A GA-PEI organic co-deposition modified PBO fiber, an insulator core, and its preparation method

The surface of PBO fibers was modified by GA-PEI co-deposition, which enhanced their interfacial adhesion to the epoxy resin matrix, solved the problem of poor surface bonding of PBO fibers, and improved the mechanical and electrical insulation properties of the composite material.

CN123108947APending Publication Date: 2026-11-17STATE GRID SICHUAN ELECTRIC POWER CORP ELECTRIC POWER RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611438462.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-09-16
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

The weak interfacial bond strength between PBO fibers and the epoxy resin matrix makes the composite material prone to interfacial delamination under stress, which limits its mechanical and electrical properties.

Method used

The surface of PBO fibers was modified by GA-PEI organic co-deposition method. The interfacial bonding was enhanced by π-π interaction, hydrogen bonding and mechanical intercalation, and polar groups were introduced to form a stable organic network coating, thereby improving the surface energy and wettability of the fibers.

Benefits of technology

It improves stress transmission at the fiber/resin interface, reduces interfacial porosity and defects, enhances the mechanical and electrical insulation properties of the composite core, and maintains its lightweight characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108947A_ABST
    Figure CN123108947A_ABST
Patent Text Reader

Abstract

This invention relates to the field of insulator materials technology, and discloses a GA-PEI organic co-deposition modified PBO fiber, an insulator core, and a preparation method thereof, comprising the following steps: preparing a weakly alkaline co-deposition modification solution containing gallic acid (GA) and polyethyleneimine (PEI); immersing PBO fibers in the weakly alkaline co-deposition modification solution and subjecting them to a shaking reaction; after the reaction is completed, removing the PBO fibers and vacuum drying them to obtain GA-PEI co-deposition modified PBO fibers. This invention utilizes the GA / PEI aqueous co-deposition method to organically functionalize the surface of PBO fibers. Under weakly alkaline conditions, a stable organic interface layer is constructed on the surface of the PBO fibers through a gallic acid oxidation-amine crosslinking reaction, thereby enhancing its interfacial adhesion performance with the epoxy resin matrix and solving the problems of poor surface adhesion and significant chemical inertness of PBO fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of insulator materials technology, and more specifically, to a GA-PEI organic co-deposition modified PBO fiber, an insulator core, and a preparation method thereof. Background Technology

[0002] Insulators are critical components in power systems, ensuring reliable power transmission. Among them, composite post insulators are gradually replacing traditional ceramic insulators due to their lightweight, ease of maintenance, and excellent external insulation performance. The insulating core, as its core structural unit, must not only bear mechanical loads but also provide stable electrical insulation strength. SF composite foam material shows great potential as a novel core material. SF is a two-phase material composed of epoxy resin as the matrix and physically closed-cell hollow polymer microspheres (such as PMMA) as the filler phase. Its unique structure endows it with excellent properties such as low density, high specific strength, extremely low water absorption, and high electrical insulation strength. However, due to insufficient toughness, SF material has difficulty releasing internal stress, which may lead to debonding of the microspheres from the resin matrix, forming micro-cracks, thus limiting its application in high-reliability fields. Existing technological approaches to improve the performance of SF material mainly include nanofiller modification, resin modification, and fiber reinforcement modification. In comparison, fiber reinforcement has proven to be an effective method that can significantly improve the mechanical properties and thermal stability of polymer materials and is feasible for large-scale production. Among many fiber materials, poly(p-phenylenebenzobisoxazole) fiber (PBO) stands out for its excellent specific strength, specific modulus, heat resistance, water resistance, and insulation properties.

[0003] Despite the excellent mechanical strength and thermal stability of PBO fibers, their relatively smooth surface and strong chemical inertness result in weak interfacial adhesion between the fiber and the matrix. Due to the limited physical and chemical bonding between the fiber and the matrix, this interfacial characteristic hinders effective load transfer, leading to interfacial delamination under stress. This significantly reduces the mechanical properties of the composite material, especially under tensile and compressive stresses, easily causing interfacial failure. The low surface energy of PBO fibers limits their effective contact with the matrix material, particularly when the fiber surface is wetted by a liquid matrix (such as epoxy resin), making it difficult to form sufficient physical adsorption or interfacial compatibility. Untreated PBO fibers lack functional groups that can chemically react with the matrix material. Due to the lack of effective chemical reactivity, the fiber and matrix can only rely on weak van der Waals forces or physical adsorption forces for bonding, resulting in insufficient interfacial adhesion and inability to provide sufficient support under stress, thus limiting the mechanical and electrical properties of the composite material.

[0004] In view of the above, this application is hereby submitted. Summary of the Invention

[0005] PBO fiber has a highly chemically inert and smooth surface lacking active functional groups, resulting in extremely weak interfacial bonding strength with the resin matrix. This severely limits its reinforcing effect on SF materials. To address these technical problems, this invention provides GA-PEI organic co-deposition modified PBO fiber, an insulator core, and a preparation method. By using GA-PEI co-deposition to modify the PBO fiber surface, on the one hand, the bonding with the PBO fiber surface can be enhanced through π-π interactions, hydrogen bonding, and mechanical intercalation, thereby forming a uniform and continuous organic functional layer. On the other hand, polar groups such as hydroxyl and amino groups can be introduced into the fiber surface, improving the fiber surface energy and wettability and interfacial compatibility with the epoxy resin matrix. This improves stress transmission at the fiber / resin interface, reduces interfacial porosity and defects, and helps suppress interfacial moisture absorption and electric field distortion, thereby enhancing the mechanical properties, electrical insulation properties, and long-term service stability of the composite core.

[0006] This invention is achieved through the following technical solution: In a first aspect, the present invention provides a method for preparing GA-PEI organic co-deposition modified PBO fibers, comprising the following steps: Prepare a weakly alkaline co-deposition modification solution containing gallic acid (GA) and polyethyleneimine (PEI); PBO fibers were impregnated in the weakly alkaline co-deposition modification solution and subjected to a shaking reaction. After the reaction was complete, the PBO fibers were removed and vacuum dried to obtain GA-PEI co-deposited modified PBO fibers.

[0007] This invention is based on an organic surface functionalization method using polyphenol oxidation-amine crosslinking. It utilizes a GA-PEI aqueous co-deposition method to organically modify the surface of PBO fibers. Under weakly alkaline conditions, gallic acid (GA) can be oxidized to generate quinone-based active intermediates, which then undergo Michael addition and Schiff base reactions with primary and secondary amines on the polyethyleneimine (PEI) molecular chain, thereby forming a stable organic network coating on the PBO fiber surface. This organic interfacial coating enhances its bonding with the PBO fiber surface through π-π interactions, hydrogen bonding, and mechanical intercalation. Furthermore, it introduces polar groups such as hydroxyl and amino groups into the fiber surface, increasing the fiber surface energy and wettability with the epoxy resin matrix. This enhances the interfacial adhesion between the fiber and the epoxy resin matrix, improves stress transmission at the fiber / resin interface, reduces interfacial porosity and defects, and helps suppress interfacial moisture absorption and electric field distortion. This improves the mechanical properties, electrical insulation properties, and long-term service stability of the composite core, solving problems such as poor surface adhesion and significant chemical inertness of PBO fibers.

[0008] The modified PBO fiber surface can form a uniform and continuous organic functional layer, improving its interfacial compatibility with epoxy-based lightweight insulation systems while maintaining the lightweight and high-strength characteristics of PBO fibers. Compared with unmodified PBO fiber composites, the resulting composite core exhibits superior flexural and tensile load-bearing capacity, lower interfacial defect sensitivity, lower water absorption tendency, and more stable insulation performance, while maintaining a lower density, thus balancing lightweight, mechanical support, and electrical reliability. This method is simple, has mild reaction conditions, and does not require complex polymerization and fluorination steps, making it suitable for the preparation of lightweight, high-insulation post composite insulator cores.

[0009] In one specific embodiment, the pH value of the weakly alkaline co-deposition modification solution is 8 to 8.5.

[0010] In one specific embodiment, the weakly alkaline co-deposition modification solution is prepared using Tris buffer solution, and the mass ratio of GA to PEI is 0.5 to 0.7.

[0011] In one specific embodiment, the concentration of GA in the weakly alkaline co-deposition modification solution is 0.5–2.0 mg / mL, and the concentration of PEI is 0.25–1.0 mg / mL.

[0012] In one specific embodiment, the reaction conditions for PBO fibers in the weakly alkaline co-deposition modification solution are: reaction at 25–40°C for 2–8 h.

[0013] This invention can adjust the thickness and functional group content of the organic deposition layer on the fiber surface by controlling the concentration, mass ratio and deposition time of GA and PEI, so as to achieve a surface modification effect that balances interfacial bonding and insulation performance.

[0014] In one specific embodiment, the vacuum drying conditions are 60-70°C for 6-12 hours.

[0015] Secondly, the present invention provides a GA-PEI organic co-deposition modified PBO fiber, comprising PBO fiber, wherein a GA-PEI organic functional layer is formed on the surface of the PBO fiber, wherein the GA-PEI organic functional layer is an organic network layer formed by Michael addition and Schiff base reaction of GA to generate quinone active intermediates and primary and secondary amines on the PEI molecular chain after oxidation.

[0016] Thirdly, the present invention provides a lightweight, high-insulation post composite insulator core reinforced with modified PBO fiber, comprising the modified PBO fiber, epoxy resin, PMMA hollow microspheres, curing agent and accelerator.

[0017] In one specific embodiment, the mass ratio of epoxy resin, curing agent and accelerator is 100:80:0.5, the mass fraction of PMMA hollow microspheres is 1%, and the mass fraction of modified PBO fiber is 1~4%.

[0018] Fourthly, the present invention provides a method for preparing the insulator core, comprising the following steps: First, mix epoxy resin, curing agent and accelerator in proportion, then add hollow microspheres to prepare epoxy resin matrix; Modified PBO fibers were added to the epoxy resin matrix and stirred until homogeneous. Pour the well-stirred mixture into a mold and allow it to stand in a high-temperature vacuum environment to complete the degassing and curing process.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The present invention provides a GA-PEI organic co-deposition modified PBO fiber, an insulator core and preparation method, which uses GA / PEI aqueous co-deposition method to organically functionalize the surface of PBO fiber. Under weakly alkaline conditions, a stable organic interface layer is constructed on the surface of PBO fiber through gallic acid oxidation-amine crosslinking reaction, thereby enhancing its interfacial adhesion performance with epoxy resin matrix and solving the problems of poor surface adhesion and significant chemical inertness of PBO fiber. 2. The GA-PEI organic co-deposition modified PBO fiber, insulator core and preparation method provided in the embodiments of the present invention have the advantages of simple process, mild conditions, no introduction of conductive filler, no need for complex polymerization and fluorination steps, and easy scale-up compared with complex polymerization or high temperature grafting methods. It can be used for interface modification of lightweight high insulation post composite insulator core and other PBO fiber reinforced insulation composite materials. 3. The present invention provides a GA-PEI organic co-deposition modified PBO fiber, an insulator core and a preparation method thereof. The resulting composite core can exhibit better bending and tensile load-bearing capacity, lower interface defect sensitivity, lower water absorption tendency and more stable insulation performance, while maintaining a low density, taking into account lightweight, mechanical support and electrical reliability. 4. The present invention provides a GA-PEI organic co-deposition modified PBO fiber, an insulator core and a preparation method thereof. The prepared PBO fiber reinforced epoxy resin composite material has a maximum tensile strength increase of 21.2% and a maximum flexural strength increase of 31.3%. In terms of electrical performance, the leakage current decreases by a maximum of 29.0% and the breakdown voltage increases by a maximum of 26.1%. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly described below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation of the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 The breakdown voltage test diagrams provided by the present invention are as follows; Figure 2 Leakage current test diagrams for embodiments and comparative examples provided by this invention; Figure 3 The tensile strength test diagrams for the embodiments and comparative examples provided by this invention are shown below. Figure 4 The bending strength test diagrams provided by the present invention are for embodiments and comparative examples. Detailed Implementation

[0022] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to the embodiments. The illustrative embodiments and descriptions of this invention are only used to explain this invention and are not intended to limit this invention.

[0023] In the following description, numerous specific details are set forth in order to provide a thorough understanding of the invention. However, it will be apparent to those skilled in the art that these specific details are not necessary to practice the invention. In other embodiments, well-known materials or methods have not been specifically described in order to avoid obscuring the invention.

[0024] Throughout this specification, references to “an embodiment,” “an example,” or “an example” mean that a particular feature, structure, or characteristic described in connection with that embodiment or example is included in at least one embodiment of the invention. Therefore, the phrases “an embodiment,” “an example,” “an example,” or “an example” appearing in various places throughout the specification do not necessarily refer to the same embodiment or example. Furthermore, specific features, structures, or characteristics can be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. The term “and / or” as used herein includes any and all combinations of one or more of the associated listed items.

[0025] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values ​​of 1 and 2 are listed, and if maximum range values ​​of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0026] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.

[0027] Example 1 This invention provides a method for preparing a lightweight, high-insulation post composite insulator core reinforced with GA / PEI organic co-deposition modified PBO fibers, comprising the following steps: (1) Prepare a Tris buffer solution and adjust the pH to 8.5. Then add gallic acid (GA) and polyethyleneimine (PEI) to the buffer solution. The concentration of GA is 0.5 mg / mL and the concentration of PEI is 1 mg / mL. The mass ratio of GA to PEI is 1:2. Stir magnetically at room temperature for 60 min to obtain a uniform GA-PEI co-deposition modified solution. (2) The PBO fibers were washed in anhydrous ethanol and deionized water in sequence to remove surface impurities and residues. The washed PBO fibers were dried in a vacuum oven at 60 °C for 12 h to obtain pretreated PBO fibers. (3) 1% by mass of pretreated PBO fibers were impregnated in the GA / PEI co-deposition modification solution and reacted at room temperature or 40 °C for 8 h. This allowed GA to be oxidized to active quinones in a weakly alkaline environment and to undergo Michael addition and Schiff base reaction with the amino groups on PEI, forming a GA / PEI organic functional layer on the fiber surface. After the reaction, the fibers were removed, washed with deionized water until the washing solution showed no obvious color change, and then vacuum dried at 60 °C for 12 h to obtain the finally activated and modified PBO fibers. (4) E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5, and then 1% by mass of hollow microspheres were added; then 1% by mass of modified PBO fiber was added to the matrix, and the mixture was stirred at a speed of 500 r / min using a vacuum planetary stirrer to ensure that the fiber and the matrix were fully and uniformly mixed. The uniformly stirred mixture was poured into a mold and allowed to stand in a vacuum environment at 90℃ for 10 hours to complete degassing and curing.

[0028] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0029] Example 2 This invention provides a method for preparing a lightweight, high-insulation post composite insulator core reinforced with GA / PEI organic co-deposition modified PBO fibers, comprising the following steps: (1) Prepare a Tris buffer solution and adjust the pH to 8.5. Then add gallic acid (GA) and polyethyleneimine (PEI) to the buffer solution. The concentration of GA is 0.5 mg / mL and the concentration of PEI is 1 mg / mL. The mass ratio of GA to PEI is 1:2. Stir magnetically at room temperature for 60 min to obtain a uniform GA-PEI co-deposition modified solution. (2) The PBO fibers were washed in anhydrous ethanol and deionized water in sequence to remove surface impurities and residues. The washed PBO fibers were dried in a vacuum oven at 60 °C for 12 h to obtain pretreated PBO fibers. (3) 1% by mass of pretreated PBO fibers were impregnated in the GA / PEI co-deposition modification solution and reacted at room temperature or 40 °C for 8 h. This allowed GA to be oxidized to active quinones in a weakly alkaline environment and to undergo Michael addition and Schiff base reaction with the amino groups on PEI, forming a GA / PEI organic functional layer on the fiber surface. After the reaction, the fibers were removed, washed with deionized water until the washing solution showed no obvious color change, and then vacuum dried at 60 °C for 12 h to obtain the finally activated and modified PBO fibers. (4) E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5, and then 1% by mass of hollow microspheres were added; then 2% by mass of modified PBO fiber was added to the matrix, and the mixture was stirred at a speed of 500 r / min using a vacuum planetary stirrer to ensure that the fiber and the matrix were fully and uniformly mixed. The uniformly stirred mixture was poured into a mold and allowed to stand in a vacuum environment at 90℃ for 10 hours to complete degassing and curing.

[0030] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0031] Example 3 This invention provides a method for preparing a lightweight, high-insulation post composite insulator core reinforced with GA / PEI organic co-deposition modified PBO fibers, comprising the following steps: (1) Prepare a Tris buffer solution and adjust the pH to 8.5. Then add gallic acid (GA) and polyethyleneimine (PEI) to the buffer solution. The concentration of GA is 0.5 mg / mL and the concentration of PEI is 1 mg / mL. The mass ratio of GA to PEI is 1:2. Stir magnetically at room temperature for 60 min to obtain a uniform GA-PEI co-deposition modified solution. (2) The PBO fibers were washed in anhydrous ethanol and deionized water in sequence to remove surface impurities and residues. The washed PBO fibers were dried in a vacuum oven at 60 °C for 12 h to obtain pretreated PBO fibers. (3) 1% by mass of pretreated PBO fibers were impregnated in the GA / PEI co-deposition modification solution and reacted at room temperature or 40 °C for 8 h. This allowed GA to be oxidized to active quinones in a weakly alkaline environment and to undergo Michael addition and Schiff base reaction with the amino groups on PEI, forming a GA / PEI organic functional layer on the fiber surface. After the reaction, the fibers were removed, washed with deionized water until the washing solution showed no obvious color change, and then vacuum dried at 60 °C for 12 h to obtain the finally activated and modified PBO fibers. (4) E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5, and then 1% by mass of hollow microspheres were added; then 3% by mass of modified PBO fiber was added to the matrix, and the mixture was stirred at a speed of 500 r / min using a vacuum planetary stirrer to ensure that the fiber and the matrix were fully and uniformly mixed. The uniformly stirred mixture was poured into a mold and allowed to stand in a vacuum environment at 90℃ for 10 hours to complete degassing and curing.

[0032] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0033] Example 4 This invention provides a method for preparing a lightweight, high-insulation post composite insulator core reinforced with GA / PEI organic co-deposition modified PBO fibers, comprising the following steps: (1) Prepare a Tris buffer solution and adjust the pH to 8.5. Then add gallic acid (GA) and polyethyleneimine (PEI) to the buffer solution. The concentration of GA is 0.5 mg / mL and the concentration of PEI is 1 mg / mL. The mass ratio of GA to PEI is 1:2. Stir magnetically at room temperature for 60 min to obtain a uniform GA-PEI co-deposition modified solution. (2) The PBO fibers were washed in anhydrous ethanol and deionized water in sequence to remove surface impurities and residues. The washed PBO fibers were dried in a vacuum oven at 60 °C for 12 h to obtain pretreated PBO fibers. (3) 1% by mass of pretreated PBO fibers were impregnated in the GA / PEI co-deposition modification solution and reacted at room temperature or 40 °C for 8 h. This allowed GA to be oxidized to active quinones in a weakly alkaline environment and to undergo Michael addition and Schiff base reaction with the amino groups on PEI, forming a GA / PEI organic functional layer on the fiber surface. After the reaction, the fibers were removed, washed with deionized water until the washing solution showed no obvious color change, and then vacuum dried at 60 °C for 12 h to obtain the finally activated and modified PBO fibers. (4) E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5, and then 1% by mass of hollow microspheres were added; then 4% by mass of modified PBO fiber was added to the matrix, and the mixture was stirred at a speed of 500 r / min using a vacuum planetary stirrer to ensure that the fiber and the matrix were fully and uniformly mixed. The uniformly stirred mixture was poured into a mold and allowed to stand in a vacuum environment at 90℃ for 10 hours to complete degassing and curing.

[0034] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0035] Comparative Example 1 This comparative example provides a method for preparing a PBO fiber-reinforced lightweight high-insulation post composite insulator core, comprising the following steps: E51 epoxy resin, methyl hexahydrophthalic anhydride (MHHPA) curing agent, and 2,4,6-tris(dimethylaminomethyl)phenol were mixed in a ratio of 100:80:0.5. Then, 1% (by mass) of hollow microspheres were added. The mixture was stirred using a vacuum planetary stirrer at 500 r / min to ensure thorough and uniform mixing. The homogeneous mixture was poured into a mold and allowed to stand under vacuum at 90℃ for 10 hours to complete degassing and curing.

[0036] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0037] Comparative Example 2 This comparative example provides a method for preparing a PBO fiber-reinforced lightweight high-insulation post composite insulator core, comprising the following steps: E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5. Then, 1% (by mass) of hollow microspheres were added, followed by 1% (by mass) of virgin PBO fibers into the matrix. The mixture was stirred using a vacuum planetary mixer at 500 r / min to ensure thorough and uniform mixing of the fibers and matrix. The homogeneous mixture was poured into a mold and allowed to stand under vacuum at 90℃ for 10 hours to complete degassing and curing.

[0038] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0039] Comparative Example 3 This comparative example provides a method for preparing a PBO fiber-reinforced lightweight high-insulation post composite insulator core, comprising the following steps: E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5. Then, 1% (by mass) of hollow microspheres were added, followed by 2% (by mass) of virgin PBO fibers into the matrix. The mixture was stirred using a vacuum planetary stirrer at 500 r / min to ensure thorough and uniform mixing of the fibers and matrix. The homogeneous mixture was poured into a mold and allowed to stand under vacuum at 90℃ for 10 hours to complete degassing and curing.

[0040] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0041] Comparative Example 4 This comparative example provides a method for preparing a PBO fiber-reinforced lightweight high-insulation post composite insulator core, comprising the following steps: E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5. Then, 1% (by mass) of hollow microspheres were added, followed by 3% (by mass) of virgin PBO fibers into the matrix. The mixture was stirred using a vacuum planetary mixer at 500 r / min to ensure thorough and uniform mixing of the fibers and matrix. The homogeneous mixture was poured into a mold and allowed to stand under vacuum at 90℃ for 10 hours to complete degassing and curing.

[0042] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0043] Comparative Example 5 This comparative example provides a method for preparing a PBO fiber-reinforced lightweight high-insulation post composite insulator core, comprising the following steps: E51 epoxy resin and methyl hexahydrophthalic anhydride (MHHPA) curing agent were mixed with 2,4,6-tris(dimethylaminomethyl)phenol in a ratio of 100:80:0.5. Then, 1% (by mass) of hollow microspheres were added, followed by 4% (by mass) of virgin PBO fibers into the matrix. The mixture was stirred using a vacuum planetary mixer at 500 r / min to ensure thorough and uniform mixing of the fibers and matrix. The homogeneous mixture was poured into a mold and allowed to stand under vacuum at 90℃ for 10 hours to complete degassing and curing.

[0044] The cured composite material samples are cut into specified shapes and sizes for performance testing.

[0045] Performance testing The main test items include breakdown strength, leakage current, tensile strength, flexural strength, tensile modulus, and flexural modulus.

[0046] Breakdown strength: The breakdown field strength is used to characterize the electrical resistance of the material. The breakdown strength test electrode is a ball-to-ball electrode. The sample thickness is 1 mm. The electrode and sample must be immersed in dimethyl silicone oil to prevent surface flashover. The test procedure is carried out in accordance with GB / T1408.1-2016. The voltage ramp rate is 2 kV / s. At least 20 samples of each type of specimen are tested, and statistical analysis is performed to obtain the average value.

[0047] Leakage current: The test was conducted in accordance with IEC 62217-2012. To more effectively characterize the leakage current flowing through the interfaces of fibers and resin, and microspheres and resin, copper foil was attached to the surface of the sample as a shielded outer surface current electrode. During the test, an effective value of 12 kV AC power frequency voltage was applied and recorded using a digital multimeter (DM-3068, RGen Technologies Co., Ltd.), with a current accuracy of ±0.1 μA and a sampling frequency of 20 Hz.

[0048] Mechanical properties: Tensile and flexural failure tests were performed on the materials to assess their ultimate tensile strength. Tests were conducted using an ETM-104C general-purpose testing machine, in accordance with standards ISO 527-4 "Plastics—Tensive properties—Determination of tensile strength" and ISO 14125 "Fiber-reinforced plastic composites—Flexural properties". The flexural specimens were 1 mm thick, 15 mm wide, and 40 mm long, with a loading span of 20 mm. The tensile specimens were 1 mm thick, with a gauge length of 50 mm and a 10 mm wide parallel section in the middle. When loading the specimens, the centerline of the specimen was aligned with the centerline of the fixture. The loading rate was 10 mm / min.

[0049] like Figure 1 The breakdown voltage test diagram is shown below: Example 1 is 23.5kV; Example 2 is 24.5kV; Example 3 is 27.9kV; Example 4 is 27.5kV.

[0050] Comparative Example 1 is 21.8kV; Comparative Example 2 is 22.9kV; Comparative Example 3 is 24.0kV; Comparative Example 4 is 27.1kV; Comparative Example 5 is 26.6kV.

[0051] It can be seen that as the amount of modified PBO fiber added increases, the breakdown voltage first increases and then decreases.

[0052] like Figure 2 The leakage current test results are as follows: Example 1 was 34.58 μA; Example 2 was 35.32 μA; Example 3 was 38.69 μA; Example 4 was 43.21 μA; (Examples 1-4 correspond to 1-4% of modified PBO fiber addition).

[0053] Comparative Example 1: 32.45 μA; Comparative Example 2: 38.74 μA; Comparative Example 3: 42.26 μA; Comparative Example 4: 50.43 μA; Comparative Example 5: 55.78 μA. (Comparative Example 1 corresponds to no PBO fiber added, and Comparative Examples 2-5 correspond to 1-4% of PBO fiber added before modification, respectively).

[0054] As can be seen, when added in the same proportion, the modified PBO fiber used in this embodiment of the invention can significantly reduce leakage current.

[0055] like Figure 3 Tensile strength test: Example 1: 682.34 MPa; Example 2: 756.28 MPa; Example 3: 950.64 MPa; Example 4: 809.32 MPa; Comparative Example 1 was 450 MPa; Comparative Example 2 was 576.82 MPa; Comparative Example 3 was 672.75 MPa; Comparative Example 4 was 784.56 MPa; Comparative Example 5 was 685.35 MPa.

[0056] As can be seen, when added in the same proportion, the modified fiber used in this embodiment of the invention significantly increases the tensile strength of the material.

[0057] like Figure 4 Bending strength test: Example 1: 452.66 MPa; Example 2: 544.32 MPa; Example 3: 753.38 MPa; Example 4: 653.65 MPa; Comparative Example 1 was 163.45 MPa; Comparative Example 2 was 302.72 MPa; Comparative Example 3 was 482.98 MPa; Comparative Example 4 was 573.65 MPa; Comparative Example 5 was 506.68 MPa.

[0058] As can be seen, when the same proportion of modified PBO fibers are added, the bending strength of the modified PBO fibers used in the embodiments of the present invention is lower than that of ordinary unmodified PBO fibers when the amount added is low. However, as the amount added increases, the bending strength of the embodiments of the present invention gradually increases and is significantly higher than that of the comparative example.

[0059] The specific embodiments described above further illustrate the purpose, technical solution, and beneficial effects of the present invention. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for preparing GA-PEI organic co-deposition modified PBO fibers, characterized in that, Includes the following steps: Prepare a weakly alkaline co-deposition modification solution containing gallic acid (GA) and polyethyleneimine (PEI); PBO fibers were impregnated in the weakly alkaline co-deposition modification solution and subjected to a shaking reaction. After the reaction was complete, the PBO fibers were removed and vacuum dried to obtain GA-PEI co-deposited modified PBO fibers.

2. The method for preparing GA-PEI organic co-deposition modified PBO fiber according to claim 1, characterized in that, The pH value of the weakly alkaline co-deposition modification solution is 8 to 8.

5.

3. The method for preparing GA-PEI organic co-deposition modified PBO fibers according to claim 1, characterized in that, The weakly alkaline co-deposition modification solution was prepared using Tris buffer solution, with a GA to PEI mass ratio of 0.5 to 0.

7.

4. The method for preparing GA-PEI organic co-deposition modified PBO fiber according to claim 3, characterized in that, The concentration of GA in the weakly alkaline co-deposition modification solution is 0.5–2.0 mg / mL, and the concentration of PEI is 0.25–1.0 mg / mL.

5. The method for preparing GA-PEI organic co-deposition modified PBO fiber according to claim 1, characterized in that, The reaction conditions for PBO fibers in a weakly alkaline co-deposition modification solution are: 30–40℃ for 2–8 h.

6. The method for preparing GA-PEI organic co-deposition modified PBO fiber according to claim 1, characterized in that, The vacuum drying conditions are 60-70℃ for 6-12 hours.

7. A GA-PEI organic co-deposition modified PBO fiber, characterized in that, The product includes PBO fibers, on the surface of which a GA-PEI organic functional layer is formed. The GA-PEI organic functional layer is an organic network layer formed by the Michael addition and Schiff base reaction of primary and secondary amines on the PEI molecular chain after GA is oxidized to generate quinone active intermediates.

8. A lightweight, high-insulation composite insulator core reinforced with modified PBO fiber, characterized in that, It includes the modified PBO fiber, epoxy resin, PMMA hollow microspheres, curing agent and accelerator obtained by any of the methods described in claims 1-6 or as described in claim 7.

9. The modified PBO fiber reinforced lightweight high-insulation post composite insulator core according to claim 8, characterized in that, The mass ratio of epoxy resin, curing agent and accelerator is 100:80:0.5, the mass fraction of PMMA hollow microspheres is 1%, and the mass fraction of modified PBO fiber is 1~4%.

10. The method for preparing the insulator core according to claim 8 or 9, characterized in that, Includes the following steps: First, mix epoxy resin, curing agent and accelerator in proportion, then add hollow microspheres to prepare epoxy resin matrix; Modified PBO fibers were added to the epoxy resin matrix and stirred until homogeneous. Pour the well-stirred mixture into a mold and allow it to stand in a high-temperature vacuum environment to complete the degassing and curing process.