terpene resin, 10%-20% emulsifier, and the balance deionized water.
[0015] In one embodiment, the dry surface activation treatment is selected from plasma treatment and / or corona treatment.
[0016] In one embodiment, after the dry surface activation treatment, the surface etching depth of the liquid crystal polymer fiber is less than or equal to 50 nm.
[0017] In one embodiment, after coating and drying the surface treatment agent, the liquid crystal polymer fiber is further subjected to a two-bath impregnation treatment.
[0018] In one embodiment, the two-bath impregnation process includes a first-bath activation impregnation and a second-bath main impregnation;
[0019] The first bath activation impregnation solution, by mass fraction, comprises 10%-20% epoxy resin, 20%-50% blocked isocyanate, 0.5%-1.5% nonionic penetrant, and the balance deionized water. The second bath main impregnation solution comprises 30%-70% phenolic resin, 10%-40% butadiene-pyridine latex, 1%-5% waterborne epoxy curing agent, and the balance deionized water.
[0020] A liquid crystal polymer fiber obtained by the surface treatment method described above.
[0021] A tire cord fabric made using the aforementioned liquid crystal polymer fiber.
[0022] In this invention, the liquid crystal polymer fiber is first subjected to dry surface activation treatment, resulting in a dual effect of physical etching and chemical activation on the fiber surface. On the one hand, grooves are formed to increase the physical anchoring points between the fiber and the subsequent impregnation layer; on the other hand, polar functional groups such as -OH, -COOH, and -C=O are introduced to increase the surface energy, transforming the fiber surface from chemically inert to chemically active. Then, a surface treatment agent is coated after the dry surface activation treatment. The reactive compounds in the surface treatment agent can chemically react with the polar functional groups introduced on the fiber surface, anchoring to the fiber surface through covalent bonds and introducing new active sites. The film-forming component can form a continuous and uniform coating layer on the fiber surface, inhibiting activity decay. During the subsequent impregnation process, it undergoes physical entanglement and diffusion interpenetration with the resin and rubber components in the impregnation solution, forming a physical cross-linked network between the fiber and the impregnation layer. Therefore, the dry surface activation treatment and the surface treatment agent coating work synergistically, ultimately forming a strong and stable interfacial bond between the LCP fiber and the rubber matrix. While maintaining the high strength of the fiber itself, it significantly improves the adhesive performance and inhibits surface activity decay. Detailed Implementation
[0023] To facilitate understanding of the present invention, it will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. Rather, these embodiments or examples are provided to make the disclosure of the present invention more thorough and complete.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments or examples only and is not intended to limit the invention. The optional scope of the term "and / or" as used herein includes any one of two or more of the related listed items, as well as any and all combinations of the related listed items, including any two related listed items, any more related listed items, or a combination of all related listed items.
[0025] In this invention, numerical ranges are involved. Unless otherwise specified, the numerical ranges are considered continuous and include the minimum and maximum values of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values of the range. Additionally, when multiple ranges are provided to describe features or characteristics, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are included.
[0026] The surface treatment method for liquid crystal polymer fibers provided by the present invention includes the following steps:
[0027] Dry surface activation treatment of liquid crystal polymer fibers;
[0028] A surface treatment agent is coated onto the surface of a liquid crystal polymer fiber after dry surface activation treatment and then dried. The surface treatment agent contains a reactive compound and / or a film-forming component. The reactive compound is selected from one or more of epoxy resin, blocked isocyanate, and polyurethane prepolymer. The film-forming component is selected from fatty acid ester smoothing agents and / or terpene resins.
[0029] In this invention, the liquid crystal polymer fiber is first subjected to dry surface activation treatment, which produces a dual effect of physical etching and chemical activation on the fiber surface. On the one hand, grooves are etched on the fiber surface to increase the physical anchoring points between the fiber and the subsequent impregnation layer. On the other hand, polar functional groups such as -OH, -COOH, and -C=O are introduced on the fiber surface to increase the surface energy, so that the fiber surface changes from chemical inert to chemical active, thereby improving the wetting and spreading ability of the impregnation solution on the fiber surface.
[0030] Then, after dry surface activation treatment, a surface treatment agent is applied. The reactive compounds in the surface treatment agent can chemically react with the polar functional groups introduced on the fiber surface, anchoring them to the fiber surface through covalent bonds, while simultaneously introducing new active sites. The film-forming component in the surface treatment agent can form a continuous and uniform coating layer on the fiber surface, isolating the passivation effect of air and moisture on the polar functional groups, inhibiting activity decay, and during the subsequent impregnation process, the film-forming component can also undergo physical entanglement and diffusion interpenetration between macromolecular chains with the resin and rubber components in the impregnation solution, forming a physical cross-linked network between the fiber and the impregnation layer.
[0031] Thus, dry surface activation treatment and surface treatment agent coating work synergistically. Dry surface activation treatment introduces active sites on the fiber surface and provides a physical anchoring structure, while surface treatment agent coating protects the active sites and further constructs an interfacial layer that can chemically bond and physically entangle with the impregnation system and rubber matrix. Ultimately, a strong and stable interfacial bond is formed between the LCP fiber and the rubber matrix, significantly improving adhesion performance and inhibiting surface activity degradation while maintaining the high strength of the fiber itself.
[0032] In this invention, the dry surface activation treatment can be selected from plasma treatment and / or corona treatment, etc. The plasma treatment atmosphere can be compressed air or nitrogen, with a gas flow rate of 10L / min-100L / min, a discharge power of 100W-1000W, a fiber running speed of 10m / min-200m / min, and an electrode-fiber spacing of 1mm-10mm. The corona treatment power can be 400W-1200W, the fiber running speed of 10m / min-150m / min, and the electrode spacing of 1mm-10mm. This results in a surface etching depth of less than or equal to 50nm for the liquid crystal polymer fiber, more preferably 10nm-30nm. This allows for the formation of uniformly distributed micron-level trenches on the fiber surface and the introduction of polar functional groups, while avoiding excessive etching into the fiber surface layer, preventing excessive breakage of the fiber surface molecular chains or peeling of the outer layer. This allows the liquid crystal polymer fiber to achieve surface activity while maintaining high bulk strength.
[0033] In this invention, the formulation of the surface treatment agent can be selected and combined according to the surface activation method, the subsequent impregnation system, and the target adhesive properties. By adjusting the types and ratios of reactive compounds and film-forming components, the surface treatment agent can be adapted to different activation treatment methods and impregnation systems.
[0034] For example, the surface treatment agent can be a reactive surface treatment agent, comprising, by mass fraction, 12%-18% water-soluble epoxy resin, 6%-9% blocked isocyanate (HDI trimer), 2%-5% coupling agent, 1%-2% wetting agent, and the balance deionized water. The coupling agent can be selected from AGE coupling agents, and the wetting agent can be selected from JFC wetting agents. In this formulation, the water-soluble epoxy resin and blocked isocyanate can form a reactive coating layer on the fiber surface at the unsealing temperature. The coupling agent enhances the bonding between the treatment agent and the fiber surface and subsequent impregnation layers, while the wetting agent improves the uniformity of the treatment agent's spread on the fiber surface.
[0035] The surface treatment agent can also be a physical coating type surface treatment agent, comprising, by mass fraction, 30%-50% fatty acid ester smoothing agent, 10%-30% terpene resin, 10%-30% antistatic agent, 10%-30% emulsifier, and the balance deionized water. The fatty acid ester smoothing agent can be selected from at least one of PEG400MO, PEG400DO, and PEG600DO; the antistatic agent can be selected from at least one of MOA-3P, MOA-3PK, and disodium lauryl sulfosuccinate; and the emulsifier can be selected from at least one of lipophilic Span and hydrophilic Tween emulsifiers. In this formulation, the fatty acid ester smoothing agent forms a continuous and uniform coating layer on the fiber surface, creating a lubricating film, reducing the coefficient of friction, and minimizing fibrillation damage during the process. The terpene resin improves the adhesion between the coating layer and the subsequent impregnation layer. The antistatic agent improves fiber bundle cohesion and yarn path stability, and the emulsifier improves the stability of the treatment agent and the uniformity of the coating.
[0036] The surface treatment agent can also be a compound surface treatment agent, comprising, by mass fraction, 20%-50% polyurethane prepolymer, 2%-6% epoxy silane coupling agent, 5%-15% terpene resin, 10%-20% emulsifier, and the balance deionized water. The emulsifier can be selected from at least one of lipophilic Span and hydrophilic Tween types. In this formulation, the polyurethane prepolymer can react with the polar functional groups on the fiber surface to form urethane bonds, the epoxy silane coupling agent can simultaneously form chemical bonds with the fiber surface and the impregnation layer, and the terpene resin is used to form a physical entanglement network.
[0037] The surface treatment agents formulated above can be applied to different activation treatment methods and subsequent impregnation systems. They can all form a stable coating layer on the surface of liquid crystal polymer fibers, inhibit the decline of surface activity, and form a good interfacial bond with the impregnation solution and rubber matrix during the subsequent impregnation process.
[0038] After coating and drying the surface treatment agent, the present invention can also perform impregnation treatment on the liquid crystal polymer fiber. The impregnation treatment is preferably a two-bath impregnation treatment, including a first bath activation impregnation and a second bath main impregnation, so as to further build an impregnation layer on the fiber surface and improve the interfacial adhesion performance between the fiber and the rubber matrix.
[0039] The impregnation solution used in the first bath for activation impregnation, by mass fraction, comprises 10%-20% epoxy resin, 20%-50% blocked isocyanate, 0.5%-1.5% nonionic penetrant, and the balance deionized water. The nonionic penetrant can be selected from JFC, etc. The epoxy resin and blocked isocyanate in this impregnation solution can react with the polar functional groups introduced onto the fiber surface and the reactive compounds in the surface treatment agent to form an activation layer on the fiber surface; the nonionic penetrant is used to improve the wetting and spreading uniformity of the impregnation solution on the fiber surface, thereby ensuring that the activation layer is uniformly adhered to the fiber surface.
[0040] By mass fraction, the impregnation solution used in the second bath comprises 30%-70% phenolic resin, 10%-40% butadiene-pyridine latex, 1%-5% aqueous epoxy curing agent, and the balance deionized water. The phenolic resin and butadiene-pyridine latex in this impregnation solution can form a main impregnation layer on the surface of the activated layer. The aqueous epoxy curing agent promotes the curing of the impregnation layer and forms a stable interfacial bond with the activated layer and the rubber matrix, thereby forming a strong interfacial bond layer between the liquid crystal polymer fibers and the rubber matrix.
[0041] This invention also provides a liquid crystal polymer fiber obtained by the aforementioned surface treatment method. This liquid crystal polymer fiber maintains high bulk strength while exhibiting excellent adhesive properties, meeting the comprehensive requirements of tire cord fabric for both fiber bulk strength and adhesive performance. Furthermore, this liquid crystal polymer fiber maintains high surface activity and adhesive properties during storage, meeting the requirements for stable adhesive performance in continuous industrial production.
[0042] The present invention also provides a tire cord fabric prepared using the aforementioned liquid crystal polymer fiber. Because the liquid crystal polymer fiber of the present invention has a strong and stable interfacial bond with the rubber matrix, the tire cord fabric is less prone to delamination from the rubber under dynamic loads, exhibiting excellent dimensional stability, heat aging resistance, and dynamic fatigue performance. This meets the requirements for the cord fabric skeleton material of high-performance tires, especially high-speed, energy-saving, and new energy vehicle tires.
[0043] The technical solution of the present invention will be further described below through specific embodiments. However, those skilled in the art will understand that the following embodiments are only for illustrating the present invention and should not be regarded as limiting the scope of the present invention. Unless otherwise specified, specific conditions in the embodiments are performed under conventional conditions or conditions recommended by the manufacturer. Reagents or instruments used without specified manufacturers are all commercially available conventional products.
[0044] Example 1
[0045] LCP resin was melt-spun using a screw extruder at a spinning temperature of 310℃ and a winding speed of 800 m / min to obtain nascent fibers. The nascent fibers underwent a three-stage heat treatment under a nitrogen atmosphere: the first stage at 160℃ for 2 hours, the second stage at 240℃ for 2 hours, and the third stage at 280℃ for 4 hours, causing solid-state polymerization and thickening of the fibers. The resulting LCP fibers were tested and found to have a tensile strength of 23.5 cN / dtex and a modulus of 586 cN / dtex.
[0046] LCP fibers were surface activated using an atmospheric pressure plasma treatment system. The treatment atmosphere was compressed air with a flow rate of 50 L / min, a discharge power of 1000 W, a fiber running speed of 15 m / min, and an electrode-fiber spacing of 6 mm. Testing revealed an etching depth of 15 nm to 35 nm, a fiber breaking strength of 22.1 cN / dtex, and a strength retention rate of 94.0%.
[0047] Plasma-activated LCP fibers were coated with a reactive surface treatment agent using an oiling roller before winding and then dried. The surface treatment agent, by mass fraction, comprised 15% water-soluble polyamide adduct epoxy resin, 8% blocked isocyanate, 5% AGE coupling agent, 2% JFC wetting agent, and the balance deionized water. Testing showed that the surface treatment agent was chemically grafted onto the fiber surface, resulting in a fiber tensile strength of 22.0 cN / dtex and a strength retention rate of 93.6%.
[0048] The LCP fibers, after being coated with a surface treatment agent and wound up, are unwound and then subjected to retwisting and a two-bath impregnation treatment. The two-bath impregnation treatment includes a first-bath activation impregnation and a second-bath main impregnation. By mass fraction, the first-bath activation impregnation solution comprises 15% epoxy resin, 35% blocked isocyanate, 1% JFC nonionic penetrant, and the remainder deionized water. The second-bath main impregnation solution comprises 70% phenolic resin, 20% butadiene-pyridine latex, 2% water-based epoxy curing agent, and the remainder deionized water. The impregnation and curing process is as follows: first-bath impregnation for 30 seconds (room temperature), followed by pre-baking at 110℃ for 2 minutes; second-bath impregnation for 30 seconds (room temperature), followed by high-temperature curing at 190℃ for 3 minutes.
[0049] Example 2
[0050] The only difference between Example 2 and Example 1 is that: a corona treatment device was used to perform surface activation treatment on the LCP fiber, with a treatment power of 800W, a fiber running speed of 20m / min, and an electrode spacing of 2mm. Testing showed that the etching depth was 10nm~20nm, the fiber breaking strength after treatment was 21.8cN / dtex, and the strength retention rate was 94.0%.
[0051] The activated LCP fibers were coated with a physical coating surface treatment agent by impregnation for 20 seconds before winding. After coating, the fibers were dried at 90℃ for 2 minutes, and then wound. The surface treatment agent, by mass fraction, consisted of 20% fatty acid ester smoothing agent PEG400MO, 30% terpene resin (Mn≈1200), 20% antistatic agent MOA-3PK, 25% emulsifier, and the balance deionized water. The treated fibers had a breaking strength of 21.7 cN / dtex and a strength retention rate of 93.5%.
[0052] Example 3
[0053] The only difference between Example 3 and Example 1 is that: an atmospheric pressure plasma treatment device was used, the treatment atmosphere was nitrogen, the gas flow rate was 80 L / min, the discharge power was 1000 W, the fiber running speed was 20 m / min, and the electrode-fiber spacing was 6 mm. Testing showed that the etching depth was 15 nm to 30 nm, the fiber breaking strength after treatment was 22.5 cN / dtex, and the strength retention rate was 94.5%.
[0054] Plasma-activated LCP fibers were impregnated with a compound surface treatment agent before winding for 15 seconds, followed by drying at 110℃ for 2 minutes. The surface treatment agent, by mass fraction, consisted of 50% polyurethane prepolymer, 3% epoxy silane coupling agent, 15% terpene resin (Mn≈1500), 30% T-20, and the balance deionized water. The treated fibers exhibited a breaking strength of 22.4 cN / dtex and a strength retention rate of 94.1%.
[0055] Comparative Example 1
[0056] The only difference between Comparative Example 1 and Example 1 is that the LCP fibers were not subjected to plasma treatment, but were directly coated with a surface treatment agent.
[0057] Comparative Example 2
[0058] The only difference between Comparative Example 2 and Example 1 is that LCP was not coated with a surface treatment agent after plasma treatment and was directly subjected to a two-bath immersion treatment.
[0059] Comparative Example 3
[0060] The only difference between Comparative Example 3 and Example 1 is that the surface treatment agent includes 30% melamine compound, 40% emulsifier and the remainder deionized water.
[0061] Comparative Example 4
[0062] The only difference between Comparative Example 4 and Example 2 is that the surface treatment agent includes 40% polymethyl methacrylate (PMMA), 20% antistatic agent MOA-3PK, 25% emulsifier, and the balance deionized water.
[0063] The performance of the LCP fibers in the above embodiments and comparative examples was tested, and the results are shown in Table 1.
[0064] Table 1
[0065]
[0066] As shown in Table 1, the LCP fibers prepared in each embodiment of the present invention have a high strength retention rate, and the adhesion grade with rubber reaches level 4. The H pull-out force is much better than that of untreated LCP fibers and comparative examples, indicating that the present invention significantly improves the interfacial adhesion effect between LCP fibers and rubber matrix while maintaining the high strength of the fiber body.
[0067] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0068] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.
Claims
1. A method for surface treatment of a liquid crystalline polymer fiber, characterized by, Includes the following steps: Dry surface activation treatment of liquid crystal polymer fibers; A surface treatment agent is coated onto the surface of a liquid crystal polymer fiber after dry surface activation treatment and then dried. The surface treatment agent contains a reactive compound and / or a film-forming component. The reactive compound is selected from one or more of epoxy resin, blocked isocyanate, and polyurethane prepolymer. The film-forming component is selected from fatty acid ester smoothing agents and / or terpene resins.
2. The surface treatment method of the liquid crystalline polymer fiber according to claim 1, characterized by, By mass fraction, the surface treatment agent comprises 12%-18% water-soluble epoxy resin, 6%-9% blocked isocyanate, 2%-5% coupling agent, 1%-2% wetting agent, and the balance being deionized water.
3. The surface treatment method of the liquid crystalline polymer fiber according to claim 1, characterized by, By mass fraction, the surface treatment agent comprises 30%-50% fatty acid ester smoothing agent, 10%-30% terpene resin, 10%-30% antistatic agent, 10%-30% emulsifier, and the balance deionized water.
4. The surface treatment method of the liquid crystalline polymer fiber according to claim 1, characterized by, By mass fraction, the surface treatment agent comprises 20%-50% polyurethane prepolymer, 2%-6% epoxy silane coupling agent, 5%-15% terpene resin, 10%-20% emulsifier, and the balance deionized water.
5. The surface treatment method for liquid crystal polymer fibers according to claim 1, characterized in that, The dry surface activation treatment is selected from plasma treatment and / or corona treatment.
6. The surface treatment method for liquid crystal polymer fibers according to claim 1, characterized in that, After the dry surface activation treatment, the surface etching depth of the liquid crystal polymer fiber is less than or equal to 50 nm.
7. The surface treatment method for liquid crystal polymer fibers according to any one of claims 1-6, characterized in that, After coating with a surface treatment agent and drying, the liquid crystal polymer fiber is also subjected to a two-bath impregnation treatment.
8. The surface treatment method for liquid crystal polymer fibers according to claim 7, characterized in that, The two-bath impregnation process includes a first-bath activation impregnation and a second-bath main impregnation. The first bath activation impregnation solution, by mass fraction, comprises 10%-20% epoxy resin, 20%-50% blocked isocyanate, 0.5%-1.5% nonionic penetrant, and the balance deionized water. The second bath main impregnation solution comprises 30%-70% phenolic resin, 10%-40% butadiene-pyridine latex, 1%-5% waterborne epoxy curing agent, and the balance deionized water.
9. A liquid crystal polymer fiber obtained by the surface treatment method according to any one of claims 1 to 8.
10. A tire cord fabric prepared using the liquid crystal polymer fiber as described in claim 9.
Citation Information
Patent Citations
Improved process and system for producing tire cords
CN1533453A