A silicone artificial leather for marine furniture and its preparation method
By adopting a multi-layer structure design that combines aramid fiber fabric with modified silicone rubber coating, the shortcomings of silicone artificial leather for marine furniture in terms of flame retardancy, low-temperature toughness, seawater corrosion resistance and weather resistance are solved, and high-performance application in extreme environments is achieved.
Patent Information
- Application Number
- CN202611255235.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-18
- Publication Date
- 2026-11-17
AI Technical Summary
Existing silicone-based artificial leather for marine furniture is inadequate in terms of flame retardancy, low-temperature toughness, seawater corrosion resistance, and weather resistance, making it difficult to meet the comprehensive requirements of polar navigation and marine environments.
Using aramid fiber fabric as the base layer, it is combined with modified silicone rubber coating to form a multi-layer structure. Through the intrinsic flame retardancy of aramid fiber and the cross-linking design of modified silicone rubber, the interfacial adhesion stability and weather resistance are improved. Adding functional additives gives the product multiple surface functions.
It achieves high flame retardancy and high interfacial adhesion stability at extreme low temperatures, as well as resistance to seawater corrosion and weathering, meeting the safety and durability requirements of marine furniture decoration. It passes the IMO FTP Code Part 8 flame retardancy test, and its smoke density is below the limit.
Smart Images

Figure CN123108950A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of silicone artificial leather technology, and in particular to a silicone artificial leather for marine furniture and its preparation method. Background Technology
[0002] Silicone-based artificial leather for marine furniture is widely used in the surface decoration of upholstered furniture in ship and yacht cabins. Due to its long-term exposure to the marine environment, this type of material must simultaneously meet multiple requirements, including resistance to seawater corrosion, resistance to high and low temperatures (especially low-temperature toughness), resistance to ultraviolet aging, and flame retardant properties that meet marine fire protection standards.
[0003] Currently, there are technical solutions for preparing synthetic leather using organosilicon materials in the field of marine furniture decoration. For example, Chinese invention patent CN113737539A discloses an "organosilicon synthetic leather for marine and yacht furniture decoration and its preparation method," which improves the folding resistance of synthetic leather at -30℃ to a certain extent by adding a composite low-temperature toughening agent composed of epoxy resin, polyarylether ketone, nano-boehmite powder, and ultra-high molecular weight polyethylene to the organosilicon slurry. However, the above-mentioned existing technologies still have the following shortcomings: First, the flame retardant performance is insufficient. The added low-temperature toughening agent components (epoxy resin and ultra-high molecular weight polyethylene) are both flammable materials, which significantly reduces the overall flame retardant performance of the synthetic leather, making it difficult to pass the International Maritime Organization (IMO) FTP Code Part 8 small flame ignition resistance test and Part 2 smoke density and toxicity test requirements. Second, there is still room for improvement in low-temperature toughness. The ambient temperature of polar ships can be as low as -40℃ or even -50℃, and the existing technology cannot meet the requirements of more extreme low-temperature conditions. Third, the resistance to seawater corrosion and interfacial adhesion stability are insufficient. After 50 days of simulated seawater immersion, the peel strength decreased by approximately 9.1%. The silane coupling agent layer on the glass fiber surface is prone to hydrolysis and failure, and the hydrophilic components in the toughening agent easily adsorb water molecules, leading to interfacial deterioration. Fourth, the weather resistance needs to be improved. The added organic components are prone to photo-oxidative degradation under long-term ultraviolet irradiation, affecting the product's service life.
[0004] In view of the problems existing in the above-mentioned related technologies, there is an urgent need in this field to develop an organosilicon artificial leather for marine furniture that has excellent flame retardant properties, low temperature toughness, seawater corrosion resistance and weather resistance, so as to meet the comprehensive requirements of safety and durability for marine and yacht furniture decoration. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an organic silicone artificial leather for marine furniture and its preparation method. By using aramid fiber fabric as the base layer and compounding it with a specific modified silicone rubber coating, a multi-layer structure is formed. This significantly improves the flame retardant properties and interfacial adhesion stability of the product while ensuring excellent low-temperature toughness and seawater corrosion resistance, thus meeting the comprehensive requirements of safety and durability for marine and yacht furniture decoration.
[0006] In the first aspect, this application provides an organosilicon artificial leather for marine furniture, which adopts the following technical solution: A type of silicone artificial leather for marine furniture has a multi-layer composite structure, including: a top adhesive layer, a base adhesive layer, and a base layer; The adhesive layer is made of modified silicone rubber material and serves as the surface layer that comes into direct contact with the usage environment. The base layer, disposed between the base layer and the top layer, is made of silicone rubber adhesive material and is used to achieve the bonding and composite bonding between the base layer and the top layer; The base layer is an aramid fiber fabric, which serves as the skeleton support layer of the overall structure; the aramid fiber fabric is either para-aramid fiber fabric or meta-aramid fiber fabric, and its unit area mass is 100-400g / m².
[0007] Through the above technical solutions, aramid fibers possess intrinsic flame retardancy, high strength and modulus, and excellent chemical corrosion resistance. They do not melt or drip when exposed to fire, fundamentally ensuring fire safety in confined spaces on ships. Simultaneously, they exhibit good chemical affinity with the base adhesive layer, forming a stable chemical bond interface when combined with surface pretreatment and tackifiers, significantly improving peel strength and resistance to seawater hydrolysis. The top adhesive layer imparts surface properties such as abrasion resistance, stain resistance, and UV aging resistance, giving the product excellent flame retardant safety, superior interfacial adhesion stability, good low-temperature toughness, and long-term weather resistance, comprehensively meeting the combined safety and durability requirements of ship and yacht furniture and decoration.
[0008] Preferably, the adhesive layer is made from the following raw materials in parts by weight: 100 parts of α,ω-divinyl polydimethylsiloxane, 2-15 parts of hydrogen-containing silicone oil crosslinking agent, 0.01-0.5 parts of platinum catalyst, 0.01-0.1 parts of alkynyl alcohol inhibitor, 10-30 parts of silica reinforcing filler, 5-30 parts of vinyl MQ silicone resin, and 1-10 parts of functional additives.
[0009] Preferably, the α,ω-divinyl polydimethylsiloxane has a viscosity of 500-12000 mPa·s and a vinyl content of 0.1-2.0 mol%; the hydrogen-containing silicone oil has a hydrogen content of 0.2-1.6 wt%.
[0010] The above technical solution utilizes α,ω-divinyl polydimethylsiloxane as the base polymer and hydrogen-containing silicone oil as the crosslinking agent. Under the action of a platinum catalyst, a three-dimensional network crosslinked structure is formed through hydrosilylation. The introduction of vinyl MQ silicone resin significantly enhances the mechanical strength and hardness adjustment capability of silicone rubber, while also imparting excellent low-temperature toughness to the coating. Silica reinforcing filler effectively improves tensile strength, tear strength, and abrasion resistance by forming a three-dimensional filler network. Alkyne alcohol inhibitors precisely control the working time and curing speed of the compound, ensuring the stability of the coating process. Functional additives flexibly impart specific surface functions to the coating, such as hydrophobicity, oleophobicity, antibacterial and antifungal properties, and UV aging resistance. This formulation system does not contain any added flammable organic toughening agents. Through intrinsic structural design, it achieves a balance between low-temperature toughness and flame retardancy, giving the topcoat layer excellent mechanical properties, weather resistance, surface functionality, and processability.
[0011] Preferably, the functional additive is two or more of the following: hydrophobic and oleophobic modifiers, UV inhibitors, and antibacterial and antifungal agents.
[0012] Preferably, the hydrophobic and oleophobic modifier is any one of fluorinated silicone oil and perfluoroalkyl silane; the UV stabilizer is any one of nano-titanium dioxide and hindered amine light stabilizer; and the antibacterial and antifungal agent is any one of nano-silver, organosilicon quaternary ammonium salt and zinc pyridinethione.
[0013] By introducing two or more functional additives into the adhesive layer using the above technical solutions, silicone-based artificial leather can be endowed with multiple surface functions. Hydrophobic and oleophobic modifiers reduce the surface energy of the coating, making it difficult for water- and oil-based stains to adhere, achieving excellent stain resistance and easy cleaning performance. Anti-UV agents effectively absorb or shield ultraviolet rays, inhibiting the photo-oxidative degradation of silicone rubber and significantly improving the coating's weather resistance and service life. Antibacterial and antifungal agents, through contact sterilization or the release of active ions, effectively inhibit the growth and reproduction of bacteria and mold on the material surface, meeting the stringent hygiene and safety requirements of interior materials in the confined spaces of ships. The synergistic effect of these functional additives gives the product multiple functions, including stain resistance, weather resistance, and antibacterial properties, fully adapting to the personalized needs of ships and yachts in different application scenarios.
[0014] Preferably, the base layer is made from the following raw materials in parts by weight: 100 parts of α,ω-divinyl polydimethylsiloxane, 2-10 parts of hydrogen-containing silicone oil crosslinking agent, 0.01-0.3 parts of platinum catalyst, 0.01-0.08 parts of alkynyl alcohol inhibitor, 5-20 parts of silica reinforcing filler, and 3-8 parts of tackifier.
[0015] Preferably, the tackifier is two or more of the following: silane coupling agents containing silane-hydrogen bonds, silane coupling agents containing epoxy groups, silane coupling agents containing acryloyloxy groups, and silane coupling agents containing vinyl groups.
[0016] Preferably, the tackifier is a combination of vinyltrimethoxysilane and γ-glycidyl etheroxypropyltrimethoxysilane in a mass ratio of (1-2):1.
[0017] The above technical solution employs an addition-type liquid silicone rubber of the same system as the topcoat layer, ensuring excellent compatibility and co-crosslinking ability between the two layers. The tackifier is a blend of vinyltrimethoxysilane and γ-glycidyl etheroxypropyltrimethoxysilane. The former anchors to the silicone rubber network through a vinyl group participating in a hydrosilylation reaction, while the latter forms chemical bonds with the surface-active functional groups of the aramid fibers through epoxy groups. Together, they construct a stable "molecular bridge." This design achieves chemical co-crosslinking between the aramid fibers and the silicone rubber coating at the molecular level, significantly improving interfacial peel strength and seawater hydrolysis resistance.
[0018] Preferably, the aramid fiber fabric is a para-aramid fiber fabric.
[0019] Secondly, this application provides a method for preparing silicone artificial leather for marine furniture, comprising the following steps: S1. Surface pretreatment of aramid fiber fabric to improve its interfacial adhesion with silicone rubber coating; S2. Rubber compound preparation: Prepare the top layer rubber compound and the base layer rubber compound according to the formula; S3. Coating and Lamination: The top adhesive layer is coated onto release paper and initially cured at 100-180℃ to form the top adhesive layer; the bottom adhesive layer is coated onto the cured top adhesive layer; the pretreated aramid fiber base layer is bonded to the top adhesive layer coated with the bottom adhesive layer and pressure is applied; a second curing is performed at 100-180℃ to fully crosslink the bottom adhesive layer and bond the base layer, bottom adhesive layer and top adhesive layer together; the release paper is then peeled off to obtain the semi-finished silicone artificial leather. S4. The semi-finished silicone artificial leather is subjected to embossing and sanding surface finishing treatments to obtain the final product; The surface pretreatment method in step S1 is any one of plasma treatment, silane coupling agent impregnation treatment, or dopamine biomimetic modification combined with hyperbranched polysiloxane in-situ growth treatment.
[0020] The above-described preparation method employs a four-step process: pretreatment, adhesive preparation, coating and lamination, and post-treatment. This process is simple to operate, highly controllable, and suitable for continuous industrial production. Step S1 involves surface pretreatment of the aramid fiber fabric, significantly improving the interfacial wettability and chemical bonding between the aramid fiber and the silicone rubber coating, laying the foundation for subsequent high-strength interfacial adhesion. Step S3 utilizes a release paper transfer coating process, first curing the top adhesive layer and then coating the base adhesive layer before hot-pressing it with the substrate. This allows for precise control of the thickness of each layer and the bonding pressure, ensuring uniform and strong interlayer adhesion. Step S4 involves surface finishing treatments such as embossing and sanding to meet the personalized needs of different application scenarios.
[0021] Preferably, in step S2, the specific steps for preparing the surface adhesive layer include: mixing α,ω-divinyl polydimethylsiloxane, silica reinforcing filler, and vinyl MQ silicone resin components evenly, vacuum dehydrating at 100-150°C for 2-4 hours, cooling to room temperature, and then adding hydrogen-containing silicone oil crosslinking agent, platinum catalyst, and functional additives and stirring evenly.
[0022] Preferably, in step S2, the specific steps for preparing the base layer adhesive include: mixing α,ω-divinyl polydimethylsiloxane, silica reinforcing filler, vinyl MQ silicone resin and other components evenly, vacuum dehydrating at 100-150℃ for 2-4 hours, cooling to room temperature, adding hydrogen-containing silicone oil crosslinking agent, platinum catalyst and tackifier and stirring evenly.
[0023] Preferably, in step S3, the coating thickness of the top adhesive layer is 0.05-0.30 mm, and the initial curing time is 1-5 minutes; the coating thickness of the bottom adhesive layer is 0.05-0.20 mm; the pressure applied during bonding is 0.1-0.5 MPa, and the secondary curing time is 5-15 minutes.
[0024] By optimizing the above process parameters, the thickness of the topcoat layer is controlled at 0.05-0.30mm, ensuring surface abrasion resistance and coverage while avoiding material waste and reduced flexibility due to excessive coating thickness. The thickness of the basecoat layer is controlled at 0.05-0.20mm, forming a complete adhesive layer without increasing interfacial stress due to excessive thickness. A bonding pressure of 0.1-0.5MPa ensures that the basecoat fully penetrates into the fiber gaps to form physical anchoring, and a secondary curing time of 5-15 minutes ensures full cross-linking of the basecoat. The synergistic effect of these parameters results in uniform and firm interlayer bonding, and stable and reliable product mechanical properties and appearance quality.
[0025] Preferably, in step S4, the semi-finished silicone artificial leather can also be coated with a functional coating on the surface of the adhesive layer, followed by embossing and sanding surface finishing treatment.
[0026] In summary, this application has the following beneficial effects: 1. This application fundamentally solves the technical contradiction of being unable to simultaneously achieve flame retardancy and low-temperature toughness by preparing a multi-layer composite structure of "aramid fiber base layer + intrinsic toughened silicone rubber coating" and replacing traditional glass fiber cloth with aramid fiber fabric. Aramid fiber is intrinsically flame retardant, does not melt or drip when exposed to fire, and passes the IMO FTP Code Part 8 flame retardancy test; at the same time, the intrinsic toughening formula does not require the addition of flammable organic toughening agents, and can still withstand more than 80,000 folds at extreme low temperatures of -50℃, meeting the requirements of polar navigation.
[0027] 2. This application utilizes the synergistic effect of fiber surface pretreatment and compounded tackifier in the base layer to construct a chemical co-crosslinking interface between aramid fiber and silicone rubber matrix. The initial peel strength reaches more than 55 N / 25 mm, and the peel strength retention rate is not less than 87% after immersion in seawater for 90 days, which completely solves the problem of interface hydrolysis failure in marine environment of traditional solutions. Attached Figure Description
[0028] Figure 1 This is a cross-sectional view of the multilayer composite structure of the silicone artificial leather for marine furniture prepared in Examples 1-9.
[0029] Figure 2 The image shows a cross-sectional scanning electron microscope image of the silicone artificial leather for marine furniture prepared in Example 1, magnified 10 times. Detailed Implementation
[0030] The technical solutions of this application are further illustrated by specific embodiments below. These specific embodiments do not represent a limitation on the scope of protection of this application. Any non-essential modifications and adjustments made by others based on the concept of this application still fall within the scope of protection of this application.
[0031] Unless otherwise specified, the experimental methods shown in the following examples are conventional methods. All reagents and materials shown are commercially available products.
[0032] α,ω-Divinyl polydimethylsiloxane: Zhejiang Xin'an Chemical Group Co., Ltd., Model: XHG-206-500 (viscosity 500 mPa·s, vinyl content 0.383-0.456 mol%), Model: XHG-206-5000 (viscosity 5000 mPa·s, vinyl content 0.164-0.201 mol%), Model: XHG-206-10000 (viscosity 10000 mPa·s, vinyl content 0.109-0.182 mol%); Hydrogen-containing silicone oil: Zhejiang Xin'an Chemical Group Co., Ltd., Model: XHG-202-503 (hydrogen content 0.27-0.33 wt%), Model: XHG-202-1608 (hydrogen content 0.77-0.8 wt%), Model: XHG-202-2410 (hydrogen content 0.92-1.12 wt%); Castells platinum catalyst: DowSIL, model: Syl-Off® 4000; Silica reinforcing filler: Yichang Huifu Silicon Materials Co., Ltd., Model: HL-200, Specific surface area 200 m² / g; Vinyl MQ silicone resin: Guangzhou Tianjiang High-Tech Materials Co., Ltd., TJ-VIMQ-02, vinyl content 0.5-1.5wt%; Nano TiO2: Beijing Zhongke Keyou Technology Co., Ltd., Product No.: ZKKY-Tio2-01-020, Average particle size 20nm; Organosilicon quaternary ammonium salt antibacterial agent: Shanghai Hetai Chemical Co., Ltd., HT-800; Fluorinated silicone oil: Jiangshan City Shengnuoyi New Material Technology Co., Ltd., Model: SNY-280-1000.
[0033] The present application will be further described in detail below with reference to embodiments and comparative examples. Example
[0034] Example 1 A method for preparing silicone artificial leather for marine furniture is provided, comprising the following steps: S1. Plasma surface pretreatment is performed on aramid fiber fabric to improve its interfacial adhesion with silicone rubber coating; S2. Rubber compound preparation: Prepare the top layer rubber compound and the base layer rubber compound according to the formula; S3. Coating and Lamination: The top adhesive layer is coated onto release paper and initially cured at 150°C for 3 minutes, with a coating thickness of 0.26 mm, forming the top adhesive layer; the bottom adhesive layer is coated onto the cured top adhesive layer, with a coating thickness of 0.2 mm; the pretreated aramid fiber base layer is bonded to the top adhesive layer coated with the bottom adhesive layer, and a pressure of 0.3 MPa is applied; a second curing at 150°C is performed for 10 minutes to fully crosslink the bottom adhesive layer and bond the base layer, bottom adhesive layer and top adhesive layer together; the release paper is then peeled off to obtain the semi-finished silicone artificial leather product; S4. Embossing and surface finishing treatment of the semi-finished silicone artificial leather to obtain the final product.
[0035] In step S1, the aramid fiber fabric is placed in a plasma treatment device and subjected to plasma treatment in an oxygen atmosphere. The treatment power is 150W and the treatment time is 120s.
[0036] In step S2, the specific steps for preparing the surface adhesive layer include: mixing α,ω-divinyl polydimethylsiloxane, silica reinforcing filler, and vinyl MQ silicone resin components evenly, vacuum dehydrating at 130°C for 3 hours, cooling to room temperature, and then adding hydrogen-containing silicone oil crosslinking agent, platinum catalyst, and functional additives and stirring evenly.
[0037] In step S2, the specific steps for preparing the base layer adhesive include: mixing α,ω-divinyl polydimethylsiloxane, silica reinforcing filler, vinyl MQ silicone resin and other components evenly, vacuum dehydrating at 130°C for 3 hours, cooling to room temperature, adding hydrogen-containing silicone oil crosslinking agent, platinum catalyst and tackifier and stirring evenly.
[0038] The α,ω-divinyl polydimethylsiloxane is selected from Xin'an Chemical's XHG-206-5000. The hydrogen-containing silicone oil is selected from Xin'an Chemical's XHG-202-1608.
[0039] The composition and dosage of the silicone artificial leather for marine furniture are shown in Table 1.
[0040]
[0041] Example 2-3 The difference from Example 1 is that the composition and dosage of the silicone artificial leather for marine furniture are shown in Table 1: Example 4 The difference from Example 1 is that the composition and dosage of the silicone artificial leather for marine furniture are shown in Table 1. The α,ω-divinyl polydimethylsiloxane is selected from XHG-206-500 of Xin'an Chemical; the hydrogen-containing silicone oil is selected from XHG-202-503 of Xin'an Chemical.
[0042] Example 5 The difference from Example 1 is that the composition and dosage of the silicone artificial leather for marine furniture are shown in Table 1. The α,ω-divinyl polydimethylsiloxane is selected from Xin'an Chemical's XHG-206-10000; the hydrogen-containing silicone oil is selected from Xin'an Chemical's XHG-202-2410.
[0043] Example 6 The difference from Example 1 is that in step S1, the aramid fiber fabric undergoes a surface pretreatment by impregnation with a silane coupling agent; the aramid fiber fabric is impregnated in a 3.5 wt% KH-550 silane coupling agent solution for 7 hours. After treatment, the aramid fabric is removed and dried at 100°C, allowing the silane coupling agent to undergo a hydrolysis-condensation reaction on the fiber surface, forming an organic-inorganic hybrid interface layer.
[0044] Example 7 The difference from Example 1 is that in step S1, the aramid fiber fabric undergoes dopamine biomimetic modification combined with hyperbranched polysiloxane in-situ growth surface pretreatment. The specific steps are as follows: (1) Deposition of polydopamine biomimetic coating: Aramid fiber fabric was immersed in a tris(hydroxymethyl)aminomethane-hydrochloric acid buffer solution with a concentration of 2 g / L dopamine hydrochloride and pH=8.5. The mass ratio of fabric to treatment solution was 1:40. The reaction was carried out at 25℃ and 80 rpm for 24 hours. After the reaction was completed, the fabric was taken out and ultrasonically cleaned three times with deionized water to remove the weakly adsorbed polydopamine particles on the surface. Each cleaning lasted 5 minutes. Then, the fabric was dried under vacuum at 50℃ for 3 hours to obtain polydopamine modified aramid fabric.
[0045] (2) Grafting of aminosilane coupling agent: Polydopamine-modified aramid fabric was immersed in a 3wt% 90% ethanol aqueous solution of γ-aminopropyltriethoxysilane and the pH value was adjusted to 5.0 with acetic acid. The mass ratio of fabric to treatment solution was 1:30. The reaction was allowed to stand at 45°C for 4 hours. After the reaction was completed, the fabric was taken out and rinsed with anhydrous ethanol 3 times. Then it was cured at 90°C for 1.5 hours to allow the grafted silane molecules to undergo dehydration condensation and form a stable siloxane network layer.
[0046] (3) In-situ growth of hyperbranched polysiloxane; Under nitrogen protection, aramid fabric grafted with aminosilane coupling agent was immersed in a reaction solution containing 150 mmol / L vinyltrimethoxysilane. The mass ratio of fabric to reaction solution was 1:40. Under nitrogen protection and slow stirring, the temperature was raised to 80°C and the reaction was kept at a constant temperature for 12 hours. After the reaction was completed, the fabric was cooled to room temperature, removed, and ultrasonically cleaned twice with anhydrous toluene for 8 minutes each time, and then cleaned once with anhydrous ethanol to remove unreacted monomers and free polymers. Finally, the fabric was dried under vacuum at 70°C for 3 hours to obtain hyperbranched polysiloxane modified aramid fabric.
[0047] Preparation of the reaction solution of vinyltrimethoxysilane: In a nitrogen-protected glove box, add 1000 mL of anhydrous toluene; add 22.2 g of vinyltrimethoxysilane and 0.22 g of dibutyltin dilaurate in sequence and stir until homogeneous to obtain a reaction solution with a vinyltrimethoxysilane concentration of 150 mmol / L, and seal for later use.
[0048] Example 8 The difference from Example 1 is as follows: Step S3 Coating and Lamination: The top adhesive layer is coated onto the release paper and initially cured at 100°C for 5 minutes, with a coating thickness of 0.05 mm, forming the top adhesive layer; the bottom adhesive layer is coated onto the cured top adhesive layer, with a coating thickness of 0.05 mm; the pretreated aramid fiber base layer is bonded to the top adhesive layer coated with the bottom adhesive layer, and a pressure of 0.1 MPa is applied; a second curing at 100°C is performed for 15 minutes to fully crosslink the bottom adhesive layer and bond the base layer, bottom adhesive layer and top adhesive layer together; the release paper is then peeled off to obtain the semi-finished product of silicone artificial leather.
[0049] Example 9 The difference from Example 1 is as follows: Step S3 Coating and Lamination: The top adhesive layer is coated onto the release paper and initially cured at 180°C for 1 minute, with a coating thickness of 0.30 mm, forming the top adhesive layer; the bottom adhesive layer is coated onto the cured top adhesive layer, with a coating thickness of 0.20 mm; the pretreated aramid fiber base layer is bonded to the top adhesive layer coated with the bottom adhesive layer, and a pressure of 0.5 MPa is applied; a second curing at 180°C is performed for 5 minutes to fully crosslink the bottom adhesive layer and bond the base layer, bottom adhesive layer and top adhesive layer together; the release paper is then peeled off to obtain the semi-finished product of silicone artificial leather.
[0050] Example 10 The difference from Example 1 is that in step S4, a functional coating is applied to the surface of the adhesive layer. The hydrophobic and oleophobic coating is uniformly applied to the surface of the adhesive layer of the silicone artificial leather semi-finished product using a spraying method. The spray gun pressure is 0.3 MPa, the nozzle distance from the product surface is 20 cm, and the spraying is performed using a uniform scanning method. The coating amount is controlled at 10 g / m². 2 After coating, the product is placed in a drying tunnel or oven and heat-cured at 120°C for 6 minutes. After curing, the product surface has a water contact angle greater than 110 degrees and an edible oil contact angle greater than 70°, exhibiting excellent hydrophobic and oleophobic properties and easy cleaning. The hydrophobic and oleophobic coating solution is prepared by dissolving heptadecafluorodecyltrimethoxysilane in a hydrofluoroether solvent or an alcohol-water mixture, with a perfluoroalkylsilane mass percentage concentration of 13%. Comparative Example
[0051] Comparative Example 1 The difference from Example 1 is that high-strength glass fiber cloth is used instead of aramid fiber fabric as the base layer. The high-strength glass fiber cloth is a plain weave glass fiber cloth with an area mass of 200 g / m².
[0052] Comparative Example 2 The difference from Example 1 is that no tackifier is added to the base layer composition.
[0053] Comparative Example 3 The difference from Example 1 is that the base aramid fiber fabric does not undergo any surface pretreatment.
[0054] Comparative Example 4 The difference from Example 1 is that vinyl MQ silicone resin is not added to the adhesive layer.
[0055] Comparative Example 5 The difference from Example 1 is that 100g of epoxy resin (E-44 type) and 80g of ultra-high molecular weight polyethylene powder (molecular weight 1.5 million, average particle size 50μm) are added to the surface adhesive layer formulation as organic low-temperature toughening agents. The dosage of other components, preparation methods and post-treatment steps are the same as in Example 1. Performance testing
[0056] The following performance tests were conducted on the silicone artificial leather for marine furniture prepared in Examples 1-10 and Comparative Examples 1-5.
[0057]
[0058] The performance test results are shown in Tables 3 and 4.
[0059]
[0060]
[0061] As can be seen from the performance test results in Tables 3 and 4, Examples 1-10 showed excellent performance in various performance indicators. The specific analysis is as follows: (1) Low temperature toughness: The number of folding cycles at -30℃ was not less than 92,000 times, and at -50℃ it was not less than 80,000 times, indicating that the present invention successfully achieved the intrinsic low temperature toughening effect through the formulation optimization of vinyl MQ silicone resin and hydrogen-containing silicone oil. (2) Interfacial bonding strength and seawater corrosion resistance: The initial peel strength of Examples 1-10 was in the range of 55.2-68.2 N / 25 mm, and the peel strength retention rate after 90 days of seawater immersion was in the range of 87.1%-95.0%; the initial peel strength (62.1 N / 25 mm) and retention rate (93.1%) of Example 3 were both high, indicating that the higher crosslinking density is beneficial to enhancing the compactness and hydrolysis resistance of the interfacial layer. (3) UV aging resistance: After 500 hours of QUV accelerated aging, the yellowing index ΔE is in the range of 0.5-0.8, and the tensile strength retention rate is in the range of 90.6%-95.8%, demonstrating excellent weather resistance. Cross-sectional views of the multi-layer composite structure of the silicone artificial leather for marine furniture in Examples 1-9 are shown below. Figure 1 As shown.
[0062] Due to the high cost of flame retardant safety testing, Example 1 in the examples was selected for flame retardant safety testing. Its total calorific value was 12.5 MJ / kg, and it passed the FTP Part 8 flame retardant test. The smoke density Dm was 128, both lower than the IMO limit of 150. A higher crosslinking density means fewer flammable small molecules and a denser network structure, which helps reduce heat release and smoke generation during combustion. The scanning electron microscope image of the cross-section of the silicone artificial leather for marine furniture prepared in Example 1 is shown below. Figure 2 As shown, the total thickness of the top and bottom adhesive layers, measured at 10x magnification, is 0.46 mm. Since both the top and bottom adhesive layers are made of silicone rubber, no obvious interface boundary is observed in the electron microscope scan image. Figure 2 The thread-like structure shown below is the base fabric.
[0063] The only difference between Comparative Example 1 and Example 1 is the use of high-strength glass fiber cloth instead of para-aramid fiber fabric as the base layer. The initial peel strength of Comparative Example 1 was only 41.5 N / 25 mm, a decrease of 29.1% compared to Example 1; after 90 days of seawater immersion, the peel strength retention rate was 82.4%, lower than the 92.6% of Example 1. The results show that the interfacial bonding force between the glass fiber cloth and the silicone rubber coating is significantly weaker than that of the aramid fiber, and the interfacial hydrolysis is more severe under long-term seawater immersion conditions, proving that the aramid fiber base layer is significantly better than the glass fiber cloth in terms of interfacial adhesion stability.
[0064] The only difference between Comparative Example 2 and Example 1 is that no tackifier was added to the base layer. The initial peel strength of Comparative Example 2 was only 32.6 N / 25 mm, a decrease of 44.3% compared to Example 1; after 90 days of seawater immersion, the peel strength retention rate was 85.3%, lower than that of Example 1. The results indicate that the tackifier is a key component in constructing the chemical bridge between the aramid fiber and the silicone rubber base layer. The lack of a tackifier leads to a significant decrease in interfacial adhesion performance, failing to meet the peel strength requirements for marine furniture.
[0065] The only difference between Comparative Example 3 and Example 1 is that the aramid fiber fabric was not subjected to any surface pretreatment and was directly bonded to the base adhesive layer. The initial peel strength of Comparative Example 3 was only 28.5 N / 25 mm, a decrease of 51.3% compared to Example 1; after immersion in seawater for 90 days, the peel strength retention rate was only 74.7%. The results show that the number of surface-active functional groups of untreated aramid fibers is limited and unevenly distributed, making it impossible to form sufficient and effective chemical bonds and physical anchoring with the base adhesive layer; surface pretreatment is a necessary step to improve the surface activity and roughness of aramid fibers and achieve high interfacial adhesion strength.
[0066] The only difference between Comparative Example 4 and Example 1 is that vinyl MQ silicone resin was not added to the adhesive layer. Comparative Example 4 exhibited severely deteriorated low-temperature toughness: the flexural resistance at -30°C was only 52,000 cycles, a 50.5% decrease compared to Example 1; the flexural resistance at -50°C was only 28,000 cycles, a 68.2% decrease compared to Example 1. The results indicate that vinyl MQ silicone resin is the core component for achieving intrinsic low-temperature toughening. Its unique core-shell structure and nanoscale effect can form uniformly distributed hard segment micro-regions in the silicone rubber network, playing a role in stress dispersion and energy dissipation. The lack of MQ silicone resin will cause the silicone rubber to harden and become brittle at low temperatures, failing to meet the requirements of extreme working conditions.
[0067] The difference between Comparative Example 5 and Example 1 lies in the addition of an external low-temperature toughening agent in the surface adhesive layer formulation, simulating the existing technical solution of CN113737539A. The low-temperature flexural resistance of Comparative Example 5 decreased instead of increased: 87,000 cycles at -30℃ and only 42,000 cycles at -50℃, both lower than Example 1; after 500h QUV aging, ΔE reached as high as 4.5, and the tensile strength retention rate was only 68.5%; simultaneously, flame retardancy safety testing was conducted, and its total calorific value reached as high as 22.3 MJ / kg, failing the IMO FTP Code Part 8 flame retardancy test, with a smoke density Dm of 628 and a carbon monoxide concentration >1500 ppm, exceeding the smoke toxicity standard. The results show that although the added toughening agent can improve the toughness at room temperature to a certain extent, it is only physically blended with the silicone rubber matrix and lacks chemical bonding. It becomes brittle at low temperatures and cannot effectively toughen the material. At the same time, the added toughening agent contains a large number of carbon-hydrogen bonds and unsaturated bonds in its molecular structure. When burning, it releases a large amount of heat, smoke and toxic gas (CO), which seriously damages the flame retardant safety and smoke toxicity of the silicone artificial leather. In addition, the unsaturated bonds and aromatic ether bonds in the toughening agent are sensitive to ultraviolet light and are prone to photo-oxidative degradation, resulting in severe yellowing of the material and a sharp decline in mechanical properties.
[0068] The above test results show that the silicone artificial leather for marine furniture prepared in this application has the following excellent properties: low-temperature folding resistance at -30℃ and -50℃ is no less than 92,000 and 80,000 cycles respectively, meeting the requirements of extreme low-temperature environments such as polar navigation; initial peel strength is no less than 55 N / 25mm, and peel strength retention rate after 90 days of seawater immersion is no less than 87%; after 500 hours of QUV aging, the yellowing index ΔE is no higher than 0.8, the tensile strength retention rate is no less than 90%, and it passes the IMO FTP Code Part 8 flame retardancy test, with smoke density lower than the IMO limit, demonstrating excellent flame retardant safety. This invention, through the overall design of "aramid fiber base layer + intrinsically toughened silicone rubber coating," successfully overcomes the technical problem of simultaneously achieving low-temperature toughness and high flame retardancy, producing a product that combines safety and durability, fully meeting the comprehensive requirements of marine furniture decoration.
[0069] This specific embodiment is merely an explanation of the present invention and is not intended to limit the invention. After reading this specification, those skilled in the art can make modifications to this embodiment without contributing any inventive step, but as long as they are within the scope of the present invention, they are protected by patent law.
Claims
1. A type of silicone artificial leather for marine furniture, characterized in that, It has a multi-layer composite structure, including: a top adhesive layer, a base adhesive layer, and a base layer; The adhesive layer is made of modified silicone rubber material and serves as the surface layer that comes into direct contact with the usage environment. The base layer, disposed between the base layer and the top layer, is made of silicone rubber adhesive material and is used to achieve the bonding and composite bonding between the base layer and the top layer; The base layer is an aramid fiber fabric, which serves as the skeleton support layer of the overall structure; the aramid fiber fabric is either para-aramid fiber fabric or meta-aramid fiber fabric, and its unit area mass is 100-400g / m².
2. The silicone artificial leather for marine furniture according to claim 1, characterized in that, The adhesive layer is made from the following raw materials in parts by weight: 100 parts of α,ω-divinyl polydimethylsiloxane, 2-15 parts of hydrogen-containing silicone oil crosslinking agent, 0.01-0.5 parts of platinum catalyst, 0.01-0.1 parts of alkynyl alcohol inhibitor, 10-30 parts of silica reinforcing filler, 5-30 parts of vinyl MQ silicone resin, and 1-10 parts of functional additives.
3. The silicone artificial leather for marine furniture according to claim 2, characterized in that, The functional additive is two or more of the following: hydrophobic and oleophobic modifiers, UV inhibitors, and antibacterial and antifungal agents.
4. The silicone artificial leather for marine furniture according to claim 3, characterized in that, The hydrophobic and oleophobic modifier is any one of fluorinated silicone oil and perfluoroalkyl silane; the UV stabilizer is any one of nano-titanium dioxide and hindered amine light stabilizer; the antibacterial and antifungal agent is any one of nano-silver, organosilicon quaternary ammonium salt and zinc pyridinethione.
5. The silicone artificial leather for marine furniture according to claim 1, characterized in that, The base layer is made from the following raw materials in parts by weight: 100 parts of α,ω-divinyl polydimethylsiloxane, 2-10 parts of hydrogen-containing silicone oil crosslinking agent, 0.01-0.3 parts of platinum catalyst, 0.01-0.08 parts of alkynyl alcohol inhibitor, 5-20 parts of silica reinforcing filler, and 3-8 parts of tackifier.
6. The silicone artificial leather for marine furniture according to claim 5, characterized in that, The tackifier is two or more of the following: silane coupling agents containing silane-hydrogen bonds, silane coupling agents containing epoxy groups, silane coupling agents containing acryloyloxy groups, and silane coupling agents containing vinyl groups.
7. The silicone artificial leather for marine furniture according to claim 5, characterized in that, The thickener is a combination of vinyltrimethoxysilane and γ-glycidyl etheroxypropyltrimethoxysilane in a mass ratio of (1-2):
1.
8. The silicone artificial leather for marine furniture according to claim 1, characterized in that, The aramid fiber fabric is a para-aramid fiber fabric.
9. A method for preparing silicone artificial leather for marine furniture as described in any one of claims 1-8, characterized in that, Includes the following steps: S1. Surface pretreatment of aramid fiber fabric to improve its interfacial adhesion with silicone rubber coating; S2. Rubber compound preparation: Prepare the top layer rubber compound and the base layer rubber compound according to the formula; S3. Coating and Lamination: The top adhesive layer is coated onto release paper and initially cured at 100-180℃ to form the top adhesive layer; the bottom adhesive layer is coated onto the cured top adhesive layer; the pretreated aramid fiber base layer is bonded to the top adhesive layer coated with the bottom adhesive layer and pressure is applied; a second curing is performed at 100-180℃ to fully crosslink the bottom adhesive layer and bond the base layer, bottom adhesive layer and top adhesive layer together; the release paper is then peeled off to obtain the semi-finished silicone artificial leather. S4. The semi-finished silicone artificial leather is subjected to embossing and sanding surface finishing treatments to obtain the final product; The surface pretreatment method in step S1 is any one of plasma treatment, silane coupling agent impregnation treatment, or dopamine biomimetic modification combined with hyperbranched polysiloxane in-situ growth treatment.
10. The method for preparing silicone artificial leather for marine furniture according to claim 9, characterized in that, In step S3, the coating thickness of the top adhesive layer is 0.05-0.30 mm, and the initial curing time is 1-5 minutes; the coating thickness of the bottom adhesive layer is 0.05-0.20 mm; the pressure applied during bonding is 0.1-0.5 MPa, and the secondary curing time is 5-15 minutes.
Citation Information
Patent Citations
Organic silicon synthetic leather for ship and yacht furniture decoration and preparation method thereof
CN113737539A