A wrinkle-resistant nylon fabric and its preparation method
By introducing urea bonds and stable bonding structures into nylon fabrics, the problem of nylon fabrics being difficult to restore to their original shape is solved, achieving a balance of wrinkle resistance, softness, and washability, and improving the fabric's deformation recovery ability and dimensional stability.
Patent Information
- Application Number
- CN202611437348.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-17
AI Technical Summary
Existing nylon fabrics are difficult to restore their original shape after being bent, folded or compressed, affecting appearance retention and dimensional stability. Traditional finishing methods cannot simultaneously achieve wrinkle resistance, softness and washability.
An anti-wrinkle modifier was prepared by reacting 6-aminohexanoic acid with isophorone diisocyanate. Urea bonds were introduced by reacting the amino group with the amino group at the chain end of PA6. Combined with L-cysteine-modified 3-isocyanate-propyltriethoxysilane and vinyl-terminated polydimethylsiloxane, hydrogen bonds and stable binding structures were formed to improve the fiber's resilience.
It improves the wrinkle recovery performance of nylon fabric, taking into account both the softness of the fabric and the finishing durability. The molecular chain slippage is restricted inside the fiber through urea bonds, and the surface is improved by a polysiloxane finishing layer.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to the field of textile materials technology, and more specifically, to an anti-wrinkle nylon fabric and its preparation method. Background Technology
[0002] Nylon 6 is characterized by high strength, good abrasion resistance, and excellent fatigue resistance, and it is widely used in clothing and industrial textiles. However, the molecular chains of nylon 6 have a certain degree of flexibility. When the fabric is bent, folded, or compressed, the molecular chain segments and fibers are prone to relative slippage. After the external force is removed, it is difficult to completely restore the original state, which easily leads to wrinkles and affects the fabric's appearance retention and dimensional stability.
[0003] Currently, methods to improve the wrinkle resistance of nylon fabrics mainly include fiber modification and finishing treatment. Simply using resin crosslinking or increasing the degree of crosslinking in the finishing layer can limit fiber deformation, but it can easily cause the fabric to feel stiff and affect the mechanical properties of the fibers. Treatment with conventional organosilicon finishing agents (such as dimethyl silicone oil and polydimethylsiloxane finishing agents) has a good softening effect, but the interaction between them and polyamide fibers mainly relies on physical adsorption, resulting in limited interfacial bonding. Furthermore, the finishing effect tends to decrease after repeated washing.
[0004] Therefore, there is an urgent need to develop a wrinkle-resistant nylon fabric and its preparation method that can improve the wrinkle recovery ability and finishing durability of nylon fabric while maintaining its softness and mechanical properties. Summary of the Invention
[0005] To address the issues of insufficient wrinkle resistance in existing nylon fabrics and the difficulty of balancing wrinkle resistance, softness, and washability using traditional finishing methods, this invention provides a wrinkle-resistant nylon fabric and its preparation method.
[0006] In a first aspect, the present invention provides a method for preparing wrinkle-resistant nylon fabric, employing the following technical solution:
[0007] A method for preparing wrinkle-resistant nylon fabric includes the following steps:
[0008] S1. Under nitrogen protection, 6-aminohexanoic acid is added to anhydrous N,N-dimethylformamide, stirred evenly, cooled to 10-15℃, isophorone diisocyanate is added, and the mixture is stirred to react. After the reaction is completed, the mixture is precipitated, filtered, washed, dried, pulverized and sieved to obtain the anti-wrinkle modifier.
[0009] S2. Mix ε-caprolactam, anti-wrinkle modifier, benzoic acid and deionized water, stir and react. After the reaction is completed, extrude, cool, granulate, and then dry after hot water extraction to obtain modified PA6 chips.
[0010] S3. Modified PA6 chips are melt-spun to obtain modified PA6 fibers; the modified PA6 fibers are woven, washed, and dried to obtain nylon fabric.
[0011] S4. Immerse the nylon fabric in the anti-wrinkle finishing solution and perform padding treatment. After the treatment is completed, perform pre-drying and baking treatment in sequence. After the treatment is completed, cool to obtain anti-wrinkle nylon fabric.
[0012] Preferably, in step S1, the mass ratio of 6-aminohexanoic acid, isophorone diisocyanate, and anhydrous N,N-dimethylformamide is 1:0.8-0.9:8-10.
[0013] Preferably, the term "stirring evenly" in step S1 refers to stirring for 30-40 minutes at a temperature of 20-25℃ and a rotation speed of 600-800 r / min.
[0014] Preferably, the stirring reaction in step S1 refers to: stirring the reaction for 40-60 minutes at a temperature of 10-15℃ and a rotation speed of 700-900 r / min; then raising the temperature to 30-35℃ and continuing the stirring reaction for 3-4 hours at a rotation speed of 600-800 r / min.
[0015] Preferably, in step S1, precipitation, filtration, washing, and drying refer to: cooling the reaction solution to 20-25°C, adding 4-6 times the mass of deionized water at a speed of 400-600 r / min, stirring for 20-30 min after addition, adjusting the pH of the system to 3.0-3.5 with 1.0 mol / L hydrochloric acid aqueous solution, and stirring for 40-60 min at a temperature of 5-10°C and a speed of 300-500 r / min to precipitate the precipitate; then filtering with a polypropylene filter cloth with a pore size of 10-20 μm, washing the filter cake 2-3 times with deionized water at a temperature of 5-10°C, and drying at a temperature of 50-55°C for 8-10 h.
[0016] Preferably, in step S1, the crushing and sieving refers to: using a high-speed crusher, crushing for 1-2 minutes at a speed of 8000-10000 r / min, and then passing it through an 80-100 mesh sieve.
[0017] Preferably, in step S2, the mass ratio of ε-caprolactam, anti-wrinkle modifier, benzoic acid and deionized water is 100:1.0-1.2:0.08-0.12:3-4.
[0018] Preferably, the stirring reaction in step S2 refers to: under nitrogen protection, first heating to 85-90℃ and stirring at 150-200 r / min for 30-40 min; then heating to 245-250℃ at a heating rate of 80-100℃ / h and holding the reaction at 120-160 r / min for 2.0-2.5 h, during which the pressure inside the reactor is controlled at 0.8-1.0 MPa through an exhaust valve; then, under the conditions of 248-252℃ and 100-140 r / min, the pressure inside the reactor is released to atmospheric pressure within 40-60 min; after the pressure is released, heating to 250-255℃ and continuing stirring at 60-100 r / min for 3-4 h.
[0019] Preferably, in step S2, the extrusion, cooling, and pelletizing process refers to: introducing the reaction system into a screw extruder, controlling the screw speed at 30-50 r / min and the die head temperature at 250-255℃, filtering it through an 80-100 mesh stainless steel melt filter, and extruding it through a discharge hole with a pore size of 2.5-3.0 mm to form strips; cooling the strips in circulating deionized water at a temperature of 20-25℃, drawing them at a traction speed of 8-12 m / min, and then pelletizing them using a pelletizer at a speed of 600-800 r / min to obtain modified PA6 particles with a length of 2.5-3.5 mm.
[0020] Preferably, the drying process after hot water extraction in step S2 refers to: mixing modified PA6 particles and deionized water at a mass ratio of 1:18-20, and extracting for 10-12 hours at a temperature of 95-98℃ and a rotation speed of 80-100 r / min, replacing an equal amount of deionized water every 3-4 hours during the extraction process; after extraction, filtering with a stainless steel filter screen with a pore size of 0.5-1.0 mm, washing the filter cake 1-2 times with deionized water at a temperature of 60-70℃, and then drying to a moisture content ≤0.06% at a temperature of 105-110℃ and a vacuum degree of -0.085MPa to -0.095MPa.
[0021] Preferably, in step S3, the melt spinning process involves: adding modified PA6 chips into a melt spinning machine for melt spinning; controlling the screw speed to be 50-70 r / min, the extruder feed section temperature to be 245-250℃, the compression section temperature to be 250-255℃, the melt section temperature to be 255-260℃, and the spinning box temperature to be 258-262℃; after filtration through a sintered stainless steel filter element with a pore size of 20-30 μm, the product is delivered by a metering pump to 24 spinneret holes with a spinneret hole diameter of 0.20 μm. The spinneret assembly extrudes nascent fibers through the spinneret orifices; the nascent fibers are cooled by side-blowing air at a temperature of 20-24℃, relative humidity of 65-70%, and wind speed of 0.4-0.5m / s, and wound at a speed of 900-1100m / min; then hot drawing is performed, controlling the temperature of the first drawing roller at 80-90℃ and the temperature of the second drawing roller at 120-130℃, with a total draw ratio of 3.2-3.5 times; after drawing, heat setting is performed at a temperature of 155-165℃ for 20-30s.
[0022] Preferably, in step S3, the weaving, washing, and drying process refers to: plain weaving the modified PA6 fibers at a loom speed of 320-380 r / min to obtain a basis weight of 100-120 g / m². 2 The nylon fabric is washed at a mass ratio of 1:18-20 with the washing liquid. The nylon fabric is added to the washing liquid and washed for 20-30 minutes at a temperature of 55-60℃ and a rotation speed of 80-120 r / min. After washing, the nylon fabric is removed and rinsed 2-3 times with deionized water at a temperature of 25-30℃, each time for 5-10 minutes. After rinsing, the fabric is dried at a temperature of 80-85℃ for 30-40 minutes.
[0023] Preferably, the washing solution is a deionized aqueous solution containing 1.0-1.5 g / L AEO-9.
[0024] Preferably, the mass ratio of nylon fabric to anti-wrinkle finishing liquid in step S4 is 1:18-20.
[0025] Preferably, the padding process in step S4 refers to: immersing the nylon fabric in an anti-wrinkle finishing solution and performing a double dip and padding process at a temperature of 25-30℃, with each dip lasting 3-5 minutes; wherein, after each dip, the fabric is rolled by a rolling mill with a roll pressure of 0.20-0.30 MPa, a roll running speed of 1-2 m / min, and the roll allowance is controlled to be 70-80%.
[0026] Preferably, the pre-drying and baking treatment in step S4 refers to: pre-drying the impregnated nylon fabric at a temperature of 85-90℃ for 3-4 minutes, and then baking it at 150-155℃ for 2-3 minutes.
[0027] Preferably, the preparation method of the anti-wrinkle finishing solution includes the following steps:
[0028] A1. Under nitrogen protection, L-cysteine was added to anhydrous N,N-dimethylformamide, stirred until homogeneous, cooled to 10-15℃, and 3-isocyanate-propyltriethoxysilane was added. The mixture was heated and stirred to react. After the reaction was completed, the modified silane intermediate was obtained through post-treatment.
[0029] A2. Under nitrogen protection, vinyl-terminated polydimethylsiloxane was added to a mixed solvent, along with a modified silane intermediate and azobisisobutyronitrile. The mixture was stirred and reacted. After the reaction was completed, the mixture was cooled and concentrated under reduced pressure to obtain functionalized polydimethylsiloxane.
[0030] A3. Mix the emulsifier and deionized water, add the functionalized polydimethylsiloxane while stirring, and after the addition is complete, shear emulsify, then add the wetting agent and penetrant, stir evenly, adjust the pH of the system to 5.0-5.5, continue to stir evenly, and let it stand to mature to obtain the anti-wrinkle finishing solution.
[0031] Preferably, in step A1, the mass ratio of L-cysteine, 3-isocyanate-propyltriethoxysilane, and anhydrous N,N-dimethylformamide is 1:1.9-2.1:8-10.
[0032] Preferably, the term "stirring evenly" in step A1 refers to stirring for 20-30 minutes at a temperature of 20-25℃ and a rotation speed of 500-700 r / min.
[0033] Preferably, the heating and stirring reaction in step A1 refers to heating to 25-30℃ and stirring at a speed of 500-700 r / min for 4-6 hours.
[0034] Preferably, the post-treatment in step A1 refers to: concentrating the solution under reduced pressure to 30-40% of the reaction liquid volume at a temperature of 40-45℃ and a vacuum degree of -0.085MPa to -0.095MPa to obtain a concentrated solution; then adding 4-5 times the volume of anhydrous ethyl acetate at a rotation speed of 300-500r / min to precipitate the solution; filtering with a polytetrafluoroethylene filter membrane with a pore size of 5-10μm; washing the filter cake with anhydrous ethyl acetate 2-3 times; and drying it at a temperature of 40-45℃ for 6-8 hours.
[0035] Preferably, in step A2, the mass ratio of vinyl-terminated polydimethylsiloxane, modified silane intermediate, azobisisobutyronitrile, and mixed solvent is 1:0.50-0.60:0.008-0.012:4-5.
[0036] Preferably, the mixed solvent in step A2 is composed of anhydrous ethyl acetate and anhydrous toluene mixed in a volume ratio of 1:0.8-1.2.
[0037] Preferably, the stirring reaction in step A2 refers to: first stirring the reaction at a temperature of 20-25℃ and a rotation speed of 500-700 r / min for 20-30 min, then raising the temperature to 64-68℃ and continuing the stirring reaction at a rotation speed of 600-800 r / min for 8-10 h.
[0038] Preferably, the vacuum concentration in step A2 refers to vacuum concentration for 2-3 hours under vacuum conditions of -0.085MPa to -0.095MPa.
[0039] Preferably, in step A3, the mass ratio of emulsifier, functionalized polydimethylsiloxane, wetting agent, penetrant and deionized water is 1.6-1.8:9-10:0.15-0.20:0.15-0.20:89-91.
[0040] Preferably, the emulsifier in step A3 is AEO-9.
[0041] Preferably, the wetting agent in step A3 is a nonionic wetting agent of acetylenol polyoxyethylene ether.
[0042] Preferably, the penetrant in step A3 is penetrant JFC.
[0043] Preferably, the addition of functionalized polydimethylsiloxane in step A3 specifically involves adding functionalized polydimethylsiloxane at a temperature of 30-35℃ and a rotation speed of 800-1000 r / min, with the addition time controlled to be 15-20 min.
[0044] Preferably, in step A3, shear emulsification refers to: using a high-speed shear emulsifier, shear emulsifying for 15-20 minutes at a temperature of 30-35℃ and a rotation speed of 8000-10000 r / min.
[0045] Preferably, the term "stirring evenly" in step A3 refers to stirring for 20-30 minutes at a temperature of 25-30℃ and a rotation speed of 500-700 r / min.
[0046] Preferably, in step A3, "continue stirring until homogeneous" means stirring for 20-30 minutes at a temperature of 25-30℃ and a rotation speed of 400-600 r / min.
[0047] Preferably, the static curing in step A3 refers to: static curing at a temperature of 20-25℃ for 2-4 hours.
[0048] Secondly, the present invention provides an anti-wrinkle nylon fabric, which adopts the following technical solution:
[0049] A wrinkle-resistant nylon fabric prepared by the above-mentioned method.
[0050] In summary, the present invention has the following beneficial effects:
[0051] 1. This invention prepares an anti-wrinkle modifier by reacting 6-aminohexanoic acid with isophorone diisocyanate. The amino group reacts with the isocyanate group to form a urea bond, while retaining the carboxyl group. This anti-wrinkle modifier can be introduced into the PA6 molecular chain during ε-caprolactam polymerization through the reaction of the carboxyl group with the terminal amino group of PA6. The introduced urea group can form hydrogen bonds with the PA6 amide group, and the isophorone alicyclic structure can restrict molecular chain segment slippage, thereby improving the deformation recovery ability and dimensional stability of PA6 fibers.
[0052] 2. This invention uses L-cysteine to modify 3-isocyanate-propyltriethoxysilane. The amino group in L-cysteine reacts with the isocyanate group to form a urea bond, while retaining the thiol and carboxyl groups. Subsequently, under the initiation of azobisisobutyronitrile, the thiol group undergoes a thiol-olefin addition reaction with the vinyl-terminated polydimethylsiloxane, grafting functional segments containing carboxyl, urea, and triethoxysilane groups onto the polydimethylsiloxane chain ends. The carboxyl and urea groups enhance the hydrogen bonding and interfacial affinity between the finishing agent and the PA6 amide segments, the triethoxysilane group forms a stable bond structure through hydrolysis and condensation on the fiber surface, and the polydimethylsiloxane segments maintain the flexibility of the finishing layer, giving the nylon fabric wrinkle resistance, washability, and softness.
[0053] 3. The functionalized polydimethylsiloxane obtained in this invention contains urea, carboxyl, and triethoxysilyl groups. The urea and carboxyl groups can form hydrogen bonds and polar interactions with the amide groups on the PA6 surface. The triethoxysilyl groups hydrolyze in the aqueous phase to form silanol groups, and further condense during the pre-drying and baking processes to form a Si-O-Si structure, thereby improving the film-forming properties and fixation strength of the finishing agent on the PA6 fiber surface, which is beneficial to improving the water wash stability of the anti-wrinkle finishing effect.
[0054] 4. This invention combines PA6 bulk modification with fabric surface finishing. Irreversible molecular chain slippage is restricted within the fiber via urea-hydrogen bonds and alicyclic structures, while a flexible polysiloxane finishing layer improves the resilience of the fiber and yarn. The combined effect enhances the wrinkle recovery performance of nylon fabric while maintaining both fabric softness and finishing durability. Detailed Implementation
[0055] The present invention will be further described in detail below with reference to the embodiments.
[0056] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.
[0057] The key raw materials used in this invention are sourced from the following sources:
[0058] 3-Isocyanate-propyltriethoxysilane was purchased from Hubei Kefule Materials Technology Co., Ltd., CAS No.: 24801-88-5;
[0059] Vinyl-terminated polydimethylsiloxane was purchased from Wuhan Lanabai Pharmaceutical Chemical Co., Ltd., CAS No.: 68083-19-2;
[0060] The nonionic wetting agent of acetylacetonate diol polyoxyethylene ether (2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate) was purchased from Hubei Qiansheng Biotechnology Co., Ltd., CAS No.: 9014-85-1.
[0061] PA6 chips were purchased from Shanghai Zhaoken New Materials Co., Ltd., brand: Juheshun, model: 2500Z.
[0062] Examples 1-3 provide an anti-wrinkle nylon fabric and its preparation method.
[0063] Example 1
[0064] The preparation method of the anti-wrinkle finishing solution includes the following steps:
[0065] A1. Controlling the mass ratio of L-cysteine, 3-isocyanopropyltriethoxysilane, and anhydrous N,N-dimethylformamide to 1:1.9:8, under nitrogen protection, L-cysteine was added to anhydrous N,N-dimethylformamide and stirred for 30 minutes at 20°C and 500 r / min. The mixture was then cooled to 10°C, and 3-isocyanopropyltriethoxysilane was added at 600 r / min over a period of 30 minutes. After addition, the temperature was increased. The mixture was stirred at 500 r / min for 6 h at 25 °C. After the reaction was completed, it was concentrated under reduced pressure to 30% of the reaction liquid volume at 40 °C and -0.085 MPa to obtain a concentrated solution. Then, anhydrous ethyl acetate, four times the volume of the concentrated solution, was added at 300 r / min to precipitate the precipitate. The solution was filtered using a polytetrafluoroethylene (PTFE) membrane with a pore size of 5 μm. The filter cake was washed twice with anhydrous ethyl acetate and dried at 40 °C for 8 h to obtain a modified silane intermediate.
[0066] A2. The mass ratio of vinyl-terminated polydimethylsiloxane, modified silane intermediate, azobisisobutyronitrile, and mixed solvent was controlled at 1:0.50:0.008:4. Under nitrogen protection, vinyl-terminated polydimethylsiloxane was added to the mixed solvent (composed of anhydrous ethyl acetate and anhydrous toluene in a volume ratio of 1:0.8). Modified silane intermediate and azobisisobutyronitrile were added. The mixture was stirred at 20°C and 500 r / min for 30 min, then heated to 64°C and stirred at 600 r / min for 10 h. After the reaction was completed, the mixture was cooled to 45°C and concentrated under reduced pressure for 3 h at a vacuum of -0.085 MPa to obtain functionalized polydimethylsiloxane.
[0067] A3. The mass ratio of AEO-9, functionalized polydimethylsiloxane, 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, penetrant JFC, and deionized water was controlled at 1.6:9:0.15:0.15:89. AEO-9 and deionized water were mixed, and functionalized polydimethylsiloxane was added at 30℃ and 800 r / min over a time of 15 min. After addition, a high-speed shear emulsifier was used at 30℃ and 800 r / min. Shear emulsification was performed at 8000 r / min for 20 min, followed by the addition of 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, and penetrant JFC. The mixture was stirred at 25°C and 500 r / min for 30 min. The pH of the system was adjusted to 5.0 using a 10% acetic acid aqueous solution. The mixture was stirred for another 30 min at 25°C and 400 r / min. Finally, the mixture was allowed to stand at 20°C for 4 h to mature, yielding the anti-wrinkle finishing solution.
[0068] A method for preparing wrinkle-resistant nylon fabric includes the following steps:
[0069] S1. Controlling the mass ratio of 6-aminohexanoic acid, isophorone diisocyanate, and anhydrous N,N-dimethylformamide to 1:0.8:8, under nitrogen protection, 6-aminohexanoic acid was added to anhydrous N,N-dimethylformamide and stirred for 40 min at 20℃ and 600 r / min. The mixture was then cooled to 10℃, and isophorone diisocyanate was added at 700 r / min over a period of 30 min. After addition, the mixture was stirred for 60 min at 10℃ and 700 r / min. Subsequently, the temperature was raised to 30℃, and the reaction was continued at 600 r / min for 4 h. After the reaction was completed, the reaction solution was cooled to 20°C. Four times the mass of deionized water was added at 400 rpm. After addition, stirring was continued for 30 min. The pH of the system was then adjusted to 3.0 using a 1.0 mol / L hydrochloric acid solution. Stirring continued for 60 min at 5°C and 300 rpm to precipitate the precipitate. The precipitate was then filtered through a 10 μm pore size polypropylene filter cloth. The filter cake was washed twice with deionized water at 5°C, dried at 50°C for 10 h, and then pulverized for 2 min at 8000 rpm using a high-speed pulverizer. Finally, it was passed through an 80-mesh sieve to obtain the anti-wrinkle modifier.
[0070] S2. Controlling the mass ratio of ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water to 100:1.0:0.08:3, mix the ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water. Under nitrogen protection, first heat to 85℃ and stir at 150 r / min for 40 min; then heat to 245℃ at a rate of 80℃ / h and maintain the temperature at 120 r / min for 2.5 h. During the reaction, control the pressure inside the reactor to 0.8 MPa through the exhaust valve. Then, at 248℃ and 100 r / min, depressurize the reactor to atmospheric pressure within 40 min. After depressurization, heat to 250℃ and continue stirring at 60 r / min for 4 h. After the reaction, transfer the reaction system to a screw extruder, controlling the screw speed at 30 r / min and the die head temperature at 25℃. At 0℃, the material is filtered through an 80-mesh stainless steel melt filter and extruded through a 2.5mm aperture outlet to form strips. The strips are then cooled in circulating deionized water at 20℃ and drawn at a traction speed of 8m / min. Subsequently, they are pelletized using a pelletizer at a speed of 600r / min to obtain modified PA6 particles with a length of 2.5mm. The modified PA6 particles and deionized water are mixed at a mass ratio of 1:18 and extracted at 95℃ and a speed of 80r / min for 12 hours, with an equal amount of deionized water replaced every 3 hours during the extraction process. After extraction, the mixture is filtered through a 0.5mm aperture stainless steel filter. The filter cake is washed once with deionized water at 60℃ and then dried at 105℃ and a vacuum of -0.085MPa until the moisture content is ≤0.06%, yielding modified PA6 chips.
[0071] S3. Modified PA6 chips are added to a melt spinning machine for melt spinning; the screw speed is controlled at 50 r / min, the extruder feed section temperature is 245℃, the compression section temperature is 250℃, the melting section temperature is 255℃, and the spinning box temperature is 258℃; after filtration through a sintered stainless steel filter with a pore size of 20μm, the fibers are delivered by a metering pump to a spinneret with 24 spinneret holes and a spinneret hole diameter of 0.20mm, and extruded through the spinneret holes to form nascent fibers; the temperature is 20℃. The nascent fibers were cooled by a side-blowing airflow with a relative humidity of 65% and a wind speed of 0.4 m / s, and then wound at a speed of 900 m / min. Subsequently, hot drawing was performed, with the temperature of the first drawing roller controlled at 80℃ and the temperature of the second drawing roller at 120℃, resulting in a total draw ratio of 3.2. After drawing, the fibers were heat-set at 155℃ for 30 seconds to obtain modified PA6 fibers. The modified PA6 fibers were then plain-weave at a loom speed of 320 r / min, yielding a basis weight of 100 g / m². 2The nylon fabric was added to the washing solution (a deionized water solution containing 1.0 g / L AEO-9) at a mass ratio of 1:18. The nylon fabric was washed for 30 minutes at a temperature of 55℃ and a rotation speed of 80 r / min. After washing, the nylon fabric was removed and rinsed twice with deionized water at a temperature of 25℃ for 10 minutes each time. After rinsing, the fabric was dried at a temperature of 80℃ for 40 minutes to obtain the nylon fabric.
[0072] S4. Control the mass ratio of nylon fabric to anti-wrinkle finishing solution to 1:18. Immerse the nylon fabric in the anti-wrinkle finishing solution and perform a two-dip and two-ply treatment at 25℃, with each immersion lasting 5 minutes. After each immersion, the fabric is rolled by a rolling mill with a roll pressure of 0.20 MPa and a roll speed of 1 m / min, and the roll allowance is controlled at 70%. After the treatment, the nylon fabric after the padding treatment is pre-dried at 85℃ for 4 minutes, and then heated to 150℃ for 3 minutes. After the baking is completed, it is cooled to room temperature to obtain the anti-wrinkle nylon fabric.
[0073] Example 2
[0074] The preparation method of the anti-wrinkle finishing solution includes the following steps:
[0075] A1. Controlling the mass ratio of L-cysteine, 3-isocyanopropyltriethoxysilane, and anhydrous N,N-dimethylformamide to 1:2.0:9, under nitrogen protection, L-cysteine was added to anhydrous N,N-dimethylformamide and stirred for 25 min at 23℃ and 600 r / min. The mixture was then cooled to 13℃, and 3-isocyanopropyltriethoxysilane was added at 700 r / min over a time of 35 min. After addition, the temperature was raised to... The mixture was stirred at 28℃ and 600 r / min for 5 h. After the reaction was completed, it was concentrated under reduced pressure at 43℃ and -0.090 MPa to 35% of the reaction liquid volume to obtain a concentrated solution. Then, 4.5 times the volume of anhydrous ethyl acetate was added at 400 r / min to precipitate the solution. The solution was filtered using a polytetrafluoroethylene membrane with an 8 μm pore size. The filter cake was washed three times with anhydrous ethyl acetate and dried at 43℃ for 7 h to obtain a modified silane intermediate.
[0076] A2. The mass ratio of vinyl-terminated polydimethylsiloxane, modified silane intermediate, azobisisobutyronitrile, and mixed solvent was controlled at 1:0.55:0.01:4.5. Under nitrogen protection, vinyl-terminated polydimethylsiloxane was added to the mixed solvent (composed of anhydrous ethyl acetate and anhydrous toluene in a volume ratio of 1:1), modified silane intermediate and azobisisobutyronitrile were added, and the mixture was stirred at 23℃ and 600 r / min for 25 min. Then the temperature was raised to 66℃ and the mixture was stirred at 700 r / min for 9 h. After the reaction was completed, the mixture was cooled to 48℃ and concentrated under reduced pressure for 2.5 h under a vacuum of -0.090 MPa to obtain functionalized polydimethylsiloxane.
[0077] A3. The mass ratio of AEO-9, functionalized polydimethylsiloxane, 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, penetrant JFC, and deionized water was controlled at 1.7:9.5:0.18:0.18:90. AEO-9 and deionized water were mixed, and functionalized polydimethylsiloxane was added at 33℃ and 900 r / min over a time of 17.5 min. After addition, a high-speed shear emulsifier was used at 32℃ and 900 r / min. Shear emulsification was performed at 9000 r / min for 17.5 min, followed by the addition of 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, and penetrant JFC. The mixture was stirred at 28°C and 600 r / min for 25 min. The pH of the system was adjusted to 5.3 using a 10% acetic acid aqueous solution. The mixture was stirred at 28°C and 500 r / min for another 25 min. Finally, the mixture was allowed to stand at 22°C for 3 h to mature, yielding the anti-wrinkle finishing solution.
[0078] A method for preparing wrinkle-resistant nylon fabric includes the following steps:
[0079] S1. Controlling the mass ratio of 6-aminohexanoic acid, isophorone diisocyanate, and anhydrous N,N-dimethylformamide to 1:0.85:9, under nitrogen protection, 6-aminohexanoic acid was added to anhydrous N,N-dimethylformamide and stirred for 35 min at 22℃ and 700 r / min. The temperature was then lowered to 13℃, and isophorone diisocyanate was added at 800 r / min over a period of 35 min. After addition, the mixture was stirred for 50 min at 13℃ and 800 r / min. Subsequently, the temperature was raised to 32℃, and the reaction was continued at 700 r / min for 3.5 h. After the reaction was completed, the reaction solution was cooled to 22°C. Five times the mass of deionized water was added at 500 rpm. After addition, stirring was continued for 25 min. The pH of the system was then adjusted to 3.2 using a 1.0 mol / L hydrochloric acid solution. Stirring continued for 50 min at 8°C and 400 rpm to precipitate the product. The product was then filtered through a 15 μm polypropylene filter cloth. The filter cake was washed three times with deionized water at 8°C, dried at 52°C for 9 h, and then pulverized for 1.5 min at 9000 rpm using a high-speed pulverizer. Finally, it was passed through a 90-mesh sieve to obtain the anti-wrinkle modifier.
[0080] S2. Controlling the mass ratio of ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water to 100:1.1:0.1:3.5, mix the ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water. Under nitrogen protection, first heat to 88℃ and stir at 180 r / min for 35 min; then heat to 248℃ at a rate of 90℃ / h and maintain the temperature at 140 r / min for 2.25 h. During the reaction, control the pressure inside the reactor to 0.9 MPa through the exhaust valve. Then, at 250℃ and 120 r / min, depressurize the reactor to atmospheric pressure within 50 min. After depressurization, heat to 252℃ and continue stirring at 80 r / min for 3.5 h. After the reaction, transfer the reaction system to a screw extruder, controlling the screw speed at 40 r / min and the die head temperature at 25℃. At 2℃, the material is filtered through a 90-mesh stainless steel melt filter and extruded through a 2.8mm aperture outlet to form strips. The strips are then cooled in circulating deionized water at 23℃ and drawn at a traction speed of 10m / min. Subsequently, they are pelletized using a pelletizer at a speed of 700r / min to obtain modified PA6 particles with a length of 3.0mm. The modified PA6 particles and deionized water are mixed at a mass ratio of 1:19 and extracted at 96℃ and a speed of 90r / min for 11h. During the extraction process, an equal amount of deionized water is replaced every 3.5h. After extraction, the mixture is filtered through a 0.7mm aperture stainless steel filter. The filter cake is washed twice with deionized water at 65℃ and then dried at 108℃ and a vacuum of -0.090MPa until the moisture content is ≤0.06%, resulting in modified PA6 chips.
[0081] S3. Modified PA6 chips are added to a melt spinning machine for melt spinning; the screw speed is controlled at 60 r / min, the extruder feed section temperature is 248℃, the compression section temperature is 252℃, the melting section temperature is 258℃, and the spinning box temperature is 260℃; after filtration through a sintered stainless steel filter element with a pore size of 25μm, the fibers are delivered by a metering pump to a spinneret with 24 spinneret holes and a spinneret hole diameter of 0.20mm, and extruded through the spinneret holes to form nascent fibers; a temperature of 22℃ is used. The nascent fibers were cooled by a side-blowing airflow with a relative humidity of 68% and a wind speed of 0.45 m / s, and then wound at a speed of 1000 m / min. Subsequently, hot drawing was performed, with the temperature of the first drawing roller controlled at 85℃ and the temperature of the second drawing roller at 125℃, resulting in a total draw ratio of 3.3. After drawing, the fibers were heat-set at 160℃ for 25 seconds to obtain modified PA6 fibers. The modified PA6 fibers were then plain-weave at a loom speed of 350 r / min, yielding a basis weight of 110 g / m². 2The nylon fabric was added to the washing solution (a deionized water solution containing 1.25 g / L AEO-9) at a mass ratio of 1:19. The nylon fabric was washed for 25 minutes at a temperature of 58℃ and a rotation speed of 100 r / min. After washing, the nylon fabric was removed and rinsed three times with deionized water at a temperature of 28℃ for 7.5 minutes each time. After rinsing, the fabric was dried at a temperature of 83℃ for 35 minutes to obtain the nylon fabric.
[0082] S4. Control the mass ratio of nylon fabric to anti-wrinkle finishing solution to 1:19. Immerse the nylon fabric in the anti-wrinkle finishing solution and perform a two-dip and two-ply treatment at 28℃, with each immersion lasting 4 minutes. After each immersion, the fabric is rolled by a rolling mill with a roll pressure of 0.25 MPa and a roll speed of 1.5 m / min, and the roll residue is controlled at 75%. After the treatment, the nylon fabric is pre-dried at 88℃ for 3.5 minutes, and then heated to 153℃ for 2.5 minutes. After calcination, the fabric is cooled to room temperature to obtain the anti-wrinkle nylon fabric.
[0083] Example 3
[0084] The preparation method of the anti-wrinkle finishing solution includes the following steps:
[0085] A1. Controlling the mass ratio of L-cysteine, 3-isocyanopropyltriethoxysilane, and anhydrous N,N-dimethylformamide to 1:2.1:10, under nitrogen protection, L-cysteine was added to anhydrous N,N-dimethylformamide and stirred for 20 min at 25℃ and 700 r / min. The mixture was then cooled to 15℃, and 3-isocyanopropyltriethoxysilane was added at 800 r / min over a time of 40 min. After addition, the temperature was increased. The mixture was stirred at 700 r / min for 4 h at 30 °C. After the reaction was completed, it was concentrated under reduced pressure to 40% of the reaction liquid volume at 45 °C and a vacuum of -0.095 MPa to obtain a concentrated solution. Then, anhydrous ethyl acetate, five times the volume of the concentrated solution, was added at 500 r / min to precipitate the precipitate. The solution was filtered using a polytetrafluoroethylene (PTFE) membrane with a pore size of 10 μm. The filter cake was washed three times with anhydrous ethyl acetate and dried at 45 °C for 6 h to obtain a modified silane intermediate.
[0086] A2. The mass ratio of vinyl-terminated polydimethylsiloxane, modified silane intermediate, azobisisobutyronitrile, and mixed solvent was controlled at 1:0.60:0.012:5. Under nitrogen protection, vinyl-terminated polydimethylsiloxane was added to the mixed solvent (composed of anhydrous ethyl acetate and anhydrous toluene in a volume ratio of 1:1.2). Modified silane intermediate and azobisisobutyronitrile were added. The mixture was stirred at 25°C and 700 r / min for 20 min, then heated to 68°C and stirred at 800 r / min for 8 h. After the reaction was completed, the mixture was cooled to 50°C and concentrated under reduced pressure at -0.095 MPa for 2 h to obtain functionalized polydimethylsiloxane.
[0087] A3. The mass ratio of AEO-9, functionalized polydimethylsiloxane, 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, penetrant JFC, and deionized water was controlled at 1.8:10:0.20:0.20:91. AEO-9 and deionized water were mixed, and functionalized polydimethylsiloxane was added at 35℃ and 1000 r / min over a time of 20 min. After addition, a high-speed shear emulsifier was used at 35℃ and 1000 r / min. Shear emulsification was performed at 10,000 r / min for 15 min, followed by the addition of 2,4,7,9-tetramethyl-5-decyn-4,7-diol, ethoxylate, and penetrant JFC. The mixture was stirred at 30°C and 700 r / min for 20 min. The pH of the system was adjusted to 5.5 using a 10% acetic acid aqueous solution. The mixture was stirred at 30°C and 600 r / min for another 20 min. Finally, the mixture was allowed to stand and mature at 25°C for 2 h to obtain the anti-wrinkle finishing solution.
[0088] A method for preparing wrinkle-resistant nylon fabric includes the following steps:
[0089] S1. Controlling the mass ratio of 6-aminohexanoic acid, isophorone diisocyanate, and anhydrous N,N-dimethylformamide to 1:0.9:10, under nitrogen protection, 6-aminohexanoic acid was added to anhydrous N,N-dimethylformamide and stirred for 30 min at 25℃ and 800 r / min. The temperature was then lowered to 15℃, and isophorone diisocyanate was added at 900 r / min over a period of 40 min. After addition, the reaction was stirred for 40 min at 15℃ and 900 r / min. Subsequently, the temperature was raised to 35℃, and the reaction was continued at 800 r / min for 3 h. The reaction result was... After the reaction was completed, the reaction solution was cooled to 25°C. Deionized water, six times the mass of the reaction solution, was added at 600 rpm. After addition, stirring was continued for 20 min. The pH of the system was then adjusted to 3.5 using a 1.0 mol / L hydrochloric acid solution. Stirring continued for 40 min at 10°C and 500 rpm to precipitate the product. The precipitate was then filtered through a 20 μm polypropylene filter cloth. The filter cake was washed three times with deionized water at 10°C, dried at 55°C for 8 h, and then pulverized for 1 min at 10000 rpm using a high-speed pulverizer. Finally, it was passed through a 100-mesh sieve to obtain the anti-wrinkle modifier.
[0090] S2. Controlling the mass ratio of ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water to 100:1.2:0.12:4, mix the ε-caprolactam, anti-wrinkle modifier, benzoic acid, and deionized water. Under nitrogen protection, first heat to 90℃ and stir at 200 r / min for 30 min; then heat to 250℃ at a rate of 100℃ / h and maintain the temperature at 160 r / min for 2.0 h. During the reaction, control the pressure inside the reactor to 1.0 MPa through the exhaust valve. Then, at 252℃ and 140 r / min, depressurize the reactor to atmospheric pressure within 60 min. After depressurization, heat to 255℃ and continue stirring at 100 r / min for 3 h. After the reaction, transfer the reaction system to a screw extruder, controlling the screw speed at 50 r / min and the die head temperature at 255℃. The material is filtered through a 100-mesh stainless steel melt filter and then extruded through a 3.0mm aperture outlet to form strips. The strips are cooled in circulating deionized water at 25℃ and drawn at a speed of 12m / min. Then, they are pelletized at 800r / min to obtain modified PA6 particles with a length of 3.5mm. The modified PA6 particles and deionized water are mixed at a mass ratio of 1:20 and extracted at 98℃ and 100r / min for 10 hours, with the same amount of deionized water replaced every 4 hours during the extraction process. After extraction, the mixture is filtered through a 1.0mm aperture stainless steel filter. The filter cake is washed twice with deionized water at 70℃ and then dried at 110℃ and a vacuum of -0.095MPa until the moisture content is ≤0.06%, resulting in modified PA6 chips.
[0091] S3. Modified PA6 chips are added to a melt spinning machine for melt spinning; the screw speed is controlled at 70 r / min, the extruder feed section temperature is 250℃, the compression section temperature is 255℃, the melting section temperature is 260℃, and the spinning box temperature is 262℃; after filtration through a sintered stainless steel filter with a pore size of 30μm, the fibers are delivered by a metering pump to a spinneret with 24 spinneret holes and a spinneret hole diameter of 0.20mm, and extruded through the spinneret holes to form nascent fibers; the temperature is 24℃. The nascent fibers were cooled by a side-blowing airflow with a relative humidity of 70% and a wind speed of 0.5 m / s, and then wound at a speed of 1100 m / min. Subsequently, hot drawing was performed, with the temperature of the first drawing roller controlled at 90℃ and the temperature of the second drawing roller at 130℃, resulting in a total draw ratio of 3.5. After drawing, the fibers were heat-set at 165℃ for 20 seconds to obtain modified PA6 fibers. The modified PA6 fibers were then plain-weave at a loom speed of 380 r / min, yielding a basis weight of 120 g / m². 2The nylon fabric was added to the washing solution (a deionized water solution containing 1.5 g / L AEO-9) at a mass ratio of 1:20. The nylon fabric was washed for 20 minutes at a temperature of 60℃ and a rotation speed of 120 r / min. After washing, the nylon fabric was removed and rinsed three times with deionized water at a temperature of 30℃ for 5 minutes each time. After rinsing, the fabric was dried at a temperature of 85℃ for 30 minutes to obtain the nylon fabric.
[0092] S4. Control the mass ratio of nylon fabric to anti-wrinkle finishing solution to 1:20. Immerse the nylon fabric in the anti-wrinkle finishing solution and perform a two-dip and two-ply treatment at 30℃, with each immersion lasting 3 minutes. After each immersion, the fabric is rolled by a rolling mill with a roll pressure of 0.30 MPa and a roll speed of 2 m / min, and the roll residue is controlled at 80%. After the treatment, the nylon fabric is pre-dried at 90℃ for 3 minutes, and then heated to 155℃ for 2 minutes. After baking, it is cooled to room temperature to obtain the anti-wrinkle nylon fabric.
[0093] To verify the comprehensive performance of the wrinkle-resistant nylon fabrics prepared in Examples 1-3 of this invention, the inventors set up Comparative Examples 1-5, as follows:
[0094] Comparative Example 1
[0095] The difference between this comparative example and Example 1 is that, in the original step S2, no anti-wrinkle modifier is added, and ε-caprolactam of the same mass as the anti-wrinkle modifier is used to make up the difference. The remaining steps and raw materials are the same as in Example 1.
[0096] Comparative Example 2
[0097] The difference between this comparative example and Example 1 is that step S4 is omitted, that is, the nylon fabric is not subjected to anti-wrinkle finishing liquid for padding, pre-drying and baking treatment, while the remaining steps and raw materials are the same as in Example 1.
[0098] Comparative Example 3
[0099] The difference between this comparative example and Example 1 is that in the original step S1, isophorone diisocyanate was replaced with hexamethylene diisocyanate by mass, while the remaining steps and raw materials were the same as in Example 1.
[0100] Comparative Example 4
[0101] The difference between this comparative example and Example 1 is that in the original step A3, functionalized polydimethylsiloxane is replaced by vinyl-terminated polydimethylsiloxane by mass, while the remaining steps and raw materials are the same as in Example 1.
[0102] Comparative Example 5
[0103] The difference between this comparative example and Example 1 is that in the original step A3, the functionalized polydimethylsiloxane was replaced by a modified silane intermediate, while the remaining steps and raw materials were the same as in Example 1.
[0104] Performance testing
[0105] The comprehensive performance of the wrinkle-resistant nylon fabrics prepared in Examples 1-3 and Comparative Examples 1-5 of this invention was tested respectively.
[0106] ① Wrinkle recovery performance
[0107] The test was conducted in accordance with the standard GB / T 3819-1997 "Textiles - Determination of Crease Recovery Property by Crease Recovery Angle Method", using a crease recovery angle tester.
[0108] Cut 40mm × 15mm samples along both the warp and weft directions of the fabric, taking 10 samples in each direction. Avoid sampling along fabric edges, creases, and obvious defects. Fold the sample lengthwise so that the two ends overlap, apply a 10N load to the folded area and hold for 5 minutes. Immediately after removing the load, place the sample on a crease recovery angle tester and allow it to recover freely. After 5 minutes, read the crease recovery angle, accurate to 1°.
[0109] Calculate the average values of the warp crease recovery angle and the weft crease recovery angle respectively, and calculate the total crease recovery angle according to the formula: Total crease recovery angle = average warp crease recovery angle + average weft crease recovery angle.
[0110] ② Water-resistant and wrinkle-resistant properties
[0111] The test was conducted in accordance with the standard GB / T 8629-2017 "Textiles - Testing - Household Washing and Drying Procedures", using a Type A standard washing machine and the 4N washing program. Standard detergent 2 was added during washing at a rate of 20±1g, and polyester fiber linens were used to adjust the total washing load to 2.0±0.1kg.
[0112] Each wash and hang-to-dry cycle is counted as one washing cycle, and 20 washing cycles are performed consecutively. After washing, the sample is conditioned for 24 hours under standard atmospheric conditions of 20±2℃ and 65±4% relative humidity. The total crease recovery angle after 20 washes is then measured according to the wrinkle recovery performance test method described above, and the wrinkle resistance retention rate is calculated using the formula: Wrinkle resistance retention rate = Total crease recovery angle after 20 washes / Total crease recovery angle before washing × 100%.
[0113] ③ Fracture strength
[0114] The test was conducted in accordance with the standard GB / T 3923.1-2013 "Textiles - Tensile Properties of Fabrics - Part 1: Determination of Breaking Strength and Elongation at Break (Strip Method)". The samples were conditioned for 24 hours at a temperature of 20±2℃ and a relative humidity of 65±4%.
[0115] Five strip samples were cut along both the warp and weft directions of the fabric, with an effective sample width of 50 mm. The sampling position was at least 150 mm from the fabric edge, avoiding obvious defects. The test was conducted using a constant speed elongation fabric strength tester with a clamping distance of 200 mm and a tensile speed of 100 mm / min. The sample should be held flat between the upper and lower clamps to avoid significant pre-tension and slippage.
[0116] Start the instrument and continuously stretch the sample until it breaks. Record the maximum tensile force and calculate the arithmetic mean of the longitudinal and latitudinal breaking strengths, in N.
[0117] ④ Bending performance
[0118] The test was conducted in accordance with the standard GB / T 18318.1-2009 "Determination of bending properties of textiles - Part 1: Inclined plane method".
[0119] Cut six 25mm × 250mm samples along both the warp and weft directions of the fabric, with each sample taken at least 100mm from the selvage. Place the samples flat on the horizontal platform of the bending length meter, aligning the long side of the sample with the length of the platform. Hold the sample down with a steel ruler and move the ruler and sample outwards from the platform at a uniform speed. When the suspended end of the sample bends under its own weight and contacts an inclined plane with an angle of 41.5°, record the extension length L of the sample.
[0120] Calculate the bending length C according to the formula: C=L / 2;
[0121] The bending stiffness G is calculated using the formula: G = m × C 3 ×10 -3 In the formula, m is the mass per unit area of the fabric, expressed in g / m².
[0122] Calculate the average bending length and average bending stiffness of the samples in the warp and weft directions respectively.
[0123] The test results are shown in Table 1.
[0124] Table 1: Performance Test Table of Wrinkle-Resistant Nylon Fabrics Prepared in Examples 1-3 and Comparative Examples 1-5
[0125]
[0126] As shown in Table 1, the anti-wrinkle nylon fabrics prepared in Examples 1-3 of this invention have good wrinkle recovery performance, water washing resistance and tensile strength, while maintaining low bending stiffness. Their overall performance is better than that of Comparative Examples 1-5.
[0127] As can be seen from the data shown in Example 1 and Comparative Example 1, no anti-wrinkle modifier was added in Comparative Example 1. The PA6 system lacks the modified structure used to adjust the molecular chain arrangement and deformation recovery, which weakens the fiber's recovery ability after being subjected to folding force, resulting in a decrease in the nylon fabric's wrinkle recovery performance, water-washable anti-wrinkle performance and breaking strength.
[0128] As can be seen from the data shown in Example 1 and Comparative Example 2, Comparative Example 2 did not use anti-wrinkle finishing liquid to impregnate, pre-dry, and bake the nylon fabric, resulting in the absence of a finishing layer with flexible recovery and interface fixation on the surface of the nylon fibers. This resulted in insufficient anti-wrinkle support on the fabric surface, leading to a decrease in both the wrinkle recovery performance and the wash-resistant wrinkle resistance of the nylon fabric.
[0129] As shown by the data from Example 1 and Comparative Example 3, in Comparative Example 3, the use of hexamethylene diisocyanate instead of isophorone diisocyanate resulted in the absence of the alicyclic structure and steric hindrance structure of isophorone diisocyanate in the anti-wrinkle modifier, which weakened its regulating effect on the regular arrangement of PA6 molecular chains, leading to a decrease in the wrinkle recovery performance, water-washable wrinkle resistance and tensile strength of nylon fabric.
[0130] Data from Example 1 and Comparative Example 4 show that: Comparative Example 4 uses vinyl-terminated polydimethylsiloxane instead of functionalized polydimethylsiloxane. Although the flexible siloxane segments can still reduce the bending resistance of the fabric, the bonding stability between the finishing components and the nylon fibers decreases due to the lack of silane fixing structure. After washing, the finishing layer is easy to migrate and fall off, resulting in a decrease in the wash resistance and wrinkle resistance of the nylon fabric.
[0131] As can be seen from the data shown in Example 1 and Comparative Example 5, Comparative Example 5 uses a modified silane intermediate for finishing. Due to the lack of flexible polydimethylsiloxane segments, the flexibility of the finished layer is reduced, the bending freedom of the fibers and yarns is restricted, the bending stiffness of the nylon fabric increases, and the elastic recovery ability after wrinkling decreases.
[0132] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but such modifications are protected by patent law as long as they are within the scope of the claims of the present invention.
Claims
1. A method for preparing an anti-wrinkle nylon fabric, characterized in that, The preparation steps include the following: S1. Under nitrogen protection, 6-aminohexanoic acid is added to anhydrous N,N-dimethylformamide, stirred evenly, cooled to 10-15℃, isophorone diisocyanate is added, and the mixture is stirred to react. After the reaction is completed, the mixture is precipitated, filtered, washed, dried, pulverized and sieved to obtain the anti-wrinkle modifier. S2. Mix ε-caprolactam, anti-wrinkle modifier, benzoic acid and deionized water, stir and react. After the reaction is completed, extrude, cool, granulate, and then dry after hot water extraction to obtain modified PA6 chips. S3. Modified PA6 chips are melt-spun to obtain modified PA6 fibers; Modified PA6 fibers are woven, washed, and dried to obtain nylon fabric; S4. Immerse the nylon fabric in the anti-wrinkle finishing solution and perform padding treatment. After the treatment is completed, perform pre-drying and baking treatment in sequence. After the treatment is completed, cool to obtain anti-wrinkle nylon fabric.
2. The method for preparing the wrinkle-resistant nylon fabric according to claim 1, characterized in that, In step S1, the mass ratio of 6-aminohexanoic acid, isophorone diisocyanate, and anhydrous N,N-dimethylformamide is 1:0.8-0.9:8-10.
3. The method for preparing the wrinkle-resistant nylon fabric according to claim 1, characterized in that, In step S2, the mass ratio of ε-caprolactam, anti-wrinkle modifier, benzoic acid and deionized water is 100:1.0-1.2:0.08-0.12:3-4.
4. The method for preparing the wrinkle-resistant nylon fabric according to claim 1, characterized in that, In step S4, the mass ratio of nylon fabric to anti-wrinkle finishing liquid is 1:18-20.
5. The method for preparing the wrinkle-resistant nylon fabric according to claim 4, characterized in that, The preparation method of the anti-wrinkle finishing liquid includes the following steps: A1. Under nitrogen protection, L-cysteine was added to anhydrous N,N-dimethylformamide, stirred until homogeneous, cooled to 10-15℃, and 3-isocyanate-propyltriethoxysilane was added. The mixture was heated and stirred to react. After the reaction was completed, the modified silane intermediate was obtained through post-treatment. A2. Under nitrogen protection, vinyl-terminated polydimethylsiloxane was added to a mixed solvent, along with a modified silane intermediate and azobisisobutyronitrile. The mixture was stirred and reacted. After the reaction was completed, the mixture was cooled and concentrated under reduced pressure to obtain functionalized polydimethylsiloxane. A3. Mix the emulsifier and deionized water, add the functionalized polydimethylsiloxane while stirring, and after the addition is complete, shear emulsify, then add the wetting agent and penetrant, stir evenly, adjust the pH of the system to 5.0-5.5, continue to stir evenly, and let it stand to mature to obtain the anti-wrinkle finishing solution.
6. The method for preparing the wrinkle-resistant nylon fabric according to claim 5, characterized in that, In step A1, the mass ratio of L-cysteine, 3-isocyanate-propyltriethoxysilane, and anhydrous N,N-dimethylformamide is 1:1.9-2.1:8-10.
7. The method for preparing the wrinkle-resistant nylon fabric according to claim 5, characterized in that, In step A2, the mass ratio of vinyl-terminated polydimethylsiloxane, modified silane intermediate, azobisisobutyronitrile, and mixed solvent is 1:0.50-0.60:0.008-0.012:4-5.
8. The method for preparing the wrinkle-resistant nylon fabric according to claim 5, characterized in that, In step A3, the mass ratio of emulsifier, functionalized polydimethylsiloxane, wetting agent, penetrant and deionized water is 1.6-1.8:9-10:0.15-0.20:0.15-0.20:89-91.
9. The method for preparing the wrinkle-resistant nylon fabric according to claim 1, characterized in that, The immersion and padding process in step S4 refers to immersing the nylon fabric in an anti-wrinkle finishing solution and performing a double immersion and padding process at a temperature of 25-30℃, with each immersion lasting 3-5 minutes. After each immersion, the fabric is rolled by a rolling mill with a roll pressure of 0.20-0.30 MPa and a roll running speed of 1-2 m / min, and the roll residue is controlled to be 70-80%.
10. A wrinkle-resistant nylon fabric prepared by the method of any one of claims 1-9.