A method for preparing micro-embossed splicing paper using an embossing process
By using nickel alloy or copper alloy hot stamping rollers and wetting treatment to form micron-level embossed textures on tipping paper, combined with hot stamping transfer and shaping treatment, the precision and cost problems of traditional dry pressing processes are solved, enabling high-speed production and rapid switching of multiple varieties of tipping paper.
Patent Information
- Application Number
- CN202611420756.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-17
AI Technical Summary
Traditional dry pressing processes have bottlenecks in maintaining micron-level texture accuracy, controlling production costs, and achieving functional integration. They are unable to form high-precision textures under high-speed production and are difficult to adapt to the rapid response of small-batch orders.
Using a nickel alloy or copper alloy hot stamping roller as a mold, the paper's plasticity is improved through wetting treatment. Combined with the synergistic effect of wet heat, micron-level concave and convex textures are imprinted under high-speed conditions, and hot stamping transfer is achieved simultaneously. Subsequently, a shaping treatment is performed to fix the texture, and finally a hydrophobic layer is sprayed on the surface.
It has achieved stable molding of micron-level embossed textures, reduced plate-making costs, improved production efficiency, enhanced the anti-counterfeiting function and tactile effect of products, and met the needs of high added value, multi-variety rapid production conversion.
Smart Images

Figure CN123109004A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of tobacco packaging materials technology, specifically a method for preparing micro-embossed splicing paper using a raised and recessed process. Background Technology
[0002] Tipping paper is a crucial packaging material at the junction of the cigarette filter and the cigarette stick. The fineness and consistency of its surface texture directly affect the appearance and tactile experience of the finished cigarette. In actual production, manufacturers typically use steel embossing rollers to dry-press the tipping paper base paper. The surface texture of the steel roller is formed by mechanical engraving or chemical etching. During embossing, the paper enters the pressing zone at room temperature, and the raised texture is created by the pressure of the roller surface and the compression deformation of the paper itself. Under this process, the basis weight of the tipping paper base paper is 34 g / m². 2 -45g / m 2 The paper is thin and the fibers are highly elastic. When dry-pressed at room temperature, the large molecular chains of the fibers cannot undergo sufficient plastic flow. After pressing, the texture rebounds rapidly after leaving the pressing area. The actual retained texture depth is only 30%-50% of the engraving depth of the pressing roller. Micron-level fine textures are particularly difficult to form.
[0003] The aforementioned traditional processing methods have significant limitations. First, the texture retention is poor. Dry embossing relies on paper compression and deformation rather than fiber plastic flow, resulting in severe texture depth decay, minimal improvement in tactile feel, and significant impact on texture clarity from speed fluctuations. When the embossing speed exceeds 120m / min, texture uniformity decreases significantly, making it impossible to balance high-speed production with high-precision textures. Second, there is a prominent conflict between plate-making costs and plate-changing efficiency. The cost of a single steel embossing roller is typically over ten thousand yuan, with a long engraving cycle. When companies need to switch between different texture varieties, frequent roller replacements lead to significant downtime losses, making it difficult to adapt to the rapid response of small-batch orders. Third, the functionality is limited. Traditional embossing only provides tactile differences; the hot stamping process must be performed separately, and the registration deviation caused by the two processes typically exceeds 0.3mm. Furthermore, there is no systematic design for anti-counterfeiting features, limiting product added value and anti-counterfeiting capabilities.
[0004] In summary, traditional dry pressing processes have bottlenecks in maintaining micron-level texture accuracy, controlling production costs, and achieving functional integration. There is an urgent need for a method to prepare tipping paper that can form micron-level fine textures at high speeds and also has hot stamping and anti-counterfeiting functions, in order to meet enterprises' production needs for high added value, multiple varieties, and rapid production transition. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing micro-embossed splicing paper using an embossing process. This method involves first preparing a nickel alloy or copper alloy hot stamping die with an engraved textured pattern on its surface as a mold; then selecting splicing paper base paper and wetting it with atomized water vapor at 30℃-60℃ until the surface moisture content reaches 8%-12%; finally, feeding the wetted base paper into a hot stamping die station at 80℃-150℃, and embossing it at a speed of 150m / min-400m / min and a pressure of 0.8bar-2.0bar to form a depth of 5μm-3. Micron-level embossed textures with a diameter of 0μm and a width of 20μm-200μm can be simultaneously introduced during embossing to achieve hot stamping and embossing in one step. The texture pattern can be selected from regular geometric shapes, biomimetic textures, or microtext with a minimum line width of 0.05mm. After embossing, the splicing paper is left to stand for 24h-48h in an environment of 20℃-40℃ and relative humidity of 20%-40% to set its shape. Finally, it is perforated, cut, and rolled up. A 0.02mm-0.08mm food-grade hydrophobic layer is sprayed on the texture surface. High-speed and stable processing of micron-level fine textures is achieved through hydrothermal synergistic plastic molding.
[0006] To solve the above-mentioned technical problems, the present invention provides the following technical solution: a method for preparing micro-embossed splicing paper using an embossing process, the specific steps of which are as follows: Step 1: Prepare a roller hot stamping plate with a preset texture pattern on the surface, as a micro-embossing mold; Step 2: Select the tipping paper base paper and wet it with atomized water vapor at a temperature of 30℃-60℃ to increase the surface moisture content of the base paper to 8%-12%. The wetting treatment time is 0.5h-2h. Step 3: Feed the moistened tipping paper into the hot stamping station. The hot stamping plate will emboss the surface of the tipping paper to form a micron-level texture. Control the embossing speed to be 150m / min-400m / min, the embossing pressure to be 0.8bar-2.0bar, and the roller temperature to be 80℃-150℃. Step 4: Place the embossed splicing paper in an environment with a temperature of 20℃-40℃ and a relative humidity of 20%-40% and let it stand for 24h-48h to set. Step 5: Punch, cut, and roll up the shaped splicing paper to obtain the finished micro-embossed splicing paper.
[0007] Furthermore, the hot stamping plate mentioned in step 1 is made of nickel alloy or copper alloy.
[0008] Furthermore, the engraving depth of the texture pattern described in step 1 is 10μm-50μm, the line width is 0.05mm-0.3mm, and the spacing between adjacent textures is 0.1mm-0.5mm.
[0009] Furthermore, the texture pattern described in step 1 is a regular geometric shape, a biomimetic texture, or microtext, wherein the minimum line width of the microtext is 0.05mm.
[0010] Furthermore, the basis weight of the tipping paper in step 2 is 34 g / m³. 2 -45g / m 2 The longitudinal tensile strength is 1.6kN / m-2.8kN / m, the longitudinal elongation is 1%-2.5%, and the moisture content is 5.5%-7.5%.
[0011] Furthermore, the surface of the tipping paper base paper is pre-coated with an ink layer or a coating layer, which contains thermochromic or photochromic pigments, and the texture of the micro-embossing is aligned with the color-changing area of the pigment.
[0012] Furthermore, the texture depth of the micron-level bump texture formed in step 3 is 5μm-30μm, and the texture width is 20μm-200μm.
[0013] Furthermore, in step 3, the embossing speed is further controlled at 200m / min-350m / min, the embossing pressure is controlled at 1.0bar-1.8bar, and the roller temperature is controlled at 100℃-140℃.
[0014] Furthermore, in step 3, during the embossing process, the electroplated aluminum foil layer is introduced between the hot stamping plate and the tipping paper to simultaneously complete the hot stamping transfer and micro-embossing.
[0015] Furthermore, step 5 also includes spraying a food-grade hydrophobic material onto the micro-embossed surface to form a hydrophobic layer with a thickness of 0.02mm-0.08mm.
[0016] Compared with existing technologies, this method for preparing micro-embossed splicing paper has the following advantages: I. This invention involves feeding wetted paper with a moisture content of 8%-12% into a hot stamping cylinder at 80℃-150℃ for embossing. The combined effect of heat and moisture softens the paper fibers and induces plastic deformation. Even under high-speed operation conditions of 150m / min-400m / min, it can still form micron-level textures with a depth of 5μm-30μm. After embossing and setting, the paper is subjected to constant temperature and humidity treatment for 24h-48h, resulting in a texture rebound rate of less than 5%. This invention solves the problems of rapid texture decay and difficulty in maintaining micron-level precision in conventional dry pressing processes, making the surface of the tipped paper delicate and the three-dimensional layers durable and stable.
[0017] II. This invention uses a roller hot stamping plate as both a micro-embossing mold and a hot stamping carrier. After introducing an electroplated aluminum foil layer at the embossing station, hot stamping transfer and micro-embossing can be completed simultaneously. The registration deviation between the hot stamping pattern and the embossed texture is controlled within ±0.1mm. Combined with the registration alignment of thermochromic or photochromic pigment coatings and microtext textures, the tipping paper simultaneously possesses three anti-counterfeiting functions: tactile texture recognition, optical color-changing verification, and microtext reading. Furthermore, the roller hot stamping plate is made of nickel alloy or copper alloy, reducing the cost per plate by 80%-90% compared to traditional embossing steel rollers, and shortening the plate changeover time to within 2 hours, thus adapting to the needs of rapid production conversion in small batches of multiple varieties.
[0018] Other advantages, objectives and features of the invention will be set forth in part in the description which follows, and in part will be apparent to those skilled in the art from the following examination or study, or may be learned from the practice of the invention. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are merely some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without any creative effort.
[0020] Figure 1 This is an overall process flow diagram of a method for preparing micro-embossed splicing paper using an embossing process; Figure 2 A process flow diagram of simultaneous hot stamping transfer and micro-embossing forming in a method for preparing micro-embossed splicing paper using an embossing process; Figure 3 This is a flowchart illustrating the post-processing steps of spraying a hydrophobic layer onto the micro-embossed surface in a method for preparing micro-embossed splicing paper using an embossing process. Detailed Implementation
[0021] To further illustrate the technical means and effects of the present invention in achieving its intended purpose, the following detailed description of the specific implementation methods, structures, features, and effects of the present invention, in conjunction with the accompanying drawings and preferred embodiments, is provided below.
[0022] Example 1 This embodiment provides a method for preparing micro-embossed splicing paper using an embossing process. This method forms micron-level embossed textures on the surface of the splicing paper, giving it a unique tactile effect and visual depth.
[0023] Step 1: Prepare a roller hot stamping plate with a preset textured pattern on its surface. In this step, the first step is to design and create a hot stamping die based on the desired embossed texture. Specifically, a nickel alloy is selected as the die material, and the preset texture is processed onto the surface of the cylinder using laser engraving or chemical etching. Nickel alloy has high hardness and wear resistance, which can meet the needs of long-term continuous embossing production, and its good thermal conductivity is conducive to the uniform temperature transfer during the embossing process.
[0024] The texture pattern is designed using regular geometric shapes, specifically a diamond-shaped grid arrangement. The engraving depth is controlled at 25μm. This depth ensures a clear raised and recessed layer on the surface of the splicing paper after embossing, while avoiding paper damage during the embossing process due to excessive engraving. The line width is controlled at 0.15mm, and the spacing between adjacent textures is controlled at 0.3mm. The selection of these engraving parameters is based on the following considerations: too small a line width will result in an insufficiently clear and prominent texture after embossing, while too large a line width will make the texture appear rough and lack refinement; too small a spacing between adjacent textures can easily cause stress concentration on the paper surface, while too large a spacing will result in insufficient texture density, affecting the overall tactile effect. After engraving, the roller surface is polished to remove burrs and sharp edges generated during the engraving process, ensuring the smoothness of the roller surface and preventing scratches on the splicing paper surface during embossing.
[0025] Step 2: Select the tipping paper base paper and perform a wetting treatment. In this step, the quantitative value is selected as 38 g / m³. 2 The base paper used is the tipping paper. This base paper has a longitudinal tensile strength of 2.2 kN / m, a longitudinal elongation of 1.8%, and a moisture content of 6.5%. The selection of these base paper parameters referenced industry standards for cigarette tipping paper, ensuring that the base paper possesses sufficient mechanical properties to withstand the tension and pressure during subsequent embossing processes.
[0026] The aforementioned tipped paper base paper is fed into the wetting treatment station, where it is wetting using atomized water vapor at a temperature of 45°C. The atomized water vapor is generated by an ultrasonic atomization device, with the water mist particle size controlled between 5μm and 10μm to ensure that the water vapor can uniformly adhere to the paper surface and penetrate into the paper fibers. The wetting treatment time is 1.5 hours. During the treatment, the moisture content of the paper is monitored in real time using an online moisture meter, ensuring that the surface moisture content of the base paper reaches 10%.
[0027] It's understandable that the main purpose of wetting treatment is to improve the plasticity of the paper. In its dry state, tipping paper has a tighter bond between fibers, making it quite rigid. Direct embossing can easily lead to fiber breakage, paper cracking, or texture rebound after embossing. Through atomized water vapor wetting treatment, water molecules penetrate between the paper fibers, weakening the hydrogen bonds between them, making the fibers softer. This significantly improves the paper's extensibility and plasticity, thus facilitating the formation of clear and durable micron-level embossed textures in subsequent embossing processes. Maintaining a moisture content within the range of 8% to 12% is the result of experimental optimization: too low a moisture content results in insufficient plasticization, making the paper prone to cracking during embossing and poor texture retention; too high a moisture content leads to excessive reduction in paper strength, making it prone to deformation or stretching in subsequent processes.
[0028] Step 3: Use a hot stamping roller to emboss a micron-level textured surface on the tipping paper. The moistened tipping paper is continuously fed into the hot stamping station. Driven by the traction roller, the tipping paper passes through the gap between the hot stamping station and the pressure roller at a constant speed. The hot stamping station has a preset textured pattern engraved on its surface, and the pressure roller is a smooth steel roller. The two work together to apply pressure to the passing tipping paper, causing the surface of the tipping paper to undergo plastic deformation according to the textured pattern of the hot stamping station, thereby forming a micron-level embossed texture.
[0029] The embossing speed is controlled at 280 m / min. The selection of embossing speed requires balancing production efficiency and embossing quality: too slow a speed, while improving embossing precision, results in low production efficiency, hindering large-scale industrial production; too fast a speed leads to insufficient paper dwell time in the embossing area, preventing sufficient fiber deformation and resulting in insufficient embossing depth or blurred texture. The embossing pressure is controlled at 1.5 bar. Embossing pressure directly determines the clarity and uniformity of the texture: too low a pressure prevents the texture on the hot stamping plate from being fully transferred to the paper surface, resulting in shallow or even indistinct embossing; too high a pressure may puncture the paper or cause excessive stretching deformation after embossing. The roller temperature is controlled at 120℃. The roller temperature setting is based on the following considerations: moderate heating makes it easier for paper fibers to undergo plastic deformation during embossing, while also aiding in rapid texture setting after embossing; too low a temperature results in insufficient fiber plasticization, while too high a temperature may cause excessive evaporation of moisture from the paper, leading to brittleness or scorching of the paper surface.
[0030] By controlling the aforementioned embossing parameters, a micron-level raised and recessed texture with a depth of 18 μm and a width of 80 μm is formed on the surface of the tipping paper. The actual values of texture depth and width depend on the size of the engraved pattern on the hot stamping plate and the setting of the embossing process parameters. During the embossing process, the paper fibers undergo plastic flow under the combined action of pressure and temperature, filling the groove area of the hot stamping plate, thereby replicating the raised and recessed structure corresponding to the pattern on the hot stamping plate on the paper surface.
[0031] Step 4: Place the embossed splicing paper in a specific environment for shaping. The embossed tipping paper is placed in a constant temperature and humidity environment (30℃, 30% relative humidity) for 36 hours for setting. During the setting process, the internal stress generated in the paper fibers during embossing is gradually released, and hydrogen bonds between fibers are re-established in new locations, thus fixing the raised and recessed texture formed by embossing. Temperature and humidity control are crucial for the setting effect: excessively high temperatures accelerate the evaporation of residual moisture in the paper, causing excessive fiber shrinkage and deformation; excessively low temperatures slow molecular movement and result in insufficient release of internal stress. Excessively high relative humidity causes the paper to continue absorbing moisture and expand, affecting the dimensional stability of the texture; excessively low relative humidity causes the paper to lose too much water and become brittle.
[0032] Step 5: Post-process the shaped splicing paper. After the tipping paper has been shaped, it undergoes a series of processes including punching, slitting, and winding. The punching process uses laser punching to create ventilation holes in predetermined areas of the tipping paper to adjust the cigarette's draw resistance and smoke dilution. The slitting process longitudinally cuts the wide tipping paper into several narrow rolls according to the finished product specifications. The winding process rewinds the slit tipping paper into a coil shape to obtain the finished micro-embossed tipping paper.
[0033] This embodiment improves the plasticity of the tipping paper base paper through wetting treatment, enabling the paper to form clear and uniform micron-level embossed textures during the embossing process. Post-embossing, constant temperature and humidity setting treatment ensures the durability of the texture. Actual testing shows that the micro-embossed tipping paper prepared according to this embodiment has good surface texture clarity and uniform texture depth, and exhibits high texture retention during subsequent storage and use, meeting the requirements for cigarette packaging materials.
[0034] Example 2 This embodiment provides a method for preparing micro-embossed splicing paper using an embossing process. Unlike embodiment one, this embodiment simultaneously completes hot stamping transfer during the embossing process and pre-coates an ink layer containing thermochromic pigments on the surface of the splicing paper base paper, so that the texture of the micro-embossing and the color-changing area of the pigment are overprinted and aligned.
[0035] Step 1: Prepare a roller hot stamping plate with a preset textured pattern on its surface. In this step, a copper alloy is selected to create the hot stamping dies. Copper alloy has excellent thermal conductivity and processing properties, making it suitable for creating hot stamping dies with fine textures. The texture pattern adopts a biomimetic design, simulating the microscopic texture structure of natural material surfaces, specifically a leaf vein-like biomimetic texture. The engraving depth is controlled at 40μm, the line width at 0.10mm, and the spacing between adjacent textures at 0.2mm. The selection of these parameters results in a delicate tactile feel in the embossed texture, and the irregular distribution of the biomimetic texture also helps to conceal minor imperfections that may occur on the paper during the embossing process.
[0036] Step 2: Select the tipping paper base paper and perform a wetting treatment. In this step, the quantitative value is selected as 42 g / m³. 2 The tipping paper base paper has a longitudinal tensile strength of 2.5 kN / m, a longitudinal elongation of 2.2%, and a moisture content of 7.0%. The basis weight of the base paper is slightly higher than that of Example 1 to accommodate the additional process load in the subsequent simultaneous hot stamping process.
[0037] Before wetting, an ink layer is first coated on the surface of the tipping paper. This ink layer contains thermochromic pigments, which can undergo reversible color changes within a specific temperature range. The ink layer is applied to the surface of the paper using gravure printing at a speed controlled at 200 m / min and a drying temperature controlled at 80°C to ensure the ink layer is fully dried and cured.
[0038] The tipped paper coated with the ink layer is fed into the wetting treatment station, where it is wetting with atomized water vapor at a temperature of 35°C for 2 hours, increasing the surface moisture content of the paper to 11%. It should be noted that the wetting treatment is performed after the ink coating is completed, at which point the ink layer has already dried and cured. The atomized water vapor mainly acts on the uncoated surface of the paper and the interior of the paper fibers, and will not significantly affect the already cured ink layer.
[0039] Step 3: Use a hot stamping roller to emboss a micron-level texture on the surface of the tipping paper, and simultaneously complete the hot stamping transfer. The moistened tipping paper is fed into the hot stamping cylinder station. Unlike Embodiment 1, in this embodiment, an electroplated aluminum foil layer is introduced between the hot stamping cylinder and the tipping paper during the printing process. Specifically, the electroplated aluminum foil is drawn from the unwinding device, passes through the guide rollers, and enters the pressing area between the hot stamping cylinder and the tipping paper. The hot stamping cylinder also functions as a hot stamping plate; its surface texture serves both as an embossing tool and as a transfer medium for hot stamping.
[0040] The embossing speed is controlled at 320 m / min. The embossing pressure is controlled at 1.8 bar. The roller temperature is controlled at 135℃. Under the combined action of the above temperature and pressure, the hot-melt adhesive layer of the electroplated aluminum foil melts, and the aluminum layer is peeled off from the electroplated aluminum base film and transferred to a predetermined area on the surface of the tipping paper under pressure. At the same time, the texture pattern on the surface of the hot stamping plate is imprinted on the surface of the tipping paper to form a micron-level embossed texture. Hot stamping transfer and micro-embossing are completed simultaneously in the same process, which not only simplifies the process flow but also ensures precise alignment between the hot stamping layer and the embossed texture.
[0041] The micron-level embossed texture formed during the embossing process has a depth of 25μm and a width of 120μm. While embossing and hot stamping are completed simultaneously, a precision registration system controls the alignment of the micro-embossed texture with the color-changing areas of the thermochromic pigment in the ink layer. The registration system uses photoelectric sensors to detect registration marks on the tipping paper surface and a servo motor to adjust the phase of the hot stamping cylinder in real time, ensuring that the relative positional deviation between the embossed texture and the thermochromic pigment area is controlled within 0.05mm.
[0042] Step 4: Place the embossed splicing paper in a specific environment for shaping. The tipping paper, after simultaneous embossing and hot stamping, is placed in a constant temperature and humidity environment (25℃, 25% relative humidity) and left to set for 42 hours. During the setting process, the internal stress of the paper fibers is gradually released, and the hot stamping layer bonds more firmly to the paper surface.
[0043] Step 5: Post-process the shaped splicing paper. After the tipping paper has been shaped, it is punched, cut and rolled up in sequence to obtain the finished micro-embossed tipping paper.
[0044] This embodiment achieves integrated processing of embossing and hot stamping by simultaneously introducing electroplated aluminum foil during the embossing process, reducing steps and improving production efficiency. Simultaneously, the precise alignment of the hot stamping layer and the embossed texture results in a more harmonious and unified decorative effect. The introduction of thermochromic pigments causes the tipping paper to change color with temperature during use, enhancing the product's visual appeal and anti-counterfeiting features. Actual testing shows that the micro-embossed tipping paper prepared according to this embodiment exhibits strong hot stamping adhesion, clear embossed texture, and normal color-changing effect of the thermochromic pigments; all performance indicators meet the requirements for cigarette tipping paper.
[0045] Example 3 This embodiment provides a method for preparing micro-embossed splicing paper using an embossing process. Unlike the previous embodiments, this embodiment further sprays a food-grade hydrophobic material onto the micro-embossed surface after embossing to form a hydrophobic layer, and uses more precise embossing parameter control during the embossing process.
[0046] Step 1: Prepare a roller hot stamping plate with a preset textured pattern on its surface. In this step, a nickel alloy material is used to create the hot stamping dies. The texture pattern uses microtext design, specifically a sequence of microtext representing the brand name, with a minimum line width of 0.05mm. The engraving depth is controlled at 15μm, the line width at 0.08mm, and the spacing between adjacent textures at 0.15mm. The microtext design gives the embossed packaging paper a high level of anti-counterfeiting value because the precision required for microtext is high, making it difficult to accurately replicate using ordinary counterfeiting methods.
[0047] Step 2: Select the tipping paper base paper and perform a wetting treatment. In this step, the quantitative value is selected as 35g / m 2 The tipping paper base paper has a longitudinal tensile strength of 1.8 kN / m, a longitudinal elongation of 1.5%, and a moisture content of 6.0%. The basis weight of the base paper is relatively low to meet the requirements of microtext for paper fineness.
[0048] The tipping paper is fed into the wetting treatment station and wetted with atomized water vapor at 50℃ for 1 hour, increasing the surface moisture content of the paper to 9%. For microtext embossing, precise control of the paper's moisture content is crucial: too high a moisture content results in overly soft paper, causing the fine lines of the microtext to easily deform or become blurred during embossing; too low a moisture content results in insufficient paper plasticity, preventing the fine lines of the microtext from fully taking shape.
[0049] Step 3: Use a hot stamping roller to emboss a micron-level textured surface on the tipping paper. The moistened tipping paper is fed into the hot stamping cylinder station. The embossing speed is controlled at 200 m / min, the embossing pressure at 1.2 bar, and the cylinder temperature at 110°C. Compared with the previous embodiment, this embodiment uses a lower embossing speed and lower embossing pressure to meet the higher embossing precision requirements of microtext. The lower embossing speed allows the paper more time to deform in the embossing area, which is beneficial for the full formation of the fine lines of the microtext; the lower embossing pressure avoids the adhesion between the fine lines of the microtext due to excessive pressure.
[0050] By controlling the embossing parameters described above, a micron-level raised texture with a depth of 10 μm and a width of 50 μm is formed on the surface of the tipping paper. This texture size matches the line width of the microtext, clearly presenting the shape and stroke details of the microtext.
[0051] Step 4: Place the embossed splicing paper in a specific environment for shaping. The embossed tipping paper is placed in a constant temperature and humidity environment controlled at 35℃ and 35% relative humidity, and left to stand for 30 hours for shaping.
[0052] Step 5: Post-process the shaped tipping paper and spray a food-grade hydrophobic material onto the micro-embossed surface. After the tipping paper has been shaped, it is first punched and slit. After slitting and before winding, a food-grade hydrophobic material is sprayed onto the micro-embossed surface using a micro-spraying device. Specifically, the food-grade hydrophobic material is a food-grade paraffin emulsion with a solid content controlled at 15% to 20%, the spraying pressure is controlled at 0.3 bar to 0.5 bar, and the spraying amount is controlled to form a hydrophobic layer with a thickness of 0.05 mm on the micro-embossed surface. The nozzles of the micro-spraying device are arranged along the width direction of the tipping paper. During spraying, the tipping paper passes through the micro-spraying station at a constant speed, and the hydrophobic material is evenly covered on the micro-embossed surface, including the raised and recessed parts of the texture.
[0053] After spraying, the tipping paper is dried using an infrared drying device at a temperature controlled between 60°C and 80°C to ensure the hydrophobic layer is fully cured. The formation of the hydrophobic layer effectively reduces the surface energy of the tipping paper, making it difficult for water molecules to adhere to and penetrate the paper surface, thus improving the tipping paper's moisture resistance and resistance to saliva penetration. Simultaneously, because the hydrophobic layer is relatively thin, it does not significantly affect the tactile effect of the micro-embossing. Finally, the paper is wound up to obtain the finished micro-embossed tipping paper.
[0054] This embodiment successfully created a micron-level embossed texture in the form of microtext on the surface of the tipping paper through precise control of embossing parameters, giving the product high anti-counterfeiting value. The coating of food-grade hydrophobic material further improves the moisture-proof performance of the tipping paper and extends the lifespan of the micro-embossing. Actual testing showed that the microtext on the tipping paper prepared according to this embodiment is clearly legible, and the contact angle measurement value of the hydrophobic layer is significantly improved compared to the untreated sample, demonstrating excellent moisture-proof performance.
[0055] Comparative Example 1 This comparative example provides a method for preparing embossing on spliced paper, which differs from the technical solution of the embodiments of the present invention. It is mainly used to illustrate the important influence of wetting treatment and shaping treatment on the embossing effect in the technical solution of the present invention.
[0056] Step 1: Prepare a roller hot stamping plate with a preset textured pattern on its surface. In this comparative example, the same nickel alloy material as in Example 1 was used to make the hot stamping dies. The texture pattern was also arranged in a diamond grid pattern, with an engraving depth of 25μm, a line width of 0.15mm, and a spacing of 0.3mm between adjacent textures.
[0057] Step 2: Select the tipping paper base paper and directly perform embossing treatment. In this comparative example, the same tipping paper as in Example 1 was selected, i.e., a basis weight of 38 g / m³. 2 The tipping paper base paper has a longitudinal tensile strength of 2.2 kN / m, a longitudinal elongation of 1.8%, and a moisture content of 6.5%. Unlike Example 1, this comparative example does not wet the base paper; instead, the base paper is directly fed into the embossing station for embossing at room temperature.
[0058] Step 3: Use a hot stamping roller to emboss the surface of the tipping paper to create a raised texture. Unwetted tipping paper is directly fed into the hot stamping station for embossing. The embossing speed is controlled at 280 m / min, the embossing pressure at 1.5 bar, and the roller temperature at 120°C. These parameters are consistent with those in Example 1 for comparison.
[0059] Step 4: Proceed directly to post-processing of the embossed splicing paper. After embossing, instead of shaping the splicing paper, the paper is directly punched, slit, and wound up to obtain the finished splicing paper.
[0060] Comparative analysis of the examples and embodiments The tipping paper prepared according to the method of Comparative Example 1 exhibited the following problems during the embossing process. First, because the base paper was not wetted, its plasticity was poor. During embossing, the paper fibers underwent brittle fracture rather than plastic deformation under pressure and temperature, resulting in obvious cracks and fiber damage in the embossed area, severely affecting the product's appearance and mechanical properties. Second, the depth of the embossed texture was uneven, with some areas showing a significantly shallower texture than the design value, resulting in unclear texture outlines and a poor tactile feel. Third, due to the lack of a setting treatment, the internal stress of the paper fibers was not fully released after embossing. During subsequent storage, the texture gradually rebounded and became shallower, resulting in poor durability of the embossing effect. After a period of storage, the texture clarity significantly decreased.
[0061] The above comparative results demonstrate that the wetting treatment in step 2 and the shaping treatment in step 4 of the present invention play an irreplaceable role in preparing high-quality micro-embossed splicing paper. The wetting treatment improves the plasticity of the paper, making the embossing process smoother and avoiding paper damage and uneven texture. The shaping treatment releases internal fiber stress and rebuilds inter-fiber hydrogen bonds, thus fixing the embossed texture and ensuring its durability. Without any of these key steps, it is difficult to obtain micro-embossed splicing paper products with clear, uniform, and durable textures.
[0062] Comparison of key process parameters between each embodiment and the comparative example To more clearly illustrate the differences between the various embodiments and the comparative examples, the following table summarizes the main process parameters and product characteristics of each scheme: The above comparison shows that each embodiment has made targeted adjustments to the wetting treatment, embossing parameters, and post-treatment according to different application requirements, and all can produce micro-embossed splicing paper products that meet the quality requirements. However, Comparative Example 1, lacking the two key steps of wetting and shaping treatments, has obvious quality defects and cannot meet the usage requirements of micro-embossed splicing paper. This fully demonstrates the necessity and rationality of the steps set in the technical solution of this invention.
[0063] In summary, the present invention provides a method for preparing micro-embossed splicing paper using an embossing process. Through the organic combination of wetting treatment, precisely controlled embossing, and shaping treatment, a clear, uniform, and durable micron-level embossed texture can be formed on the surface of the splicing paper. The various embodiments illustrate specific implementation schemes in different application scenarios, including the preparation of conventional micro-embossed splicing paper, the preparation of composite functional splicing paper with simultaneous embossing and hot stamping, and the preparation of functional splicing paper with micro-text anti-counterfeiting and a hydrophobic coating. The comparative results further verify the irreplaceable nature of the key steps in the technical solution of the present invention. Those skilled in the art can reasonably adjust the process parameters based on the above embodiments according to actual production needs without departing from the protection scope of the present invention.
[0064] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention in any way. Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Any person skilled in the art can make some modifications or alterations to the above-disclosed technical content to create equivalent embodiments without departing from the scope of the present invention. Any simple modifications, equivalent changes and alterations made to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing micro-embossed splicing paper using an embossing process, characterized in that, The specific steps of this preparation method are as follows: Step 1: Prepare a roller hot stamping plate with a preset texture pattern on the surface, as a micro-embossing mold; Step 2: Select the tipping paper base paper and wet it with atomized water vapor at a temperature of 30℃-60℃ to increase the surface moisture content of the base paper to 8%-12%. The wetting treatment time is 0.5h-2h. Step 3: Feed the moistened tipping paper into the hot stamping station. The hot stamping plate will emboss the surface of the tipping paper to form a micron-level texture. Control the embossing speed to be 150m / min-400m / min, the embossing pressure to be 0.8bar-2.0bar, and the roller temperature to be 80℃-150℃. Step 4: Place the embossed splicing paper in an environment with a temperature of 20℃-40℃ and a relative humidity of 20%-40% and let it stand for 24h-48h to set. Step 5: Punch, cut, and roll up the shaped splicing paper to obtain the finished micro-embossed splicing paper.
2. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The hot stamping plate mentioned in step 1 is made of nickel alloy or copper alloy.
3. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The engraving depth of the texture pattern described in step 1 is 10μm-50μm, the line width is 0.05mm-0.3mm, and the spacing between adjacent textures is 0.1mm-0.5mm.
4. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The texture pattern mentioned in step 1 is a regular geometric shape, a biomimetic texture, or microtext, wherein the minimum line width of the microtext is 0.05mm.
5. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The basis weight of the tipping paper in step 2 is 34 g / m³. 2 -45g / m 2 The longitudinal tensile strength is 1.6kN / m-2.8kN / m, the longitudinal elongation is 1%-2.5%, and the moisture content is 5.5%-7.5%.
6. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The surface of the tipping paper base paper is pre-coated with an ink layer or a coating layer, which contains thermochromic or photochromic pigments, and the texture of the micro-embossing is aligned with the color-changing area of the pigment.
7. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, The texture depth of the micron-level bump texture formed in step 3 is 5μm-30μm, and the texture width is 20μm-200μm.
8. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, In step 3, the embossing speed is further controlled at 200m / min-350m / min, the embossing pressure is controlled at 1.0bar-1.8bar, and the roller temperature is controlled at 100℃-140℃.
9. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, In step 3, during the embossing process, the electroplated aluminum foil layer is introduced between the hot stamping plate and the tipping paper to simultaneously complete the hot stamping transfer and micro-embossing.
10. The method for preparing a micro-embossed splicing paper according to claim 1, characterized in that, Step 5 also includes spraying a food-grade hydrophobic material onto the micro-embossed surface to form a hydrophobic layer with a thickness of 0.02mm-0.08mm.