Quick-drying working solution for fabric finishing, quick-drying pure cotton fabric and its preparation method

By using a quick-drying working fluid containing crosslinking agents, catalysts, and nano-boron nitride in pure cotton fabric, combined with specific processing techniques, a hydrophobic and thermally conductive structure is formed, solving the problem of pure cotton fabric being difficult to dry after absorbing moisture. This achieves a highly efficient, environmentally friendly, and washable quick-drying effect that meets standards.

CN123108934APending Publication Date: 2026-11-17SHENZHEN PURCOTTON TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611212556.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-11
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing pure cotton fabrics are difficult to dry quickly after absorbing moisture, and cannot simultaneously meet the requirements of 'pure cotton feel', 'zero formaldehyde and environmental protection', 'fluorine-free health and safety', 'durable washability' and 'high drying rate', and cannot consistently meet the GB/T 21655.1-2023 standard.

Method used

A quick-drying working fluid consisting of crosslinking agents, catalysts, nano-boron nitride, and polyethylene wax with specific particle sizes is used. Combined with liquid ammonia treatment, padding, pre-drying, baking, washing, and mechanical pre-shrinking processes, a discontinuous hydrophobic film and a three-dimensional porous structure are formed, which improves the hydrophobicity and thermal conductivity of the fabric and ensures the stability of chemical reagents and fiber strength.

Benefits of technology

It achieves rapid drying of pure cotton fabric, maintains the soft feel of pure cotton, is environmentally friendly and formaldehyde-free, has good washability, and meets the GB/T 21655.1-2023 standard, possessing excellent moisture absorption and quick-drying performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses a quick-drying working solution for fabric finishing, a quick-drying pure cotton fabric, and a method for preparing the same. The quick-drying working solution comprises a crosslinking agent, a catalyst, nano-boron nitride, polyethylene wax, and a solvent. The crosslinking agent is at least one selected from 1,2,3,4-butanetetracarboxylic acid, citric acid, polymaleic acid, and a citric acid-polymaleic acid composite. The catalyst is at least one selected from sodium hypophosphite, cyanamide, and a mixed phosphate catalyst. The polyethylene wax has a particle size of 30-50 nm. In the finishing of pure cotton fabric, the 30-50 nm polyethylene wax in the quick-drying working solution can penetrate into the gaps between cotton fibers and even into the fiber interior, imparting hydrophobicity to the cotton fabric and forming a discontinuous hydrophobic film. This allows moisture to diffuse more readily onto the fabric surface, thereby shortening the drying time. The polyethylene wax can fill the space between the crosslinking network of the crosslinking agent and the nano-boron nitride particles, acting as a dispersant and flexible buffer, thus improving the stability of the quick-drying working solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of quick-drying fabric technology, and in particular to a quick-drying working solution for fabric finishing, a pure cotton quick-drying fabric, and a method for preparing the same. Background Technology

[0002] Pure cotton fabric is widely loved by consumers for its softness, skin-friendliness, and breathability. However, the macromolecular structure of pure cotton (cellulose) contains a large number of hydrophilic hydroxyl groups (-OH). When the human body sweats, cotton fibers readily absorb moisture and undergo rapid and intense lateral swelling, restricting capillary diffusion of moisture. Furthermore, much of the moisture is locked inside the fibers as "bound water," making it difficult for the moisture to evaporate. This results in pure cotton clothing often feeling clingy, damp, and sticky after absorbing sweat, failing to meet modern consumers' demand for "moisture-wicking and quick-drying" sportswear.

[0003] Quick-drying fabrics generally refer to fabrics that meet the moisture-wicking and quick-drying performance requirements of the national standard GB / T 21655.1-2023. In response to the problem that pure cotton fabrics cannot meet the "moisture-wicking and quick-drying" requirements, the existing solutions are mainly as follows: (1) Chemical fiber substitution method. Most of the quick-drying clothes on the market use synthetic fibers such as polyester and nylon. Through the "cross-shaped" or "groove-shaped" irregular cross section spinning technology, the capillary effect is used to achieve water-wicking and quick-drying. The defects and shortcomings of this method are that it lacks the natural skin-friendly properties of pure cotton, is prone to odor and static electricity, and is not as comfortable to wear as pure cotton. (2) Pure cotton one-way moisture-wicking finishing method: Water-repellent agents, such as fluorine or silicone water-repellent agents, are printed on one side of pure cotton fabric to direct sweat from the inner layer that has been treated with water-repellent to the outer layer that has not been treated with water-repellent. This method is mostly a semi-coating finishing, with poor air permeability. Fluorine water-repellent agents pose a potential threat to human health and damage the natural environment. Silicon water-repellent agents have poor water resistance and the quick-drying effect drops sharply after a few washes. (3) Resin crosslinking finishing: 2D resin is used to crosslink cotton fibers to reduce water absorption. However, 2D resin contains formaldehyde, which poses a risk of formaldehyde release and does not meet modern environmental protection requirements. In addition, the crosslinking network is rigid and has a hard hand feel. It needs to be squeezed under great pressure to obtain a better hand feel. However, this also causes the pores between yarns to be compacted, destroying the capillary channels required for water evaporation. As a result, water cannot diffuse through the capillary channels, reducing the drying rate.

[0004] In summary, existing pure cotton quick-drying technology cannot simultaneously achieve the effects of "pure cotton feel", "zero formaldehyde and environmental protection", "fluorine-free health and safety", "durable washability" and "high drying rate", and cannot make all-cotton quick-drying fabrics stably pass the GB / T 21655.1-2023 standard. Summary of the Invention

[0005] The purpose of this application is to provide a new quick-drying working solution for fabric finishing, a pure cotton quick-drying fabric prepared using the quick-drying working solution, and a method for preparing the same.

[0006] To achieve the above objectives, this application adopts the following technical solution:

[0007] This application discloses a quick-drying working solution for fabric finishing, comprising a crosslinking agent, a catalyst, nano-boron nitride (Nano-BN), polyethylene wax, and a solvent; wherein the crosslinking agent is at least one selected from 1,2,3,4-butanetetracarboxylic acid (BTCA), citric acid, polymaleic acid, and a citric acid-polymaleic acid composite; the catalyst is at least one selected from sodium hypophosphite (SHP), cyanamide, and a mixed phosphate catalyst; and the polyethylene wax (PE wax) has a particle size of 30-50 nm. When the crosslinking agent is citric acid, although citric acid is prone to yellowing, the purpose of reducing the water absorption of hydroxyl groups can still be achieved by adding a yellowing inhibitor.

[0008] It should be noted that this application incorporates polyethylene wax with a particle size of 30-50 nm into the quick-drying working solution. When finishing pure cotton fabrics, this wax easily penetrates into the gaps between cotton fibers and even into the fibers themselves, imparting a certain degree of hydrophobicity to the cotton fabric. Combined with subsequent processes such as washing and mechanical pre-shrinking, this causes some damage to the film, forming a discontinuous hydrophobic film. This allows moisture to diffuse more readily on the fabric surface rather than penetrate deeply, thus significantly shortening the drying time. Furthermore, this specific-sized nano-polyethylene wax not only imparts hydrophobicity but, more importantly, it can precisely fill the gap between the crosslinking network of the crosslinking agent and the Nano-BN particles, acting as both a "nanoscale dispersant" and a "flexible buffer layer." This not only solves the stability problem of the working solution but also significantly improves the tensile strength of the fabric. In a strongly acidic, high-electrolyte crosslinking system containing crosslinking agents and catalysts, the polyethylene wax emulsion with this specific particle size exhibits an excellent synergistic effect of dispersion and protection for Nano-BN.

[0009] It should also be noted that in conventional high-salt crosslinking solutions, nanoparticles are prone to agglomeration due to van der Waals forces caused by the compression of the electric double layer. In this application, on the one hand, the nonionic / polymeric emulsifier segments enriched around the PE wax emulsion can adsorb onto the Nano-BN surface. Their hydrophilic segments extending into the aqueous phase construct a highly effective steric hindrance layer independent of charge, successfully resisting electrostatic failure under high-salt conditions. On the other hand, the extremely small particle size of 30-50 nm gives the PE wax emulsion perfect size matching. These nanoscale wax microparticles, acting as a physical buffer, are uniformly interspersed between Nano-BN particles, effectively blocking direct contact between BN particles. The synergy of these two factors completely overcomes the technical bias of inorganic nanomaterials being prone to demulsification and agglomeration in acidic non-ironing / crosslinking working solutions, ensuring not only the long-term stability of the working solution but also ensuring uniform film formation and efficient thermal conductivity on the fiber surface.

[0010] In one implementation of this application, the amount of crosslinking agent used is 30-50 g / L.

[0011] In one implementation of this application, the crosslinking agent is 1,2,3,4-butanetetracarboxylic acid.

[0012] In one implementation of this application, the amount of catalyst used is 6-10 g / L.

[0013] In one implementation of this application, the catalyst is sodium hypophosphite.

[0014] It should be noted that in some implementations, BTCA is used as the crosslinking agent and SHP as the catalyst. Under SHP catalysis, the four carboxyl groups of BTCA undergo esterification and crosslinking with the hydroxyl groups of cotton fibers. This significantly consumes the hydrophilic groups of cotton fibers, such as -OH, and simultaneously forms a three-dimensional network crosslinking, limiting the swelling of cotton fibers after water absorption. The space inside the cotton fiber that "holds water" is reduced, and the moisture content is significantly decreased, which is the physical basis for quick drying. Furthermore, BTCA molecules have four carboxyl groups (-COOH). During crosslinking, usually only 2-3 carboxyl groups bind to the cotton fiber, leaving 1-2 free carboxyl groups that wander like "tentacles." The edges of surface-treated Nano-BN usually have hydroxyl (-OH) or amino (-NH2) groups. During high-temperature baking, the remaining carboxyl groups of BTCA react with the groups on the edge of Nano-BN to form strong hydrogen bonds. This means that BTCA not only binds to the cotton fibers, but its remaining carboxyl groups also react with or form strong hydrogen bonds with the groups on the edge of Nano-BN. This effectively "welds" Nano-BN firmly to the cotton fibers using chemical bonds, resulting in an exponential increase in the number of washes. This is fundamentally different from existing technologies that use 2D resins to crosslink with cotton fibers, which only provide a "physical encapsulation" effect on Nano-BN; such "physical encapsulation" easily leads to Nano-BN slippage and loss after multiple washes. For example, in some implementations of this application, pure cotton fabrics treated with a quick-drying working solution containing BTCA, 30-50 nm polyethylene wax, and Nano-BN show a 40% increase in evaporation rate and a Nano-BN retention rate as high as 90% after 50 washes.

[0015] In one implementation of this application, the amount of polyethylene wax used is 15-20 g / L.

[0016] In one implementation of this application, the amount of nano-boron nitride used is 3-5 g / L.

[0017] It should be noted that Nano-BN, known as "white graphene," has extremely high thermal conductivity, meaning it has excellent thermal conductivity. Traditional quick-drying methods rely solely on hydrophobicity, but with the addition of Nano-BN in this application, the fabric can rapidly conduct heat from the external environment or body temperature to water molecules on the fabric surface, forcibly accelerating the vaporization and evaporation rate of moisture.

[0018] In one implementation of this application, the solvent is water.

[0019] It should be noted that in some implementations, this application creatively utilizes BTCA to reduce the water absorption of cotton fabric, uses polyethylene wax of a specific size to change the water absorption of pure cotton fabric from longitudinal absorption into the fiber interior to diffusion along the plane to the fiber surface, and utilizes the excellent thermal conductivity of Nano-BN to evaporate the surface moisture like a micro heater. The combination of these three elements works synergistically to form a quick-drying closed loop of "water repellency-thermal conduction-evaporation promotion".

[0020] This application also discloses a method for preparing a pure cotton quick-drying fabric, including the following steps:

[0021] The liquid ammonia treatment step includes treating the fabric that has undergone pretreatment, dyeing and printing with liquid ammonia; wherein, the pretreatment, dyeing and printing can refer to existing technology and are not specifically limited here;

[0022] The quick-drying working fluid impregnation step includes impregnating the fabric treated with liquid ammonia with the quick-drying working fluid of this application, controlling the water-pinching rate at 65%-75%;

[0023] The pre-drying and high-temperature baking steps involve pre-drying the fabric after the quick-drying working liquid impregnation step, and then baking it at a high temperature of 155-170℃ for 60-120 seconds. This high-temperature baking temperature can effectively avoid acid degradation and yellowing caused by over-baking, and while achieving the ultimate quick-drying life, it can stabilize the tear strength retention rate of the finished product at more than 75%.

[0024] The washing step, including flat or / or loose washing, removes unreacted chemical reagents and releases the warp tension caused by the padding quick-drying working fluid step and the pre-drying and high-temperature baking steps;

[0025] The pressureless, loose drying process involves tumbling the wet fabric after the washing process with hot air without warp and weft tension until the moisture content drops to 6%-8%.

[0026] The mechanical pre-shrinking step includes physical pre-shrinking of the fabric after the pressureless loose drying step to stabilize the fabric dimensions and make the fabric surface smooth and flat. A smooth and flat fabric surface means, for example, that, depending on the fabric category requirements, the singeing grade is ≥3-4, the weft skew / bow skew is ≤3%, and the fabric has no serious defects when inspected using a quarter-point system.

[0027] It should be noted that existing technologies do not combine the above steps into a single process, and offer no technical inspiration for the combination and effects of the technical solution presented in this application. The preparation method of this application utilizes liquid ammonia treatment to extremely swell cotton fibers, transforming their crystalline region from "cellulose I" to "cellulose III," significantly increasing the amorphous region and micropore volume within the fiber. This avoids the swelling and compression of capillary channels caused by subsequent water contact, preserving the capillary effect and maintaining the water diffusion area. Furthermore, it allows Nano-BN and 30-50nm PE wax, which originally could only adhere to the fiber surface, to smoothly penetrate into the fiber interior. In some implementations, if BTCA and SHP remain on the fabric surface after high-temperature baking, they will absorb moisture and undergo acidic hydrolysis during subsequent storage, causing the cotton fabric to become brittle and its strength to drop drastically. The thorough loose washing in this application not only removes unreacted chemical reagents but also allows the fabric to fully shrink in a wet state, releasing the warp tension caused by the padding and baking machines. Furthermore, it restores the capillary channels squeezed during the impregnation of quick-drying agents, removes chemical residues clogging the yarn gaps, and thoroughly unclogs the microscopic capillary network used for sweat conduction. Further, in a state without warp and weft tension, the drying process utilizes the kneading and lifting action of upper and lower airflows to allow the cross-linked pure cotton yarns to fully shrink and expand in three-dimensional space. The preparation method of this application preserves the three-dimensional porous structure inside the fabric, namely the capillary channels, so that sweat can only be discharged to the surface of the fabric as "free water" through the pores and evaporate. Then, through mechanical pre-shrinking, such as a rubber blanket pre-shrinking machine, the treated cotton fabric not only has a soft and curly feel and a flat appearance, but also has good dimensional stability.

[0028] In one implementation of this application, the liquid ammonia treatment includes drying a pure cotton cloth with a moisture content controlled at ≤3% and drying it in an ammonia removal cylinder at a temperature of 85℃±2℃.

[0029] In one implementation of this application, the liquid ammonia vehicle speed for liquid ammonia processing is 20-30 m / min.

[0030] In one implementation of this application, the immersion and rolling process includes at least two immersions and two rolling cycles.

[0031] In one implementation of this application, infrared pre-baking is used, and the infrared pre-baking uses mid-wave infrared light with a wavelength range of 2.0-4.0 μm.

[0032] In one implementation of this application, the infrared pre-baking uses mid-wave infrared light with a wavelength range of 2.5-3.0 μm.

[0033] It should be noted that the wavelength bands of 2.0-4.0 μm or 2.5-3.0 μm precisely match the characteristic absorption peaks of the stretching vibrations of the OH bonds within water molecules. Therefore, in this band, water molecules inside the fabric exhibit strong selective absorption and molecular resonance of infrared radiation, directly converting radiant energy into internal heat energy, achieving "in-situ vaporization." This is fundamentally different from using short-wave infrared rays with wavelengths less than 2.0 μm (which have excessive penetration leading to low water molecule absorption) and far-infrared rays with wavelengths greater than 4.0 μm (which are limited to surface absorption, resulting in "dry outside and wet inside" fabrics). The specific mid-wave infrared rays selected in this application can uniformly penetrate to the core of the pure cotton fibers swollen by liquid ammonia, enabling the water adsorbed with formaldehyde-free resin (BTCA) and catalyst to evaporate synchronously and at the same rate in both the inner and outer layers of the fiber cross-section. This precise wavelength matching completely cuts off the capillary migration path of moisture inside the fabric from a thermodynamic perspective, perfectly locking the uniform distribution of the polycarboxylic acid crosslinking agent among the cotton fiber macromolecules, providing the best reaction basis for subsequent high-temperature esterification crosslinking.

[0034] In one implementation of this application, the pre-baking speed is 15-35 m / min.

[0035] In one implementation of this application, the tension control during high-temperature baking is a micro-overfeed state of +2% to +5%.

[0036] In one implementation of this application, the washing step includes: placing clean water in the washing machine's padding tank, immersing the fabric with a padding rate of 55-65%, steaming in a steamer for 3-5 minutes, and then sequentially washing the fabric in washing tanks at 85-95℃, 65-75℃, 45-55℃, 45-55℃, and 25-35℃ for 35-45 seconds each, and finally drying the fabric without raising the temperature.

[0037] In one implementation of this application, the liquid level in the washing machine's trough is 70%-75%.

[0038] In one implementation of this application, the temperature of the steam oven is 90°C.

[0039] In one implementation of this application, the pressureless loose drying step employs an airflow loose dryer or a rotary drum dryer.

[0040] It should be noted that pressureless loose drying only needs to meet the physical conditions of "no warp and weft tension and drying by hot air tumbling" to achieve the purpose of maintaining the three-dimensional shape and capillary effect of the yarn; it is not limited to airflow loose dryers or drum dryers.

[0041] In one implementation of this application, citric acid is added to the feed trough of the airflow loose dryer to neutralize the pH, maintaining it at 5.5~6.5, with a roll-off rate of 60% and a drying temperature of 110-130℃. The fabric is lifted, rubbed, and thoroughly dried using alternating high-efficiency hot airflows.

[0042] It should be noted that, under conditions of no warp or weft tension, the kneading and lifting action of the airflow from above and below allows the pure cotton yarn, which has completed its cross-linking reaction, to fully shrink and expand in three-dimensional space. This perfectly preserves the three-dimensional porous structure of the fabric, such as capillary channels, allowing sweat to be quickly discharged to the fabric surface as "free water" and evaporate.

[0043] In one implementation of this application, the mechanical pre-shrinking step uses a rubber blanket pre-shrinking machine for physical pre-shrinking.

[0044] This application also discloses a pure cotton quick-drying fabric, which is prepared using the preparation method of this application.

[0045] It should be noted that, compared with existing quick-drying fabrics, the pure cotton quick-drying fabric of this application achieves quick-drying properties of pure cotton fabric; moreover, the pure cotton quick-drying fabric of this application also takes into account the effects of "pure cotton touch", "zero formaldehyde and environmental protection", "fluorine-free health and safety", "durable and washable" and "high drying rate". The pure cotton quick-drying fabric of this application can stably pass the GB / T21655.1-2023 standard.

[0046] Due to the adoption of the above technical solutions, the beneficial effects of this application are as follows:

[0047] The quick-drying working solution of this application, when used to finish pure cotton fabric, allows the polyethylene wax with a particle size of 30-50 nm to penetrate into the gaps between cotton fibers and even into the fibers themselves, giving the cotton fabric a certain degree of hydrophobicity and forming a discontinuous hydrophobic film. This makes it easier for moisture to diffuse on the surface of the fabric rather than penetrate deeply, thus greatly shortening the drying time. In addition, the polyethylene wax with a particle size of 30-50 nm can fill the gaps between the cross-linking network of the cross-linking agent and the nano boron nitride particles, playing a role in dispersion and flexible buffering. This not only solves the stability problem of the quick-drying working solution, but also significantly improves the tensile strength of the fabric. Detailed Implementation

[0048] Existing quick-drying technologies for pure cotton cannot simultaneously achieve "pure cotton feel," "zero formaldehyde and environmental friendliness," "fluorine-free health and safety," "durable washability," and "high drying rate." Furthermore, current quick-drying processes cannot consistently ensure that all-cotton quick-drying fabrics meet the GB / T 21655.1-2023 standard. The key challenge remains to develop pure cotton quick-drying fabrics that meet the standard of GB / T 21655.1-2023 "Evaluation of Moisture Absorption and Quick-Drying Properties of Textiles Part 1: Single-Item Combination Test Method," without altering the natural properties of pure cotton fabrics. This challenge lies in how to reduce the binding force of cotton fibers to water (reducing bound water) through environmentally friendly (formaldehyde-free) chemical modification, combined with specific finishing processes, to preserve the three-dimensional capillary channels between yarns at the macroscopic level (increasing the conduction of free water).

[0049] This application creatively proposes adding polyethylene wax with a particle size of 30-50 nm to the quick-drying working solution of nano-boron nitride. The polyethylene wax of this specific size penetrates into the gaps between cotton fibers and even into the fibers themselves, giving the cotton fabric a certain degree of hydrophobicity and forming a discontinuous hydrophobic film, allowing moisture to diffuse on the fabric surface and shortening the drying time. Furthermore, the polyethylene wax of this size can fill the gaps between the crosslinking agent and the nano-boron nitride particles, playing a dispersing and buffering role and improving the stability of the quick-drying working solution.

[0050] Therefore, this application first develops a quick-drying working fluid for fabric finishing, comprising a crosslinking agent, a catalyst, nano-boron nitride, polyethylene wax, and a solvent; wherein the crosslinking agent is at least one of 1,2,3,4-butanetetracarboxylic acid, citric acid, polymaleic acid, and citric acid-polymaleic acid composite; the catalyst is at least one of sodium hypophosphite, cyanamide, and mixed phosphate catalyst; and the polyethylene wax has a particle size of 30-50 nm.

[0051] Based on this, this application further develops an improved method for preparing pure cotton quick-drying fabric, including: a liquid ammonia treatment step, which involves treating the fabric that has undergone pretreatment, dyeing, and printing with liquid ammonia; wherein the pretreatment, dyeing, and printing processes can refer to existing technologies and are not specifically limited here; a padding quick-drying working solution step, which involves padding the fabric treated with liquid ammonia with the quick-drying working solution of this application, controlling the water-pinching rate at 65%-75%; and a pre-drying and high-temperature baking step, which involves pre-drying the fabric after the padding quick-drying working solution step, and then... The process includes: high-temperature baking at 155-170℃ for 60-120 seconds; a washing step, including flat-width or / or loose washing to remove unreacted chemical reagents and release the warp tension caused by the padding quick-drying working solution and the pre-drying and high-temperature baking steps; a pressureless loose drying step, including hot air tumbling drying of the wet fabric after the washing step without warp and weft tension until the moisture content drops to 6%-8%; and a mechanical pre-shrinking step, including physical pre-shrinking treatment of the fabric after the pressureless loose drying step to stabilize the fabric dimensions and make the fabric surface smooth and flat.

[0052] It should be noted that in this application, the liquid ammonia treatment is not simply for improving gloss, but rather as a micro-pore engineering technique. The size of the micropores formed after the liquid ammonia swells matches the size of the PE wax and Nano-BN in the quick-drying working solution of this application, allowing the PE wax and Nano-BN to better embed into the cotton fibers. This is fundamentally different from existing alkaline mercerizing methods, which only produce limited pore expansion and nanoparticles can only aggregate on the surface. It can be understood that one of the functions of the liquid ammonia treatment step in the preparation method of this application is to form fiber micropores after swelling. For pure cotton fabrics with a loose structure and low warp and weft density, whose physical gaps are relatively large, the liquid ammonia treatment step can be omitted, and the fabric that has undergone pretreatment, dyeing, and printing can be directly impregnated with the quick-drying working solution. Although the strength retention and hand feel of the final product are slightly inferior to those of the technology containing the liquid ammonia treatment step, a basic quick-drying effect can still be achieved.

[0053] It should also be noted that this application creatively combines pressureless loose drying with mechanical pre-shrinking as a key step after the quick-drying cross-linking reaction. By utilizing the physical shrinkage of fibers in three-dimensional space and the reorganization of yarn structure, the fabric is given a large structural deformation margin, thereby perfectly compensating for the brittleness caused by microscopic chemical cross-linking on a macroscopic level. This is not a simple accumulation of conventional processes, but a closed-loop process designed to solve the specific technical problem of strength reduction caused by quick-drying cross-linking in this application.

[0054] The quick-drying working solution of this application and the pure cotton quick-drying fabric prepared therefrom have the following advantages:

[0055] (1) Improved safety and environmental protection: Crosslinking agents, such as BTCA and other polycarboxylic acid resins, are used to replace traditional 2D or modified 2D resins, eliminating the generation of formaldehyde from the source and fully complying with the Class A safety standards for textiles that come into direct contact with the skin of infants and young children.

[0056] (2) Durable washability: Unlike surface coating finishing, this application combines formaldehyde-free resin with cotton fiber through covalent bonds (ester bonds), resulting in strong bonding. Through the embedding of polyethylene wax with specific particle size and nano boron nitride, the fabric's hand feel and quick-drying performance are greatly improved. In some implementations, the quick-drying performance does not decrease after 30 or even 50 standard washes.

[0057] (3) Perfect preservation of comfort: Combining the swelling effect of liquid ammonia and the relaxation effect of pressureless loose drying, while preserving the three-dimensional capillary channels, it overcomes the defects of hardening of the fabric surface and reduction of strength caused by traditional cross-linking resin, and preserves the original soft feel of pure cotton.

[0058] The present application will be further described in detail below through specific embodiments. The following embodiments are only for further illustration of the present application and should not be construed as limiting the present application.

[0059] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0060] Most of the reagents used in the following examples were commercially available. BTCA was purchased from Shandong Zhongkang Guochuang New Materials Co., Ltd., brand name: DP-5825; SHP was purchased from Shandong Zhongkang Guochuang New Materials Co., Ltd., brand name: DP-5801; polyethylene wax emulsion was purchased from Guangdong Taili New Materials Technology Co., Ltd., brand name: XLA40; boron nitride (Nano-BN) was purchased from Shenzhen Baopeng New Materials Technology Co., Ltd., brand name: BP-Cosm; citric acid was purchased from Shanghai Yayun Textile Auxiliaries Co., Ltd., brand name: NA; and the remaining materials were all conventional commercially available products.

[0061] Example 1

[0062] The test specifications were CM 50S+SP 20D plain weave fabric, 32G, 173CM×160gsm.

[0063] The preparation methods for pure cotton quick-drying fabrics include: pretreatment, dyeing and printing, liquid ammonia treatment, padding with quick-drying working solution, pre-drying and high-temperature baking, flat or loose washing, pressureless loose drying, and mechanical pre-shrinking.

[0064] The pretreatment process is as follows: singeing → boiling → bleaching → dyeing / printing.

[0065] Liquid ammonia treatment: The moisture content of the incoming fabric should be ≤3%, the liquid ammonia truck speed is 25m / min, and the temperature of the ammonia removal drying cylinder is 85℃±2℃.

[0066] Impregnation quick-drying working fluid:

[0067] The formula for the quick-drying working solution is as follows: DP-5825 (BTCA): 40 g / L; DP-5801 (SHP): 8 g / L; Polyethylene wax (40nm): 15 g / L; BP-Cosm (Boron Nitride Nano-BN): 3 g / L; Water: balance.

[0068] Two dips and two rolls, with a roll yield of 65% in the first roll and 75% in the second roll.

[0069] Pre-baking and high-temperature baking:

[0070] Pre-baking: Infrared pre-baking is adopted, and mid-wave infrared light with a main emission wavelength of 2.5 μm is used. Vehicle speed: 30m / min.

[0071] Baking: Oven temperature 155℃, 120s, machine speed: 30m / min, tension 1.5kg, overfeed +5%.

[0072] Flat-width washing: Put clean water into the washing machine's padding tank to a level of 70%-75%, immerse the fabric, and remove 55%-65% of the fabric. Steam the fabric in a steamer at 90℃ for 3 minutes, and then wash it for 35 seconds in each of the following washing tanks: 85-95℃, 65-75℃, 45-55℃, 45-55℃, and 25-35℃. Remove the fabric from the drying tank without raising the temperature.

[0073] Pressureless loose drying: Add neutralizing acid NA to maintain pH at 5.5-6.5, roll residue rate 60%, drying room temperature 120℃, upper air volume 80%, lower air volume 65%, exhaust air volume 60%, machine speed: 15m / min.

[0074] Mechanical pre-shrinkage: machine speed 20m / min, rubber blanket temperature 80℃, nylon blanket temperature 120℃, roll gap 5mm.

[0075] Example 2

[0076] The test specifications were CM 50S+SP 20D plain weave fabric, 32G, 173CM×160gsm.

[0077] The preparation method of the pure cotton quick-drying fabric in this example is similar to that in Example 1. The difference is that this example does not involve liquid ammonia treatment. After pretreatment, dyeing, and printing, the fabric is directly impregnated with the quick-drying working solution. The method in this example includes: pretreatment, dyeing and printing, impregnation with the quick-drying working solution, pre-drying and high-temperature baking, flat or loose washing, pressureless loose drying, and mechanical pre-shrinking.

[0078] Pretreatment, dyeing / printing: Same as in Example 1.

[0079] Impregnation and quick-drying working fluid: The formula of the quick-drying working fluid is the same as in Example 1.

[0080] Two dips and two rolls, with a roll yield of 65% in the first roll and 75% in the second roll.

[0081] Pre-baking and high-temperature baking:

[0082] Pre-baking: Same as in Example 1.

[0083] Baking: Same as in Example 1.

[0084] Flat-width water washing: Same as Example 1.

[0085] Pressureless loose drying: Same as in Example 1.

[0086] Mechanical pre-shrinkage: Same as in Example 1.

[0087] Comparative Example 1

[0088] Using ordinary 2D resin: In the quick-drying working solution, BTCA is not used, but 2D resin (BASF, grade BZ-6035) is used to replace BTCA in an equal amount, and the rest is the same as in Example 1.

[0089] Comparative Example 2

[0090] Using polyethylene wax with a common particle size: In the quick-drying working fluid formulation, 30-50nm polyethylene wax emulsion is not used. Instead, polyethylene wax with a common particle size of 100nm is used (the polyethylene wax emulsion was purchased from Guangdong Taili New Material Technology Co., Ltd., brand name XLA100). The rest is the same as in Example 1.

[0091] Comparative Example 3

[0092] Boron nitride Nano-BN not used: In the quick-drying working solution formulation, boron nitride Nano-BN is not used, otherwise it is the same as in Example 1.

[0093] Comparative Example 4

[0094] Polyethylene wax and boron nitride Nano-BN are not used: The quick-drying working fluid formulation does not use polyethylene wax and boron nitride Nano-BN, and the rest is the same as in Example 1.

[0095] Comparative Example 5

[0096] No washing process: After pre-drying and high-temperature baking, no flat or loose washing is performed, and the rest is the same as in Example 1.

[0097] Comparative Example 6

[0098] Drying with a conventional setting machine: Replace the pressureless loose drying with the setting and drying of a conventional setting machine, and the rest is the same as in Example 1.

[0099] The traditional setting and drying process of a setting machine specifically includes: machine speed: 15m / min, drying room temperature: 150℃, and rolling mill.

[0100] Comparison of core test data

[0101] Test standard notes:

[0102] 1. Quick-drying performance is tested according to GB / T 21655.1-2023 (before washing and after 20 washes);

[0103] 2. Strength test according to GB / T 3917.2 (tear strength);

[0104] 3. Free formaldehyde shall be tested in accordance with GB / T 2912.1.

[0105] The fabrics prepared in the examples and comparative examples were tested using the above methods. Simultaneously, a plain cotton fabric with conventional pretreatment was used as a blank control group, and the same tests were performed. The blank control group did not undergo any quick-drying or modification treatment. The test results are shown in Tables 1 and 2.

[0106] Table 1

[0107] Water droplet diffusion time (before washing / after washing) Water absorption rate (%) Cartridge height (before / after washing) Example 1 2.1 s / 2.8 s 175% 125 mm / 135 mm Example 2 1.1 s / 2.5 s 160% 150 mm / 145 mm Comparative Example 1 2.5 s / 2.3 s 195% 85 mm / 80 mm Comparative Example 2 8.4 s / 11.6 s 150% 102 mm / 98 mm Comparative Example 3 2.8 s / 3.3 s 165% 108 mm / 136 mm Comparative Example 4 2.6 s / 3.0 s 170% 110 mm / 133 mm Comparative Example 5 2.5 s / 8.5 s 180% 60 mm / 125 mm Comparative Example 6 2.2 s / 4.0 s 175% 65 mm / 83 mm Blank control 2.5 s / 5.2 s 245% 115 mm / 100 mm

[0108] Table 2

[0109] Drying rate (before washing / after washing) Formaldehyde content Tear strength retention GB / T 21655.1 rating Example 1 0.30 g / h / 0.32 g / h Not detected 78% Overall, it reached Level Π Example 2 0.24 g / h / 0.22 g / h Not detected 75% Overall, it has reached Level I. Comparative Example 1 0.15 g / h / 0.13 g / h 58 mg / kg 62% Substandard Comparative Example 2 0.22 g / h / 0.23 g / h Not detected 72% Substandard Comparative Example 3 0.18 g / h / 0.23 g / h Not detected 72% Substandard Comparative Example 4 0.19 g / h / 0.22 g / h Not detected 70% Substandard Comparative Example 5 0.14 g / h / 0.22 g / h Not detected 72% Substandard Comparative Example 6 0.11 g / h / 0.09 g / h Not detected 68% Substandard Blank control 0.12 g / h / 0.10 g / h Not detected 100% Substandard

[0110] In Tables 1 and 2, "before washing" refers to the fabric obtained directly from the preparation process and tested without washing; "after washing" refers to the fabric being washed 20 times according to the usual clothing washing method before testing, specifically referring to the standard GB / T 21655.1-2023. In Table 2, the tear strength retention rate is the tear strength retention rate of the fabrics in each example and comparative example relative to the blank control group fabric.

[0111] The results in Tables 1 and 2 show that both Example 1 and Example 2 have excellent moisture absorption and quick-drying properties, achieving the quick-drying effect of GB / T21655.1 ratings Π and Ι, respectively. They have the advantages of low strength loss and high safety, showing a significant advantage over the comparative example.

[0112] To better illustrate the effect of PE wax with a particle size of 30-50nm, experiments were conducted using PE wax with particle sizes of 20nm, 30nm, 40nm, 50nm, 60nm, and 80nm, respectively. Except for the different PE waxes, the rest were the same as in Example 1. The experimental data are shown in Table 3.

[0113] Table 3

[0114] Drying rate (before washing / after washing) Water droplet diffusion time (before washing / after washing) Water absorption rate (%) Cartridge height (before / after washing) PE wax particle size 20nm 0.22 g / h / 0.22 g / h 3.2 s / 3.7 s 176% 135 mm / 142 mm PE wax particle size 30nm 0.29 g / h / 0.32 g / h 2.1 s / 3.3 s 165% 143 mm / 135 mm PE wax particle size 40nm 0.31 g / h / 0.33 g / h 3.1 s / 3.5 s 177% 137 mm / 126 mm PE wax particle size 50nm 0.30 g / h / 0.32 g / h 3.4 s / 3.6 s 158% 145 mm / 118 mm PE wax particle size 60nm 0.25 g / h / 0.26 g / h 4.8 s / 6.3 s 172% 108 mm / 106 mm PE wax particle size 70nm 0.19 g / h / 0.21 g / h 5.6 s / 6.0 s 175% 95 mm / 93 mm PE wax particle size 80nm 0.17 g / h / 0.19 g / h 7.6 s / 6.5 s 168% 96 mm / 95 mm

[0115] Table 3 shows that PE wax with a particle size of 30-50 nm produces a high drying rate for pure cotton quick-drying fabric. Regarding water diffusion time, PE wax with a particle size no larger than 50 nm exhibits a shorter water diffusion time. For larger particle sizes, such as 60 nm or larger, the water diffusion time increases, and this increase gradually increases with increasing particle size. In conclusion, the optimal PE wax particle size is neither too large nor too small; PE wax with a particle size of 30-50 nm provides the best overall performance.

[0116] The above description, in conjunction with specific embodiments, provides a further detailed explanation of this application and should not be construed as limiting the specific implementation of this application to these descriptions. Those skilled in the art to which this application pertains can make several simple deductions or substitutions without departing from the concept of this application.

Claims

1. A quick-drying working solution for fabric finishing, characterized in that: Includes crosslinking agents, catalysts, nano boron nitride, polyethylene wax, and solvents; The crosslinking agent is at least one of 1,2,3,4-butanetetracarboxylic acid, citric acid, polymaleic acid, and citric acid-polymaleic acid complex. The catalyst is at least one of sodium hypophosphite, cyanamide, and mixed phosphate catalyst; The polyethylene wax has a particle size of 30-50 nm.

2. The quick-drying working fluid according to claim 1, characterized in that: The amount of the crosslinking agent used is 30-50 g / L; Preferably, the crosslinking agent is 1,2,3,4-butanetetracarboxylic acid.

3. The quick-drying working fluid according to claim 1, characterized in that: The amount of catalyst used is 6-10 g / L; Preferably, the catalyst is sodium hypophosphite.

4. The quick-drying working fluid according to claim 1, characterized in that: The amount of polyethylene wax used is 15-20 g / L.

5. The quick-drying working fluid according to any one of claims 1-4, characterized in that: The amount of the nano-boron nitride used is 3-5 g / L; Optionally, the solvent is water.

6. A method for preparing a pure cotton quick-drying fabric, characterized in that: Includes the following steps, The liquid ammonia treatment process includes treating fabrics that have undergone pretreatment, dyeing, and printing with liquid ammonia. The step of impregnating the fabric with the quick-drying working fluid includes impregnating the fabric treated with liquid ammonia with the quick-drying working fluid according to any one of claims 1-5, and controlling the water rinsing rate at 65%-75%; The pre-drying and high-temperature baking steps involve pre-drying the fabric that has undergone the impregnation and quick-drying working liquid step, and then baking it at a high temperature of 155-170℃ for 60-120 seconds. The washing step, including flat or / or loose washing, removes unreacted chemical reagents and releases the warp tension caused by the padding quick-drying working fluid step and the pre-drying and high-temperature baking steps; The pressureless, loose drying process involves tumbling the wet fabric after the washing process with hot air without warp and weft tension until the moisture content drops to 6%-8%. The mechanical pre-shrinking step includes physical pre-shrinking of the fabric after the pressureless loose drying step to stabilize the fabric size and make the fabric surface smooth and flat.

7. The preparation method according to claim 6, characterized in that: The liquid ammonia treatment includes drying pure cotton cloth with a moisture content controlled at ≤3% and drying the ammonia removal cylinder at a temperature of 85℃±2℃. Optionally, the liquid ammonia vehicle speed for liquid ammonia treatment is 20-30 m / min.

8. The preparation method according to claim 6, characterized in that: The impregnation and quick-drying working fluid step includes at least two impregnations and two rolls.

9. The preparation method according to any one of claims 6-8, characterized in that: The pre-baking process employs infrared pre-baking, specifically mid-wave infrared radiation with a wavelength range of 2.0-4.0 μm. Preferably, the infrared pre-baking uses mid-wave infrared light with a wavelength range of 2.5-3.0 μm; Optionally, the pre-drying speed is 15-35 m / min; Optionally, the tension control during the high-temperature baking is a slightly overfeed state of +2% to +5%; Optionally, the washing step includes placing clean water in the washing machine's padding tank, immersing the fabric with a padding rate of 55-65%, steaming it in a steamer for 3-5 minutes, and then sequentially washing it in washing tanks at 85-95℃, 65-75℃, 45-55℃, 45-55℃, and 25-35℃ for 35-45 seconds each, and then drying the fabric without raising the temperature. Optionally, the liquid level in the washing machine's trough is 70%-75%; Optionally, the temperature of the steamer is 90°C; Optionally, the pressureless loose drying step may employ an airflow loose dryer or a rotary drum dryer; Optionally, citric acid is added to the feed trough of the airflow loose dryer to neutralize it, maintaining the pH at 5.5-6.5, with a pick-up rate of 60% and a drying temperature of 110-130℃. The fabric is lifted, rubbed, and thoroughly dried using alternating high-efficiency hot airflows. Optionally, the mechanical pre-shrinking step uses a rubber blanket pre-shrinking machine for physical pre-shrinking.

10. A pure cotton quick-drying fabric, characterized in that: It is prepared by the preparation method according to any one of claims 6-9.