A method for repairing and reinforcing tunnels in subway operating sections without interrupting service.
By combining an integrated drilling and injection geological drilling rig with anti-segregation early-strength micro-expansion composite cement grout, efficient and reliable repair of defects in tunnels in operating subway sections has been achieved, solving the problems of equipment adaptability and construction cycle, and improving the reinforcement quality and long-term reliability.
Patent Information
- Application Number
- CN202611287580.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-24
- Publication Date
- 2026-11-17
AI Technical Summary
Existing anchor bolt construction equipment and processes cannot meet the miniaturization requirements of operational subway sections, have long construction cycles, and the vibrations from subway operation affect the reinforcement effect, making it impossible to efficiently complete tunnel repair without interrupting operation.
An integrated drilling and grouting geological drilling rig was used to install anchor bolts at the skylight points. Anti-segregation early-strength micro-expansion composite cement grout was used for forward grouting, combined with drill rods as permanent anchor bolts, and supplementary grouting was used to form an effective anchoring system.
It achieves efficient and high-quality tunnel repair without interrupting subway operation, with good reinforcement quality, high long-term reliability, and adaptability to subway operation vibrations, thus solving the problems of equipment adaptability and construction cycle.
Smart Images

Figure SMS_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of subway tunnel repair technology, specifically relating to a method for repairing and reinforcing tunnels in operating subway sections without interrupting service. Background Technology
[0002] With the rapid development of my country's urban rail transit network and the continuous increase in its operational years, a large number of subway tunnel sections are entering a period of high incidence of defects. Problems such as lining cracks, structural water leakage, track bed voids, and structural deformation are becoming increasingly prominent, seriously threatening the operational safety and service life of subways. For the repair and reinforcement of defective structures in operating subway sections, anchor bolt support is a commonly used and effective technical means.
[0003] However, the current anchor bolt support construction has the following problems:
[0004] 1) Existing anchor bolt construction equipment and methods are mainly designed for new tunnels or open-cut foundation pits. The equipment is large in size and heavy in weight, which cannot meet the needs of miniaturized equipment for the lower rail of the platform screen doors in operating subway sections.
[0005] 2) Traditional anchor bolt construction process is complicated and has a long construction period, which cannot meet the limited working time requirements of operating subway sections;
[0006] 3) The contradiction between the repair and reinforcement construction of the subway section and the normal operation of the subway. The geological vibration generated by the subway operation will affect the reinforcement effect.
[0007] Therefore, there is an urgent need for a method to repair and reinforce tunnels in subway sections without interrupting operation, so as to complete the repair of tunnel defects in subway sections. Summary of the Invention
[0008] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for repairing and reinforcing tunnels in subway sections without interrupting subway operation. This method can efficiently complete the repair of tunnel defects without interrupting subway operation and achieves good repair and reinforcement quality.
[0009] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0010] A method for repairing and reinforcing tunnels in an operational subway section without interrupting service, employing a method of installing anchor bolts at skylight points for anti-buoyancy reinforcement and treatment of structural defects, specifically including the following steps:
[0011] Step 1: Position the geological drilling rig and lay out the anchor bolt holes and drill the holes;
[0012] Step 2, Advance Grouting Drilling and Final Hole Grouting: After the drill rod of the geological drilling rig penetrates the tunnel bed and subway structure into the strata, advance grouting begins. After drilling to the designed position at the bottom of the hole, final hole grouting is performed.
[0013] The forward grouting and final hole grouting use anti-segregation early-strength micro-expansion composite cement grout.
[0014] During the forward grouting process, the anti-segregation early-strength micro-expansion composite cement grout permeates and diffuses into the surrounding strata through the reserved grouting diffusion holes along the internal channels of the drill rod. After grouting is completed, drilling continues to the next stroke position, and this process is repeated until the designed bottom position of the hole is reached. After reaching the designed bottom position of the hole, the anti-segregation early-strength micro-expansion composite cement grout is injected until the rated grouting pressure (0.5MPa) and the designed grouting volume are reached to ensure that the grout in the anchor bolt hole and the surrounding strata are full.
[0015] Step 3, Remove the drill rod and leave the anchor: After the final hole grouting is completed, remove the drill rod and leave the drill rod that entered the formation in the formation to be used as an anchor.
[0016] Step 4: Install anchor plates: Install anchor plates at the exposed end of the anchor rod and tighten them with nuts to ensure a reliable connection between the anchor rod and the existing subway structure, thus completing the anchor rod construction.
[0017] Step 5, Supplementary grouting: After the anchor bolt construction is completed, a set time is set to perform supplementary grouting inside the anchor bolt. The supplementary grouting uses a low-shrinkage, high-permeability compensating grout.
[0018] The purpose of supplementary grouting in this invention is:
[0019] ①Prevent the two-component fast-setting grout injected during drilling for sealing purposes from hydrolyzing and losing its effectiveness over time;
[0020] ② Further fill the gap between the anchor bolt and the stratum to enhance the anchoring force of the anchor bolt;
[0021] ③ Ensure the long-term working performance of the anchor bolts.
[0022] Furthermore, the geological drilling rig is an integrated drilling and injection geological drilling rig, which is transported to the construction location by a rail flatbed vehicle.
[0023] Furthermore, the drill rod is a self-propelled hollow grouting anchor rod, and grouting diffusion holes are pre-reserved on the side wall of the drill rod; the number of grouting diffusion holes is 2.
[0024] Furthermore, the drill rod has a diameter of 42-50mm (preferably 42mm) and a length of 0.5-3m (preferably 2m); the grouting diffusion hole has a diameter of 2-5mm (preferably 3mm).
[0025] Furthermore, the stroke length of the forward grouting is 20-40cm (preferably 40cm), and the grouting pressure is less than or equal to 0.5MPa;
[0026] Furthermore, in step 2, if water or sand comes out during the drilling process, emergency sealing slurry needs to be injected to seal the hole and lubricate the drill bit.
[0027] Furthermore, the emergency sealing grout is a two-component fast-setting grout;
[0028] Furthermore, the two-component rapid-setting slurry comprises a liquid A and a liquid B; the mass ratio of liquid A to liquid B is 1:0.48-1.17; wherein,
[0029] Liquid A comprises the following raw materials in parts by weight:
[0030] Water glass: 100 parts; water: 20-80 parts; stabilizer: 0.1-1 parts; thickener: 0.05-0.3 parts;
[0031] Solution B comprises the following raw materials in parts by weight: aluminum sulfate: 5-20 parts; water: 80-120 parts.
[0032] Furthermore, the water glass used is water glass with a modulus of 2.4 to 3.3.
[0033] In this invention, the dual-liquid fast-setting grout can quickly block the water and sand outlet channels, prevent borehole instability, and reduce the loss of subsequent main grout, thus creating conditions for continued forward grouting.
[0034] Furthermore, the gel time of the two-component fast-setting grout is adjustable from 10s to 180s; its water dispersibility is such that the scouring residue rate is >80%; the two-component fast-setting grout of the present invention is significantly superior to ordinary cement grout and can form an initial water-stopping sealing layer.
[0035] Furthermore, based on a total cementitious material volume of 100 parts by weight, the anti-segregation early-strength micro-expansion composite cement slurry includes the following raw materials in parts by weight:
[0036] Ordinary Portland cement: 70-85 parts;
[0037] Ultrafine cement: 10-25 parts;
[0038] Silica fume: 3-8 parts;
[0039] Micro-expanded component: 2-6 parts;
[0040] Water-retaining and thickening components: 0.05–0.30 parts;
[0041] Dispersed water-reducing component: 0.2–1.0 parts;
[0042] Early-strength coagulation promoting component: 0.5–3 parts;
[0043] Defoaming component: 0.02–0.10 parts;
[0044] Water: Water-to-binder ratio 0.45–0.65.
[0045] In this invention, ordinary silicate cement is the main source of strength; ultrafine cement improves permeability and adapts to filling micro-voids around formation fissures and anchor bolts; silica fume improves grout density, impermeability, and steel-grout interface bonding; micro-expansion component compensates for shrinkage and enhances the density of the anchor bolt wrapping; water-retaining and viscosity-enhancing component improves suspension stability, prevents segregation and bleeding, and is suitable for low-pressure segmented forward grouting; dispersing and water-reducing component ensures pumpability at a low water-cement ratio; early-setting and early-strength component meets the short-time construction needs of nighttime skylights and improves early-stage stability; defoaming component reduces air bubbles in the grout and improves the density of the aggregate.
[0046] Furthermore, the micro-expansion component is selected from one or two of calcium sulfoaluminate-based expansion agents and calcium oxide-based expansion agents;
[0047] Furthermore, the water-retaining and thickening component is selected from one or more of hydroxypropyl methylcellulose, xanthan gum, and polyacrylamide;
[0048] Furthermore, the dispersed water-reducing component is selected from one or two of polycarboxylate water-reducing agents and naphthalene-based water-reducing agents;
[0049] Furthermore, the coagulation-promoting and early-strength component is selected from one or more of aluminum sulfate, calcium formate, and chlorine-free early-strength agents;
[0050] Furthermore, the defoaming component is selected from one or two of polyether defoamers and silicone defoamers.
[0051] Furthermore, the performance parameters of the anti-segregation early-strength micro-expansion composite cement grout are as follows: fluidity: 160~220mm; 30min fluidity retention rate: ≥80%; bleeding rate: ≤3%; initial setting time: 10~40 min; 1d compressive strength: ≥8MPa; 28d compressive strength: ≥30 MPa; volume expansion rate: 0.1%~1.5%.
[0052] Furthermore, the supplementary grouting is carried out 1.5-2.5 months (preferably 2 months) after the anchor bolt construction is completed.
[0053] Furthermore, based on 100 parts by weight of the total amount of cementitious material, the low-shrinkage, high-permeability compensating slurry comprises the following raw materials in parts by weight:
[0054] Ultrafine cement: 60-85 parts;
[0055] Ordinary Portland cement: 10-30 parts;
[0056] Silica fume or mineral admixtures: 3-10 parts;
[0057] Micro-expansion component: 2-8 parts;
[0058] Dispersed water-reducing component: 0.3–1.2 parts;
[0059] Water-retaining and thickening components: 0.03–0.20 parts;
[0060] Water: Water-to-binder ratio 0.40–0.55.
[0061] Furthermore, the ultrafine cement is cement that has passed through a 700-900 mesh (preferably 800 mesh) sieve.
[0062] The low-shrinkage, high-permeability compensating grout of this invention improves the ability to refill existing microcracks and grout shrinkage voids by using a higher proportion of ultrafine cement; it enhances long-term anchoring by compensating for shrinkage through micro-expansion components; and it balances fluidity and strength by using a low water-cement ratio and water-reducing agent.
[0063] Furthermore, the performance parameters of the low-shrinkage, high-permeability compensating slurry are as follows: Flowability: 180–260 mm; Bleeding rate: ≤2%; 1-day compressive strength: ≥10 MPa; 28-day compressive strength: ≥40 MPa; Linear shrinkage rate: ≤0.03%.
[0064] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0065] 1. This invention utilizes an integrated drilling and injection geological drilling rig, which is characterized by its small size and light weight (it can be lifted by 4 people). It can enter the track area from the lower rail of the subway station platform screen door and be transported to the construction position by a track flatbed truck, thus enabling the equipment to be placed without interrupting the operation of the subway section.
[0066] 2. The drill rod of the integrated drilling and grouting geological drilling rig of this invention adopts a self-advancing hollow grouting anchor rod. The drill rod is used as a permanent anchor rod, which combines the traditional three processes of anchor rod hole formation, anchor rod installation and anchor rod grouting into one process. During the drilling process, forward grouting is carried out simultaneously, and grouting is completed when the drilling reaches the bottom, which greatly improves the construction efficiency.
[0067] 3. The drill rod of this invention adopts a standard rod body with a diameter of 42mm and a length of 2m. Two grouting diffusion holes with a diameter of 3mm are reserved on the side wall of each drill rod to ensure that the grout can be evenly diffused from the inside of the drill rod to the surrounding strata.
[0068] 4. A forward grouting process is employed for formation reinforcement. Two months after construction, supplementary grouting is carried out within the installed anchor rods (drill rods). Abnormal sealing is also performed when water or sand leaks, achieving a seamless process of "grouting while drilling – abnormal sealing – later reinforcement," significantly improving the quality of non-stop repair construction. The forward grouting process penetrates and diffuses into the surrounding formation through grouting diffusion holes on the drill rod sidewall, filling formation fissures and voids to form a concretion, achieving continuous grouting and segmented reinforcement. The anti-segregation, early-strength, micro-expansion composite cement grout used is composed of ordinary cement, ultrafine cement, silica fume, micro-expansion components, viscosity-enhancing and water-reducing components, and water-reducing components. It maintains good pumpability, anti-segregation, and early strength formation ability even under low pressure conditions of less than or equal to 0.5 MPa. The drill rods are then used as permanent anchor rods. The hollow rod body is then used to perform supplementary grouting with low-shrinkage, high-permeability compensating grout. This breaks through the limitations of the traditional passive grouting process (that is, grouting is performed after problems occur in the repair and reinforcement process). Supplementary grouting is carried out after the forward grouting is completed, before external defects such as cracks or water leakage appear (that is, about 2 months later). The active grouting reinforcement method is used for secondary reinforcement treatment. On the one hand, it can prevent the modified water glass injected during drilling from hydrolyzing and failing, further enhancing the anchoring force of the anchor rod. On the other hand, it can repair solidified cracks caused by geological vibration during subway operation, make up for the early attenuation of sealing materials and voids in the anchoring zone, and improve the long-term anchoring reliability. The dual-liquid fast-setting grout used for abnormal sealing when water or sand is leaking can quickly form a sealing layer in the hole, reducing the risk of grout loss and hole wall instability.
[0069] In summary, this invention utilizes forward grouting to inject cement grout under high pressure into the stratum, filling stratum fissures and voids, improving stratum density and bearing capacity, and thus playing a role in stratum grouting reinforcement. The drill rod is left in the stratum as a permanent anchor and connected to the existing subway structure through anchor plates to form an effective anchoring system, playing a role in structural repair and reinforcement. At the same time, the supplementary grouting process improves the long-term anchoring reliability. It can not only reinforce the stratum around the damaged structure, but also provide additional anchoring force to the existing structure, and improve the anchoring quality, thus achieving overall reinforcement of the structure and the stratum. Detailed Implementation
[0070] The technical solution of the present invention will be clearly and completely described below. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.
[0071] 1. Integrated drilling and injection geological drilling rig: Model ZLJ1200, purchased from Shandong Jujiang Machinery Group;
[0072] 2. Drill pipe: Model Purchased from Linqing Taiyu Drill Tools Manufacturing Co., Ltd.
[0073] 3. Unless otherwise specified, all raw materials used in this invention are commercially available.
[0074] Example 1:
[0075] A reinforcement project for an operating subway section:
[0076] (1) Project Overview
[0077] After many years of operation, a subway tunnel section developed lining cracks and water leakage, requiring structural repair and reinforcement of the affected sections.
[0078] (2) Construction preparation
[0079] An integrated drilling and grouting geological drilling rig was selected as the construction equipment. The rig measures approximately 1200mm x 500mm x 600mm (length x width x height) and weighs about 500kg. It can be lifted by four workers and is easily lowered from the subway station platform screen doors. Hollow drill rods with a diameter of 42mm and a length of 2m were used, with two 3mm diameter grouting diffusion holes pre-drilled on the sidewall of each drill rod.
[0080] (3) Construction procedures:
[0081] A method for repairing and reinforcing tunnels in an operational subway section without interrupting service, employing a method of installing anchor bolts at skylight points for anti-buoyancy reinforcement and treatment of structural defects, specifically including the following steps:
[0082] Step 1: Position the geological drilling rig and lay out the anchor bolt holes and drill the holes.
[0083] The integrated drilling and injection geological drilling rig was transported to the subway platform. During the nighttime maintenance window, four workers placed the rig under the platform screen door and onto the track, then transported it to the construction site via a rail flatbed truck.
[0084] According to the design drawings, the anchor bolt hole positions are marked out. After accurate positioning, the geological drilling rig is in place.
[0085] Step 2, Forward grouting drilling:
[0086] The drill rod of the integrated drilling and grouting geological drilling rig penetrates the tunnel bed and subway lining structure. After entering the strata, it begins forward grouting. The specific operation is as follows:
[0087] ① Each stroke is 40cm long, and grouting is performed once after each 40cm stroke is completed;
[0088] ② The grouting pressure is controlled at less than or equal to 0.5 MPa, and the grout used in the forward grouting method is an anti-segregation early-strength micro-expansion composite cement grout;
[0089] ③The grout penetrates and diffuses into the surrounding strata through the internal channels of the drill pipe and through two 3mm grouting diffusion holes reserved on the side wall of the drill pipe;
[0090] ④ After grouting is completed, continue drilling to the next 40cm stroke position, and repeat this process until the bottom of the designed hole is reached;
[0091] ⑤ If water or sand comes out during drilling, inject emergency sealing grout to seal the hole. This grout also serves as a drill bit lubricant.
[0092] After drilling to the designed position at the bottom of the hole, inject anti-segregation early-strength micro-expansion composite cement grout until the rated grouting pressure (0.5MPa) and the designed grouting volume are reached to ensure that the grout in the anchor bolt hole and the surrounding stratum is full.
[0093] Step 3, Remove the drill rod and leave the anchor: After the final hole grouting is completed, remove the drill rod and leave the drill rod that entered the formation in the formation to be used as an anchor.
[0094] Step 4: Install anchor plates: Install anchor plates at the exposed ends of the anchor rods and tighten them with nuts to ensure a reliable connection between the anchor rods and the existing subway structure, thus completing the anchor rod construction.
[0095] Step 5, Supplementary Grouting: Two months after the anchor bolt construction is completed, supplementary grouting is carried out again through the internal channel of the drill rod (anchor bolt) left in the formation; low shrinkage and high permeability compensation grout is used for supplementary grouting; the supplementary grouting method is full-hole one-time grouting; the pressure of supplementary grouting is less than or equal to 0.5MPa.
[0096] In this embodiment,
[0097] The anti-segregation early-strength micro-expansion composite cement slurry comprises the following raw materials in parts by weight:
[0098] Ordinary Portland cement (P·O 42.5): 75 parts;
[0099] Ultrafine cement (800 mesh): 15 parts;
[0100] Silica fume: 5 parts;
[0101] Micro-expansion component (calcium sulfoaluminate-based expander): 3 parts;
[0102] Water-retaining and thickening component (xanthan gum): 0.14 parts;
[0103] Dispersed water-reducing component (polycarboxylate superplasticizer): 0.8 parts;
[0104] Promoting early coagulation and strength (calcium formate): 1 part;
[0105] Defoaming component (polyether defoamer): 0.06 parts;
[0106] Water: 55 parts;
[0107] Water-to-binder ratio: 0.55;
[0108] The two-component rapid-setting slurry includes a liquid A and a liquid B, with a weight ratio of liquid A to liquid B of 1:0.47~1.17;
[0109] Liquid A comprises the following raw materials in parts by weight:
[0110] Water glass with a modulus of 2.4 to 3.3: 100 parts;
[0111] Water: 20-80 parts;
[0112] Stabilizer: 0.1 to 1 part;
[0113] Tackifier: 0.05–0.3 parts;
[0114] Liquid B comprises the following raw materials in parts by weight:
[0115] Aluminum sulfate: 5-20 parts;
[0116] Water: 80-120 parts;
[0117] The low-shrinkage, high-permeability compensating slurry comprises the following raw materials in parts by weight:
[0118] Ultrafine cement (800 mesh): 73 parts;
[0119] Ordinary Portland cement (P·O 42.5): 16 parts;
[0120] Silica fume: 5 parts;
[0121] Micro-expansion component (calcium sulfoaluminate-based expander): 5 parts;
[0122] Dispersed water-reducing component (polycarboxylate superplasticizer): 0.9 parts;
[0123] Water-retaining and thickening component (xanthan gum): 0.1 parts;
[0124] Water: 48 portions;
[0125] Water-to-binder ratio: 0.48.
[0126] Example 2
[0127] (1) Project Overview
[0128] After many years of operation, a subway tunnel section developed structural uplift defects, requiring structural repair and reinforcement of the affected section.
[0129] (2) Construction preparation
[0130] An integrated drilling and grouting geological drilling rig was selected as the construction equipment. The rig measures approximately 1200mm x 500mm x 600mm (length x width x height) and weighs about 500kg. It can be lifted by four workers and is easily lowered from the subway station platform screen doors. Hollow drill rods with a diameter of 42mm and a length of 2m were used, with two 3mm diameter grouting diffusion holes pre-drilled on the sidewall of each drill rod.
[0131] (3) Construction procedures:
[0132] A method for repairing and reinforcing tunnels in an operating subway section without interrupting service is the same as in Example 1; the difference is:
[0133] The anti-segregation early-strength micro-expansion composite cement slurry comprises the following raw materials in parts by weight:
[0134] Ordinary Portland cement (P·O 42.5): 80 parts;
[0135] Ultrafine cement (800 mesh): 10 parts;
[0136] Silica fume: 4 parts;
[0137] Micro-expansion component (calcium sulfoaluminate-based expander): 5 parts;
[0138] Water-retaining and thickening component (hydroxypropyl methylcellulose): 0.14 parts;
[0139] Dispersed water-reducing component (naphthalene-based water-reducing agent): 0.8 parts;
[0140] Promoting coagulation and early strength (aluminum sulfate): 1 part;
[0141] Defoaming component (polyether defoamer): 0.06 parts;
[0142] Water: 50 parts;
[0143] Water-to-glue ratio: 0.50;
[0144] The weight ratio of liquid A to liquid B in the two-liquid rapid setting slurry is 1:0.47~1.17;
[0145] The low-shrinkage, high-permeability compensating slurry comprises the following raw materials in parts by weight:
[0146] Ultrafine cement (800 mesh): 78 parts;
[0147] Ordinary Portland cement (P·O 42.5): 11 parts;
[0148] Silica fume: 5 parts;
[0149] Micro-expansion component (calcium sulfoaluminate-based expander): 5 parts;
[0150] Dispersed water-reducing component (naphthalene-based water-reducing agent): 0.9 parts;
[0151] Water-retaining and thickening component (hydroxypropyl methylcellulose): 0.1 parts;
[0152] Water: 48 portions;
[0153] Water-to-binder ratio: 0.48.
[0154] Example 3
[0155] (1) Project Overview
[0156] After many years of operation, a subway tunnel section developed structural slab heave defects, requiring structural repair and reinforcement of the affected section.
[0157] (2) Construction preparation
[0158] An integrated drilling and grouting geological drilling rig was selected as the construction equipment. The rig measures approximately 1200mm x 500mm x 600mm (length x width x height) and weighs about 500kg. It can be lifted by four workers and is easily lowered from the subway station platform screen doors. Hollow drill rods with a diameter of 42mm and a length of 2m were used, with two 3mm diameter grouting diffusion holes pre-drilled on the sidewall of each drill rod.
[0159] (3) Construction procedures:
[0160] A method for repairing and reinforcing tunnels in an operating subway section without interrupting service is the same as in Example 1; the difference is:
[0161] The anti-segregation early-strength micro-expansion composite cement slurry comprises the following raw materials in parts by weight:
[0162] Ordinary Portland cement (P·O 42.5): 70 parts;
[0163] Ultrafine cement (800 mesh): 20 parts;
[0164] Silica fume: 6 parts;
[0165] Micro-expansion component (calcium oxide-based expander): 3 parts;
[0166] Water-retaining and thickening component (polyacrylamide): 0.14 parts;
[0167] Dispersed water-reducing component (naphthalene-based water-reducing agent): 0.8 parts;
[0168] Promoting coagulation and early strength (aluminum sulfate): 1 part;
[0169] Defoaming component (organic silicone defoamer): 0.06 parts;
[0170] Water: 50 parts;
[0171] Water-to-glue ratio: 0.50;
[0172] The weight ratio of liquid A to liquid B in the two-liquid rapid setting slurry is 1:0.8;
[0173] The low-shrinkage, high-permeability compensating slurry comprises the following raw materials in parts by weight:
[0174] Ultrafine cement (800 mesh): 68 parts;
[0175] Ordinary Portland cement (P·O 42.5): 21 parts;
[0176] Silica fume: 7 parts;
[0177] Micro-expansion component (calcium oxide-based expander): 3 parts;
[0178] Dispersed water-reducing component (naphthalene-based water-reducing agent): 0.9 parts;
[0179] Water-retaining and thickening component (polyacrylamide): 0.1 parts
[0180] Water: 48 portions;
[0181] Water-to-binder ratio: 0.48.
[0182] In embodiments 1-3 of the present invention,
[0183] The performance parameters of the anti-segregation early-strength micro-expansion composite cement grout are as follows:
[0184] Flowability: 160–220 mm;
[0185] 30-minute flowability retention rate: ≥80%;
[0186] Percolation rate: ≤3%;
[0187] Initial setting time: 10–40 min;
[0188] 1-day compressive strength: ≥8 MPa;
[0189] 28-day compressive strength: ≥30 MPa;
[0190] Volume expansion rate: 0.1%~1.5%.
[0191] The performance parameters of the two-component rapid-setting slurry are as follows:
[0192] Gel time: Adjustable from 10s to 180s;
[0193] Water dispersibility: Rinsing residue > 80%;
[0194] The performance parameters of the low-shrinkage, high-permeability compensating slurry are as follows:
[0195] Flowability: 180~260mm;
[0196] Perfusion rate: ≤2%;
[0197] 1-day compressive strength: ≥10MPa;
[0198] 28-day compressive strength: ≥40MPa;
[0199] Linear shrinkage rate: ≤0.03%.
[0200] Comparative Example 1
[0201] (1) Project Overview: Same as Example 1;
[0202] (2) Construction preparation: Same as in Example 1;
[0203] (3) Construction procedures:
[0204] A method for repairing and reinforcing tunnels in an operating subway section without interrupting service is the same as in Example 1; the difference is that step 5, supplementary grouting, is not performed.
[0205] Comparative Example 2
[0206] (1) Project Overview
[0207] After many years of operation, a subway tunnel section developed lining cracks and water leakage, requiring structural repair and reinforcement of the affected sections.
[0208] (2) Construction preparation: Same as in Example 1;
[0209] (3) Construction procedures:
[0210] A method for repairing and reinforcing tunnels in an operating subway section without interrupting service is the same as in Example 1; the difference is that: in step 5, the supplementary grouting is performed using a pressure of 2.0 MPa for fracturing grouting; the supplementary grouting material is: cement grouting material, with the following specific formula: 100 parts by weight of 425 silicate cement and 100 parts by weight of water.
[0211] Comparative Example 3
[0212] (1) Project Overview:
[0213] After many years of operation, a subway tunnel section developed lining cracks and water leakage, requiring structural repair and reinforcement of the affected sections.
[0214] (2) Construction preparation: Same as in Example 1;
[0215] (3) Construction procedures:
[0216] A method for repairing and reinforcing tunnels in an operating subway section without interrupting operation is the same as in Example 1; the difference is that: 1) step 5, which involves supplementary grouting, is not performed; 2) the grouting material used in the forward grouting in step 2 is cement grouting material, with the following specific formula: 100 parts by weight of 425 silicate cement and 100 parts by weight of water.
[0217] Example 1: Quality Inspection
[0218] After the repair is completed, anchor pull-out force testing, structural deformation monitoring, water leakage inspection, ground density testing, and grout stone strength testing are required to assess the repair quality.
[0219] Detection method:
[0220] 1. Anchor bolt pull-out force test: An anchor bolt pull-out test is conducted on site using an anchor bolt pull-out tester. One anchor bolt is randomly selected from every 10 anchor bolts for testing. The pull-out force should not be lower than the design value (usually ≥150kN).
[0221] 2. Structural Deformation Monitoring: High-precision level instruments are used to monitor the settlement, uplift, and horizontal displacement of the tunnel structure. The monitoring frequency is once a week within the first month after construction, once every two weeks within the first 1 to 3 months, and once a month after the third month. The cumulative deformation should be ≤5mm.
[0222] 3. Leakage inspection: Visual inspection combined with a leakage detector is used to check whether there is still leakage in the affected area. The reduction rate of the number of leakage points should be ≥90%, and there should be no obvious dripping or line flow.
[0223] 4. Soil density testing: Ground-penetrating radar is used to scan the strata in the reinforcement area. The soil reflection signals before and after construction are compared. The soil density improvement rate after grouting reinforcement should be ≥30%.
[0224] 5. Strength test of grout aggregate: Take grout aggregate samples on site, or obtain hardened grout samples by core drilling, and test their 7-day and 28-day compressive strength. The 28-day compressive strength should be ≥ the design requirements.
[0225] The test results of Example 1 and each comparative example are shown in Table 1;
[0226] Table 1 Comparison of reinforcement effect test results of various schemes
[0227]
[0228] As shown in Table 1, all indicators of Example 1 using the complete process of this invention meet the design requirements, and the reinforcement effect is optimal: the anchor pull-out force reaches 172kN, which is 14.7% higher than the design value; the cumulative deformation of the structure is only 2.3mm, which is far below the limit of 5mm; the leakage point reduction rate reaches 96%, which basically solves the original leakage problem; the soil density is increased by 42%, and the soil reinforcement effect is significant; the grout 28-day compressive strength reaches 37MPa, which meets the long-term stress requirements of the structure.
[0229] Comparative Example 1 did not undergo supplementary grouting, and the anchor pull-out force and ground compaction did not meet the design requirements, resulting in insufficient long-term anchoring performance. Comparative Example 2 used high-pressure fracturing grouting and ordinary cement grout for supplementary grouting. Although the pull-out force met the requirements, the grout strength was insufficient, and high-pressure grouting posed a risk of disturbing the existing structure. Comparative Example 3 neither underwent supplementary grouting nor used ordinary cement grouting for forward grouting. All indicators failed to meet the standards and could not meet the reinforcement requirements of the operating subway section.
[0230] The embodiments described above are merely preferred embodiments of the present invention, and not an exhaustive list of all possible implementations of the present invention. Any obvious modifications made by those skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.
Claims
1. A method for operating a subway section without stopping to repair and reinforce the tunnel, characterized in that, The method of using skylight anchor bolts for anti-buoyancy reinforcement and treatment of structural defects includes the following steps: Step 1: Position the geological drilling rig and lay out the anchor bolt holes and drill the holes; Step 2, Advance Grouting Drilling and Final Hole Grouting: After the drill rod of the geological drilling rig penetrates the tunnel bed and subway structure into the strata, advance grouting begins. After drilling to the designed position at the bottom of the hole, final hole grouting is performed. The forward grouting and final hole grouting use anti-segregation early-strength micro-expansion composite cement grout. Step 3, Remove the drill rod and leave the anchor: After the final hole grouting is completed, remove the drill rod and leave the drill rod that entered the formation in the formation to be used as an anchor. Step 4: Install anchor plates: Install anchor plates at the exposed ends of the anchor bolts to complete the anchor bolt construction; Step 5, Supplementary grouting: After the anchor bolt construction is completed, a set time is set to perform supplementary grouting inside the anchor bolt. The supplementary grouting uses a low-shrinkage, high-permeability compensating grout.
2. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... The geological drilling rig is an integrated drilling and injection geological drilling rig, which is transported to the construction site by rail flatbed truck; The drill rod is a self-propelled hollow grouting anchor rod, and grouting diffusion holes are reserved on the side wall of the drill rod; The drill rod has a diameter of 42-50 mm and a length of 0.5-3 m; the grouting diffusion hole has a diameter of 2-5 mm.
3. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... The stroke length of the forward grouting is 20-40cm, and the grouting pressure is less than or equal to 0.5MPa.
4. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... In step 2, if water and sand leak out during the drilling process, emergency sealing grout needs to be injected to seal the hole and lubricate the drill bit.
5. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... The emergency sealing grout is a two-component fast-setting grout.
6. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 5, is characterized in that... The two-component rapid-setting slurry comprises a liquid A and a liquid B; the mass ratio of liquid A to liquid B is 1:0.48-1.17; wherein, Liquid A comprises the following raw materials in parts by weight: Water glass: 100 parts; water: 20-80 parts; stabilizer: 0.1-1 parts; thickener: 0.05-0.3 parts; Solution B comprises the following raw materials in parts by weight: aluminum sulfate: 5-20 parts; water: 80-120 parts.
7. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... Anti-segregation, early-strength, micro-expansion composite cement slurry comprises the following raw materials in parts by weight: Silicate cement: 70-85 parts; Ultrafine cement: 10-25 parts; Silica fume: 3-8 parts; Micro-expanded component: 2-6 parts; Water-retaining and thickening components: 0.05–0.30 parts; Dispersed water-reducing component: 0.2–1.0 parts; Early-strength coagulation promoting component: 0.5–3 parts; Defoaming component: 0.02–0.10 parts; Water: Water-to-binder ratio 0.45–0.
65.
8. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 7, is characterized in that... The micro-expansion component is selected from one or two of calcium sulfoaluminate expansion agents and calcium oxide expansion agents; The water-retaining and thickening component is selected from one or more of hydroxypropyl methylcellulose, xanthan gum, and polyacrylamide; The dispersed water-reducing component is selected from one or two of polycarboxylate water-reducing agents and naphthalene-based water-reducing agents; The coagulation-promoting and early-strength-enhancing component is selected from one or more of aluminum sulfate, calcium formate, and chlorine-free early-strength agents; The defoaming component is selected from one or two of polyether defoamers and silicone defoamers.
9. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... The supplementary grouting is carried out 1.5-2.5 months after the anchor bolt construction is completed.
10. The method for repairing and reinforcing tunnels in an operating subway section without interrupting service, as described in claim 1, is characterized in that... The low-shrinkage, high-permeability compensating slurry comprises the following raw materials in parts by weight: Ultrafine cement: 60-85 parts; Ordinary Portland cement: 10-30 parts; Silica fume or mineral admixtures: 3-10 parts; Micro-expansion component: 2-8 parts; Dispersed water-reducing component: 0.3–1.2 parts; Water-retaining and thickening components: 0.03–0.20 parts; Water: Water-to-binder ratio 0.40–0.55.