Reflective photomask blank, reflective photomask and its manufacturing method

By using a light-absorbing film composed of platinum (Pt) and ruthenium (Ru) in a reflective photomask and controlling the reduction of its platinum (Pt) content along the thickness direction, the problem of thickness variation caused by cleaning is solved, the cleaning tolerance and etching efficiency of the reflective photomask are improved, and stable transfer of high-precision patterns is achieved.

CN123113231APending Publication Date: 2026-11-17SHIN ETSU CHEMICAL CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202610653247.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2025-05-15
Filing Date
2026-05-13
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing reflective photomasks exhibit significant variations in the thickness of the light-absorbing film during sulfuric acid and alkaline cleaning processes, leading to unstable phase difference and reflectivity. Furthermore, the low success rate of correction during etching makes it difficult to meet the high-precision pattern transfer requirements of logic generations 3nm and above.

Method used

The light-absorbing film is made of platinum (Pt) and ruthenium (Ru) materials in a predetermined ratio, and the platinum (Pt) content gradually decreases along the thickness direction. Combined with electron beam activated fluorine gas dry etching, the cleaning tolerance and etching efficiency are improved.

Benefits of technology

This technology achieves high tolerance of the light-absorbing film to sulfuric acid and alkali cleaning, improves wafer transfer characteristics (NILS value), and makes the etching process more controllable, ensuring stable transfer of high-precision patterns.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123113231A_ABST
    Figure CN123113231A_ABST
Patent Text Reader

Abstract

This invention relates to a reflective photomask preform having a light-absorbing film formed on a substrate, wherein the light-absorbing film has a thickness of 35-40 nm, is formed of a material containing platinum and ruthenium, and has a platinum content of 40 atomic% or more and less than 60 atomic% and a ruthenium content of more than 40 atomic% and less than 60 atomic% as an overall average of more than 96 atomic% of platinum and ruthenium, and the platinum content on the side furthest from the substrate is more than 50 atomic% and less than 90 atomic%; in part or all of the light-absorbing film, along its thickness direction from the side furthest from the substrate toward the substrate side, the platinum content decreases intermittently or continuously; the light-absorbing film has a reflectivity of 3-10% and a phase difference of 200-230 degrees to the exposure light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a reflective photomask for manufacturing semiconductor devices, a method for manufacturing a reflective photomask, and a reflective photomask blank for manufacturing a reflective photomask as a material for the reflective photomask. Background Technology

[0002] With the miniaturization of semiconductor devices, especially the high integration of large-scale integrated circuits, projection exposure requires high pattern resolution. In this context, phase-shifting photomasks have been developed in the field of photomasks as a means to improve the resolution of transferred patterns. The principle of the phase-shifting method is as follows: The phase of the transmitted light beam passing through the opening of the phase-shifting film of the phase-shifting photomask is controlled to be approximately 180 degrees phase-reversed with the phase of the transmitted light beam passing through the portion of the phase-shifting film adjacent to the opening. This causes interference of the transmitted light at the boundary between the opening and the portion adjacent to the opening, thereby reducing the light intensity and resulting in improved resolution and depth of focus of the transferred pattern. Photomasks based on this principle are generally called phase-shifting photomasks. In this case, the phase-shifting photomask is a transmission photomask that transmits the exposure light.

[0003] In the fabrication of phase-shifting photomasks, the phase-shifting photomask preform most commonly has a structure in which a phase-shifting film is stacked on a transparent substrate such as a glass substrate, and a film formed of a chromium (Cr)-containing material is stacked on the phase-shifting film. Phase-shifting films typically have a phase difference of 175 to 185 degrees and an exposure transmittance of approximately 6 to 30%. Most phase-shifting films are silicon (Si)-containing films, particularly those formed of materials containing molybdenum (Mo) and silicon (Si). Furthermore, films formed of chromium (Cr)-containing materials are used in combination with phase-shifting films and are controlled to have a thickness that provides the desired optical density. Films formed of chromium (Cr)-containing materials are often used as both a light-shielding film and an etching mask for etching the phase-shifting film.

[0004] As a phase-shifting photomask preform obtained by sequentially forming a phase-shifting film made of a silicon (Si)-containing material and a light-shielding film made of a chromium (Cr)-containing material on a transparent substrate, a method for manufacturing a phase-shifting photomask by patterning the phase-shifting film is generally known as follows: First, a photoresist film is formed on the light-shielding film made of the chromium (Cr)-containing material of the phase-shifting photomask preform, and a pattern is drawn on the photoresist film with light or an electron beam and developed to form a photoresist pattern. Then, using the photoresist pattern used as an etching mask, the light-shielding film made of the chromium (Cr)-containing material is dry-etched with a chlorine-based gas to form a pattern of the light-shielding film. Furthermore, using the pattern of the light-shielding film used as an etching mask, the phase-shifting film made of the silicon (Si)-containing material is dry-etched with a fluorine-based gas to form a pattern of the phase-shifting film, after which the photoresist pattern is removed, and the pattern of the light-shielding film is removed by dry etching with a chlorine-based gas.

[0005] In this case, a light-shielding film is allowed to remain outside the portion of the pattern (circuit pattern) on which the phase-shifting film is formed, and the outer periphery of the phase-shifting photomask is used as a light-shielding portion (light-shielding pattern) having an optical density of 3 or higher based on the total optical density of the phase-shifting film and the light-shielding film. This is to prevent exposure light from leaking from the outer periphery of the phase-shifting photomask when the circuit pattern is transferred to the wafer by a wafer exposure apparatus, so that the photoresist film on the adjacent chip of the wafer is irradiated from the portion located outside the circuit pattern. As a method for forming such a light-shielding pattern, the commonly used method includes: forming a new photoresist film after forming the pattern of the phase-shifting film and removing the photoresist pattern; forming a photoresist pattern in which the photoresist film is retained on the outer periphery of the light-shielding film by pattern drawing and development; and etching a film formed of a chromium (Cr)-containing material using the photoresist pattern as an etching mask to leave a light-shielding film on the outer periphery of the phase-shifting photomask.

[0006] In phase-shift photomask preforms requiring high-precision pattern formation, dry etching using gas plasma is primarily employed. Dry etching using chlorine-based gases (chlorine-based dry etching) is used for dry etching of films formed from chromium (Cr)-containing materials, while dry etching using fluorine-based gases (fluorine-based dry etching) is used for dry etching of films formed from silicon (Si)-containing materials or films formed from materials containing both molybdenum (Mo) and silicon (Si). In particular, it is known that in dry etching of films formed from chromium (Cr)-containing materials, using an etching gas containing 10 to 25% by volume oxygen (O2) relative to chlorine (Cl2) gas increases chemical reactivity and etching rate.

[0007] With the miniaturization of circuit patterns, there is a growing need for techniques to finely form circuit patterns for phase-shifting photomasks. In particular, auxiliary patterns for line patterns that support the resolution of the main pattern in a phase-shifting photomask are required to be formed smaller than the main pattern so that they are not transferred to the wafer during the transfer of the circuit pattern to the wafer via a wafer exposure apparatus. In phase-shifting photomasks used to generate line and spacing patterns on a wafer at a 10 nm half-pitch, the linewidth of the auxiliary patterns for the line patterns in the circuit of the phase-shifting photomask is required to be approximately 40 nm.

[0008] Chemically amplified resists capable of forming fine patterns consist of, for example, a base resin, an acid-generating agent, and a surfactant. Sensitivity can be increased because many reactions can utilize the acid generated through exposure as a catalyst. Using chemically amplified resists allows for the formation of mask patterns, such as fine phase-shift film patterns with linewidths below 0.1 µm. The resist is applied to the photomask preform via spin coating using a resist coater.

[0009] Furthermore, recent projection exposures require higher pattern resolution. However, even with transmission phase-shifted light masks, achieving the desired pattern resolution has become difficult. Therefore, starting with the logic 7nm generation, EUV lithography (EUVL), which uses extreme ultraviolet (EUV) light as the exposure light, began to be used.

[0010] Because EUV light is easily absorbed by any material, transmission lithography methods, such as those using conventional ArF excimer lasers, cannot be used. Therefore, reflective optics are used in EUVL. The wavelength of EUV light used in EUVL is 13 to 14 nm, while the wavelength of conventional ArF excimer laser light is 193 nm. Therefore, compared to conventional lithography using ArF excimer laser light, the exposure wavelength is shorter, and finer patterns can be transferred in the photomask.

[0011] Photomasks used in EUVL are reflective photomasks that reflect exposure light. They typically have a structure on a substrate, such as a glass substrate, in which a reflective film reflecting EUV light, a protective film protecting the reflective film, and an absorbing film absorbing EUV light are sequentially formed. As the reflective film, a multilayer reflective film obtained by alternately stacking low-refractive-index layers and high-refractive-index layers is used to improve the reflectivity of EUV light applied to the surface of the reflective film. Typically, a molybdenum (Mo) layer is used as the low-refractive-index layer of the multilayer reflective film, while a silicon (Si) layer is used as the high-refractive-index layer. A ruthenium (Ru) film is typically used as the protective film. Conversely, for the absorbing film, a material with a high absorption coefficient for EUV light is used, specifically, for example, a material containing chromium (Cr) or tantalum (Ta) as the main component. In earlier generations of EUVL, binary reflective photomasks that did not reflect light through the absorbing film were used.

[0012] A reflective photomask blank is formed by sequentially forming a reflective film that reflects EUV light, a protective film that protects the reflective film, and a light-absorbing film that absorbs EUV light on a substrate. As a method for manufacturing a reflective photomask from this reflective photomask, the light-absorbing film is patterned. Specifically, the following method is generally known: First, a resist film is formed on the light-absorbing film; a pattern is drawn on the resist film using light or an electron beam; and then, development is performed to form a resist pattern. Then, the light-absorbing film is patterned using the resist pattern used as an etching mask to form a pattern of the light-absorbing film; finally, the resist pattern is removed.

[0013] In EUVL at the logic 3nm generation or later, reflective photomasks (reflective phase-shift photomasks) with patterns of light-absorbing films possessing phase-shifting capabilities are used to form finer patterns on the wafer. Using reflective phase-shift photomasks yields higher wafer transfer characteristics than binary reflective photomasks. Wafer transfer characteristics can be represented by the normalized image logarithmic slope (NILS), which corresponds to the contrast of the light intensity transferred to the wafer. NILS can be obtained from the following formula:

[0014] NILS = (dI / dx) / (W × Ith)

[0015] Where W is the desired pattern size, Ith is the threshold for the light intensity providing W, and dI / dx is the gradient of the spatial image. When the NILS value is large, the optical image becomes sharper, and the dimensional controllability of the resist pattern on the wafer improves. Therefore, a large NILS value is effective for forming finer patterns on the wafer. Using a reflective phase-shifting photomask can provide a larger NILS value than a binary reflective photomask.

[0016] NILS is affected by the size of the pattern on the wafer, the spacing of the pattern, the reflectivity of the reflective phase-shifting mask to the exposure light, and the phase difference to the exposure light. For example, in a line and spacing pattern on the wafer with a size of 18 nm for both the line and the spacing, NILS takes a favorable value when the reflectivity to the exposure light is about 4% and the phase difference to the exposure light is about 215 degrees.

[0017] Furthermore, in reflective phase-shift photomasks, exposure light is incident and reflected at an angle on the reflective photomask. The phase-shift film needs to have a predetermined thickness to absorb a portion of the exposure light and provide a predetermined reflectivity. If the phase-shift film is thick, the masking effect of the phase-shift film blocking the exposure light during incident and reflection becomes more significant. To reduce the influence of the masking effect, a thinner phase-shift film that provides a predetermined reflectivity is advantageous.

[0018] Furthermore, during the fabrication of reflective phase-shifting photomasks, their use, and pattern correction, the light-absorbing film is exposed to cleaning with sulfuric acid and alkali. Repeated cleaning with sulfuric acid or alkali reduces the thickness of the light-absorbing film. In phase-shifting light-absorbing films, even slight variations in thickness can lead to significant changes in the phase difference and reflectivity to EUV light. Therefore, to stably form patterns of desired dimensions on a wafer, phase-shifting light-absorbing films require higher resistance to cleaning.

[0019] JP-A 2024-142177 (Patent Document 1) discloses a reflective mask preform having a substrate, a multilayer reflective film disposed on the substrate, and a thin film disposed on the multilayer reflective film. The thin film has a lower layer and an upper layer disposed on the lower layer. The lower layer is composed of a material containing an amorphous structure or a microcrystalline structure, and the crystallinity of the upper layer is higher than that of the lower layer. JP-A2024-142177 (Patent Document 1) also discloses an absorber film disposed on the multilayer reflective film, specifically an absorber film composed of a lower layer of a CrN film (a layer in contact with a protective film or a buffer layer) and an upper layer such as a PtRu film, and discloses that the absorber film has a phase-shifting function.

[0020] Reference List

[0021] Patent Document 1: JP-A 2024-142177 Summary of the Invention

[0022] JP-A 2024-142177 (Patent Document 1) discloses a CrN film for use as a lower layer, having a chromium (Cr) content of 90 atomic% and a nitrogen (N) content of 10 atomic%; and a PtRu film for use as an upper layer containing platinum (Pt) and ruthenium (Ru), having a platinum (Pt) content of at least 22 atomic% and at most 53 atomic% platinum (Pt). The total thickness of these films, i.e., the thickness of the absorber film, is 30 nm.

[0023] However, when the platinum (Pt) content is below 50 atomic%, repeated cleaning with sulfuric acid or alkali significantly reduces the thickness of the light-absorbing film. In contrast, when the platinum (Pt) content is high, the reflectivity as a phase-shifting film is lower than the preferred reflectivity of 3 to 10% because platinum (Pt) has a larger extinction coefficient k relative to ruthenium (Ru), and the phase difference as a phase-shifting film deviates significantly from the preferred phase difference of about 215 degrees, resulting in deterioration of wafer transfer characteristics (NILS).

[0024] Furthermore, in the case of films containing platinum (Pt) and ruthenium (Ru), the pattern can be corrected by dry etching using an electron beam-activated fluorine-based gas. However, in absorber films consisting of a lower CrN film and an upper layer such as a PtRu film, the CrN film cannot be processed by dry etching using an electron beam-activated fluorine-based gas; instead, it must be corrected by dry etching using an electron beam-activated chlorine-based gas. Therefore, in absorber films consisting of a lower CrN film and an upper layer such as a PtRu film, correction is performed using two types of etching with different etching gases. As a result, the success rate of pattern correction for the light-absorbing film is significantly reduced compared to the case of correction using a single type of etching.

[0025] The present invention was completed to solve the above-mentioned problems. The object of the present invention is to provide a reflective photomask preform, a reflective photomask having a pattern of a light-absorbing film, and a method for manufacturing a reflective photomask from the reflective photomask preform, wherein the reflective photomask preform has the light-absorbing film as a phase-shifting light-absorbing film, the light-absorbing film having high tolerance to cleaning with sulfuric acid and alkali, high wafer transfer characteristics (high NILS), and the light-absorbing film that can be easily processed by dry etching using an electron beam activated fluorine gas.

[0026] As a result of in-depth research aimed at solving the aforementioned problems, the inventors made the following discovery: In reflective photomask blanks and reflective photomasks, the light-absorbing film is formed from a material containing predetermined amounts of platinum (Pt) and ruthenium (Ru) as main components, and is configured such that the platinum (Pt) content is set high on the side of the light-absorbing film furthest from the substrate, while the platinum (Pt) content decreases along the thickness direction of the light-absorbing film from the side furthest from the substrate towards the substrate side. It has been found that, due to this configuration, a relatively thin light-absorbing film with high wafer transfer characteristics (NILS) and phase shifting function exhibits high tolerance to cleaning with sulfuric acid and alkali, and can be easily processed using dry etching with electron beam activated fluorine gas during pattern correction of the light-absorbing film. Based on this discovery, the present invention was realized.

[0027] Therefore, the present invention provides the following reflective photomask blank, reflective photomask, and method for manufacturing reflective photomask.

[0028] 1. A reflective photomask preform, comprising a substrate, a multilayer reflective film formed on the substrate and reflecting exposure light as extreme ultraviolet (EUV) light, a protective film formed on the multilayer reflective film for protecting the multilayer reflective film, and a light-absorbing film formed on the protective film in contact with the protective film, which absorbs exposure light and has a phase-shifting function, wherein...

[0029] The light-absorbing film has a thickness of 35nm or more and 40nm or less.

[0030] The light-absorbing film is formed from a material containing platinum (Pt) and ruthenium (Ru).

[0031] As the overall average value in the light-absorbing film, the content of platinum (Pt) is greater than 40 atomic% and less than 60%, the content of ruthenium (Ru) is greater than 40 atomic% and less than 60 atomic%, and the total content of platinum (Pt) and ruthenium (Ru) is greater than 96 atomic%.

[0032] The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is greater than 50 atomic% and less than 90 atomic%.

[0033] In part or all of the light-absorbing film, along its thickness direction, from the side of the light-absorbing film furthest from the substrate towards the substrate side, the platinum (Pt) content decreases intermittently or continuously, and

[0034] The light-absorbing film has a reflectivity of 3% or more and less than 10% for the exposed light and a phase difference of 200 degrees or more and less than 230 degrees for the exposed light.

[0035] 2. According to the reflective photomask blank of 1, wherein the content of platinum (Pt) on the side of the light-absorbing film closest to the substrate is 40 atomic% or more and 50 atomic% or less.

[0036] 3. According to the reflective photomask blank of 1, wherein the content of platinum (Pt) on the side of the light-absorbing film furthest from the substrate is 52 atomic% or more.

[0037] 4. According to the reflective photomask blank of 1, when the protective film and the light-absorbing film are etched under the same conditions by dry etching using an electron beam-activated fluorine gas, the ratio of the etching rate of the light-absorbing film to the etching rate of the protective film is 50 or more.

[0038] 5. The reflective photomask blank according to 1, wherein the protective film is formed of a material containing rhodium (Rh).

[0039] 6. The reflective photomask preform according to 1, further comprising a hard mask film formed on and in contact with the light-absorbing film.

[0040] 7. The reflective photomask preform according to 6, wherein the hard mask film is formed of a material that is resistant to fluorine-based dry etching and can be etched by chlorine-based dry etching.

[0041] 8. The reflective photomask preform according to 7, wherein the hard mask film is formed of a material containing chromium (Cr) and has a thickness of more than 2 nm and less than 14 nm.

[0042] 9. A reflective photomask, comprising a substrate, a multilayer reflective film formed on the substrate and reflecting exposure light as extreme ultraviolet (EUV) light, a protective film formed on the multilayer reflective film for protecting the multilayer reflective film, and a pattern of a light-absorbing film formed on the protective film in contact with the protective film, which absorbs exposure light and has a phase-shifting function, wherein...

[0043] The light-absorbing film has a thickness of 35nm or more and 40nm or less.

[0044] The light-absorbing film is formed from a material containing platinum (Pt) and ruthenium (Ru).

[0045] As the overall average value in the light-absorbing film, the content of platinum (Pt) is greater than 40 atomic% and less than 60%, the content of ruthenium (Ru) is greater than 40 atomic% and less than 60 atomic%, and the total content of platinum (Pt) and ruthenium (Ru) is greater than 96 atomic%.

[0046] The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is greater than 50 atomic% and less than 90 atomic%.

[0047] In part or all of the light-absorbing film, along its thickness direction, from the side of the light-absorbing film furthest from the substrate towards the substrate side, the platinum (Pt) content decreases intermittently or continuously.

[0048] The light-absorbing film has a reflectivity of 3% or more and less than 10% for the exposed light and a phase difference of 200 degrees or more and less than 230 degrees for the exposed light.

[0049] 10. According to the reflective photomask of 9, the content of platinum (Pt) on the side of the light-absorbing film closest to the substrate is 40 atomic% or more and 50 atomic% or less.

[0050] 11. According to the reflective photomask of 9, the content of platinum (Pt) on the side of the light-absorbing film furthest from the substrate is 52 atomic% or more.

[0051] 12. According to the reflective photomask of 9, when the protective film and the light-absorbing film are etched under the same conditions by dry etching using an electron beam-activated fluorine gas, the ratio of the etching rate of the light-absorbing film to the etching rate of the protective film is 50 or more.

[0052] 13. The reflective photomask according to 9, wherein the protective film is formed of a material containing rhodium (Rh).

[0053] 14. A method for manufacturing a reflective photomask including a pattern of a light-absorbing film from a reflective photomask preform according to any one of 6 to 8, the method comprising the steps of:

[0054] (A) Forming a resist film that contacts the side of the hard mask film furthest from the substrate.

[0055] (B) Patterning the resist film to form a resist pattern.

[0056] (C) Using a resist pattern as an etching mask, a hard mask film is patterned by dry etching with chlorine-based gases to form the pattern of the hard mask film.

[0057] (D) Remove the resist pattern.

[0058] (E) Using the pattern of the hard mask film as an etching mask, the light-absorbing film is patterned by dry etching with fluorine-based gases to form the pattern of the light-absorbing film, and

[0059] (F) The pattern of the hard mask film is removed by dry etching using chlorine-based gases.

[0060] Beneficial effects of the present invention

[0061] The light-absorbing film patterns of the reflective photomask preform and the reflective photomask of the present invention, as light-absorbing films with phase-shifting functions, exhibit high tolerance to sulfuric acid and alkaline cleaning, with minimal thickness reduction caused by sulfuric acid and alkaline cleaning. Furthermore, when correcting the pattern of the light-absorbing film, it can be easily processed by dry etching using an electron beam-activated fluorine gas. The reflective photomask with the light-absorbing film pattern has high wafer transfer characteristics (high NILs). Therefore, the reflective photomask of the present invention provides for the transfer of finely detailed line and spacing patterns on a wafer and excellent transfer patterns. Attached Figure Description

[0062] Figure 1 This is a cross-sectional view depicting an example of a first embodiment of a reflective photomask blank according to the present invention.

[0063] Figure 2 This is a cross-sectional view depicting an example of a second embodiment of a reflective photomask blank according to the present invention.

[0064] Figure 3 This is a cross-sectional view depicting a third-order example of a reflective photomask blank according to the present invention.

[0065] Figure 4 This is a cross-sectional view depicting an example of a first embodiment of the reflective photomask of the present invention.

[0066] Figure 5 This is a cross-sectional view depicting an example of a second embodiment of the reflective photomask of the present invention.

[0067] Figure 6 (A) to 6(F) are cross-sectional views for explaining the steps of manufacturing a reflective photomask according to the second aspect of the invention from a reflective photomask blank according to the second aspect of the invention. Detailed Implementation

[0068] The invention will be described in more detail below.

[0069] The reflective photomask preform according to the present invention comprises a substrate, a multilayer reflective film formed on the substrate (on one of the main surfaces of the substrate), a protective film formed on the multilayer reflective film, and a light-absorbing film formed on the protective film. The reflective photomask preform of the present invention may additionally include a hard mask film formed on the light-absorbing film. Furthermore, the reflective photomask preform of the present invention may additionally include a resist film formed directly or via other films on the light-absorbing film or the hard mask film.

[0070] The reflective photomask blank of the present invention can be used to obtain a reflective photomask, which has, for example, a substrate, a multilayer reflective film formed on the substrate, a protective film formed on the multilayer reflective film, and a pattern (circuit pattern or photomask pattern) of a light-absorbing film formed on the protective film.

[0071] When a reflective photomask is held on the mask stage of an exposure apparatus, it is typically secured by an electrostatic chuck. Therefore, the reflective photomask blank and reflective photomask of the present invention may additionally have a conductive film (back film) for securing the reflective photomask to the substrate by an electrostatic chuck (on the back side of the substrate (the surface opposite to the surface on which, for example, a multilayer reflective film is formed, i.e., another main surface)).

[0072] The structure of the reflective photomask blank and the reflective photomask of the present invention will be described below with reference to the accompanying drawings. In the description of the drawings, the same reference numerals are used to denote the same components, and their descriptions may be omitted. Furthermore, for convenience, the drawings may be shown in an enlarged form, and the dimensional ratios of individual components are not necessarily the same as the actual dimensional ratios.

[0073] Figure 1 This is a cross-sectional view depicting an example of a first embodiment of a reflective photomask blank according to the present invention. The reflective photomask blank 101 has a substrate 1, a multilayer reflective film 2 formed in contact with the substrate 1 on one of the main surfaces of the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2 on the multilayer reflective film 2, and a light-absorbing film 4 formed in contact with the protective film 3 on the protective film 3.

[0074] Figure 2 This is a cross-sectional view depicting an example of a second embodiment of a reflective photomask preform according to the present invention. The reflective photomask preform 102 includes a substrate 1, a multilayer reflective film 2 formed in contact with one of the main surfaces of the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, a light-absorbing film 4 formed in contact with the protective film 3, and a hard mask film 5 formed in contact with the light-absorbing film 4. Furthermore, a conductive film 6 is provided, which is formed on and in contact with another main surface of the substrate 1.

[0075] Figure 3This is a cross-sectional view depicting a third-order example of a reflective photomask preform according to the present invention. The reflective photomask preform 103 includes a substrate 1, a multilayer reflective film 2 formed in contact with the substrate 1 on one of the main surfaces of the substrate 1, a protective film 3 formed in contact with the multilayer reflective film 2, a light-absorbing film 4 formed in contact with the protective film 3, a hard mask film 5 formed in contact with the light-absorbing film 4, and a photoresist film 7 formed in contact with the hard mask film 5. Furthermore, a conductive film 6 is provided, which is formed on and in contact with another main surface of the substrate 1.

[0076] Figure 4 This is a cross-sectional view depicting an example of a first embodiment of a reflective photomask according to the present invention. The reflective photomask 201 has a pattern 4a of a substrate 1, a multilayer reflective film 2 formed on the substrate 1 in contact with the substrate 1, a protective film 3 formed on the multilayer reflective film 2 in contact with the multilayer reflective film 2, and a light-absorbing film formed on the protective film 3 in contact with the protective film 3.

[0077] Figure 5 This is a cross-sectional view depicting an example of a second embodiment of the reflective photomask of the present invention. The reflective photomask 202 has a pattern 4a of a substrate 1, a multilayer reflective film 2 formed on and in contact with the substrate 1, a protective film 3 formed on and in contact with the multilayer reflective film 2, and a light-absorbing film formed on and in contact with the protective film 3. Furthermore, a conductive film 6 is provided, which is formed on and in contact with another main surface of the substrate 1.

[0078] There are no particular restrictions on the type and size of the substrate. The substrate for reflective photomask preforms and reflective photomasks may or may not be transparent at the exposure wavelength. For example, glass substrates, such as quartz substrates, can be used as substrates. Furthermore, the substrate is preferably a substrate referred to as, for example, a 6025 substrate, which has dimensions of 6 inches square and a thickness of 0.25 inches, and is defined in the SEMI standard. If SI units are used, a 6025 substrate is typically expressed as a substrate of 152 mm square and 6.35 mm thick.

[0079] A multilayer reflective film is a film that reflects exposure light as extreme ultraviolet (EUV) light. The multilayer reflective film is preferably formed in contact with a substrate. EUV light has a wavelength of 13 to 14 nm, and is typically light with a wavelength of about 13.5 nm.

[0080] The material used to form the multilayer reflective film is preferably a material that is resistant to dry etching (chlorine-based dry etching) using chlorine-based gases (e.g., chlorine gas alone (Cl2 gas), or a mixture of chlorine gas (Cl2 gas) and oxygen gas (O2 gas).

[0081] Specific examples of materials used to form multilayer reflective films include silicon (Si) and molybdenum (Mo). As a multilayer reflective film, a stack of films consisting of about 20 to 60 layers obtained by alternately stacking silicon (Si) layers and molybdenum (Mo) layers is typically used (Si / Mo stack).

[0082] The thickness of the multilayer reflective film is preferably 200 nm or more, more preferably 220 nm or more, and preferably 340 nm or less, more preferably 280 nm or less. The thickness of the silicon (Si) layer is preferably 2 nm or more, more preferably 3 nm or more, and preferably 6 nm or less, more preferably 5 nm or less. The thickness of the molybdenum (Mo) layer is preferably 1 nm or more, more preferably 2 nm or more, and preferably 5 nm or less, more preferably 4 nm or less.

[0083] A protective film is used to protect a multilayer reflective film. The protective film is preferably formed in contact with the multilayer reflective film. The protective film is provided for example, to protect the multilayer reflective film during cleaning in the processing from a reflective photomask preform to a reflective photomask, and during the cleaning and correction of the reflective photomask. Furthermore, the protective film preferably has the function of protecting the multilayer reflective film when patterning the light-absorbing film by etching and preventing oxidation of the multilayer reflective film.

[0084] The material used to form the protective film is preferably a material with different etching properties than that of the light-absorbing film, and specifically, a material resistant to dry etching using fluorine-based gases (SF6, CF4, etc.), such as dry etching using a mixture of SF6 and helium (He) (fluorine-based dry etching), and dry etching using chlorine-based gases (e.g., only chlorine (Cl2) or a mixture of chlorine (Cl2) and oxygen (O2) (chlorine-based dry etching). Furthermore, the material used to form the protective film is preferably a material resistant to cleaning solutions containing sulfuric acid or alkali.

[0085] Specific examples of materials used to form the protective film include materials containing rhodium (Rh). The materials used to form the protective film are preferably resistant to fluorine-based dry etching, chlorine-based dry etching, and dry etching by activating fluorine gases with an electron beam. From this point of view, elemental rhodium (Rh) is more preferably used to form the protective film.

[0086] The protective film can be a single-layer film or a multi-layer film (e.g., a film composed of 2 to 4 layers). Furthermore, the protective film can be a film with a gradient composition. The thinner the protective film, the higher the reflectivity of the exposure light from the multi-layer reflective film of the reflective photomask. In exposure using a reflective photomask, a larger amount of exposure light is applied to the wafer, and the productivity in exposure using a reflective photomask is improved. Conversely, if the thickness is too thin, the protective film loses its function of protecting the multi-layer reflective film. Therefore, the thickness of the protective film is preferably 1 nm or more, preferably 6 nm or less, and more preferably 4 nm or less.

[0087] The light-absorbing film is a film that absorbs exposure light in the extreme ultraviolet region. The light-absorbing film and its pattern are preferably formed in contact with a protective film.

[0088] The material used to form the light-absorbing film is preferably a material that can be etched using dry etching with fluorine-based gases (SF6, CF4, etc.) (fluorine-based dry etching), such as dry etching using a mixture of SF6 and helium (He). Furthermore, the material used to form the light-absorbing film is preferably a material that is resistant to dry etching using chlorine-based gases (e.g., chlorine alone, or a mixture of chlorine (Cl2) and oxygen (O2)) (chlorine-based dry etching).

[0089] Specific examples of such materials include those containing platinum (Pt) and ruthenium (Ru). The light-absorbing film is preferably formed solely of materials containing platinum (Pt) and ruthenium (Ru). Specific examples of materials containing platinum (Pt) and ruthenium (Ru) include platinum-ruthenium (PtRu).

[0090] The light-absorbing film can be formed from a material containing only platinum (Pt) and ruthenium (Ru), or from a material containing other elements as well as platinum (Pt) and ruthenium (Ru). In this case, the total content of platinum (Pt) and ruthenium (Ru) in the light-absorbing film, as the overall average content in the film, is preferably 96 atomic% or more. Examples of elements other than platinum (Pt) and ruthenium (Ru) include metallic elements such as niobium (Nb), and light elements such as oxygen (O), nitrogen (N), carbon (C), and boron (B).

[0091] In the light-absorbing film, the platinum (Pt) content, as the overall average of the light-absorbing film, is 40 atomic% or more, preferably 42 atomic% or more, and 60 atomic% or less, preferably less than 60%, and more preferably 48 atomic% or less. Furthermore, in the light-absorbing film, the ruthenium (Ru) content, as the overall average of the light-absorbing film, is 40 atomic% or more, preferably greater than 40 atomic%, more preferably 52 atomic% or more, and 60 atomic% or less, preferably 58 atomic% or less. From the viewpoint of achieving a reflectivity of exposed light of a predetermined value or higher, particularly a reflectivity of exposed light of 3% or higher, the light-absorbing film preferably has an extinction coefficient k, as the overall average of the light-absorbing film, of 0.05 or less.

[0092] When manufacturing a reflective photomask from a reflective photomask preform, the light-absorbing film is exposed to sulfuric acid or alkali cleaning during the cleaning step. Furthermore, the reflective photomask is exposed to the atmosphere in the storage environment or the environment where the wafer exposure machine is used. Therefore, a higher platinum (Pt) content than a ruthenium (Ru) content, particularly the highest platinum (Pt) content on the side of the light-absorbing film furthest from the substrate, is advantageous from the viewpoint of cleaning resistance and oxidation resistance. In this invention, the platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is preferably 50 atomic% or more, more preferably greater than 50 atomic%, and even more preferably 52 atomic% or more, and preferably 90 atomic% or less, more preferably 70 atomic% or less, and even more preferably 60 atomic% or less.

[0093] Conversely, because the extinction coefficient k of platinum (Pt) is greater than that of ruthenium (Ru), if the platinum (Pt) content in the entire light-absorbing film is too high, the reflectivity to exposed light will decrease. Therefore, from the viewpoint of obtaining a reflectivity to exposed light of a predetermined value or higher, particularly a reflectivity of 3% or higher, it is effective to intermittently or continuously reduce the platinum (Pt) content along its thickness direction from the side of the light-absorbing film furthest from the substrate towards the substrate side in a portion or all of the light-absorbing film. In this case, the ruthenium (Ru) content can be kept constant along its thickness direction from the side of the light-absorbing film furthest from the substrate towards the substrate side in a portion or all of the light-absorbing film, but it is preferable that the content increases intermittently or continuously along its thickness direction in a portion or all of the light-absorbing film.

[0094] Examples of variations in platinum (Pt) content along the thickness direction of the light-absorbing film include:

[0095] The content of this content is constant from the side of the light-absorbing film furthest from the substrate towards the substrate side, and then decreases continuously towards the substrate side until it reaches the side closest to the substrate.

[0096] This content decreases continuously from the side of the light-absorbing film furthest from the substrate towards the midway towards the substrate side, and becomes a constant variation from, for example, the center of the light-absorbing film in the thickness direction, particularly the center, to the side closest to the substrate.

[0097] The content decreases continuously from the side of the light-absorbing film furthest from the substrate towards the substrate side, and once it becomes constant, it decreases continuously again towards the substrate side until it is closest to the substrate side.

[0098] The content of this content decreases continuously from the side of the light-absorbing film furthest from the substrate toward the substrate side until it is closest to the substrate side.

[0099] Examples of variations in ruthenium (Ru) content along the thickness direction of the light-absorbing film include:

[0100] The content of this content is constant from the side of the light-absorbing film furthest from the substrate towards the substrate side, and then increases continuously towards the substrate side until it reaches the side closest to the substrate.

[0101] The content increases continuously from the side of the light-absorbing film furthest from the substrate towards the midway towards the substrate side, and changes constantly from, for example, the center of the light-absorbing film in the thickness direction, particularly the center, to the side closest to the substrate.

[0102] This content increases continuously from the side of the light-absorbing film furthest from the substrate towards the substrate side, and once it becomes constant, it increases continuously again towards the substrate side until it is closest to the substrate side.

[0103] The content of this content increases continuously from the side of the light-absorbing film furthest from the substrate toward the substrate side until it is closest to the substrate side.

[0104] Note that if the light-absorbing film contains other elements besides platinum (Pt) and ruthenium (Ru), the content of these other elements along the thickness direction of the film, from the side furthest from the substrate toward the substrate side, may be constant or may increase or decrease intermittently or continuously.

[0105] In this invention, the content of platinum (Pt) on the side of the light-absorbing film closest to the substrate is preferably 40 atomic% or more, more preferably 42 atomic% or more, and preferably 50 atomic% or less, more preferably 48 atomic% or less. Furthermore, the content of ruthenium (Ru) on the side of the light-absorbing film closest to the substrate is preferably 50 atomic% or more, more preferably 52 atomic% or more, and preferably 60 atomic% or less, more preferably 58 atomic% or less.

[0106] In this invention, the content of platinum (Pt) at the center in the thickness direction of the light-absorbing film is preferably 40 atomic% or more, more preferably 42 atomic% or more, and preferably 56 atomic% or less, more preferably 50 atomic% or less, and even more preferably 48 atomic% or less. Furthermore, the content of ruthenium (Ru) at the center in the thickness direction of the light-absorbing film is preferably 44 atomic% or more, more preferably 50 atomic% or more, even more preferably 52 atomic% or more, and preferably 60 atomic% or less, more preferably 58 atomic% or less.

[0107] After the light-absorbing film of a reflective photomask preform is patterned, correction is performed if the pattern does not have the desired shape. For the correction of reflective photomasks, electron beam correction is primarily used because the fabrication accuracy of the photomask pattern is satisfactory. Fluorine-based gases, such as xenon fluoride (XeF2), are used for electron beam correction of light-absorbing films formed from materials containing platinum (Pt) and ruthenium (Ru). The pattern of the light-absorbing film can be corrected by dry etching of micro-regions using an electron beam-activated fluorine-based gas. The light-absorbing film is preferably formed from a material that can be corrected solely by dry etching using an electron beam-activated fluorine-based gas.

[0108] When correcting the pattern of the light-absorbing film, if the pattern of the light-absorbing film is completely etched, the etching reaches the protective film. However, in this case, if the protective film is also etched, the function of the protective film is impaired in the reflective photomask. Therefore, when the protective film and the light-absorbing film are etched under the same conditions by dry etching using an electron beam activated fluorine gas, the ratio (selectivity) of the etching rate of the light-absorbing film to the etching rate of the protective film is preferably 50 or more, more preferably 70 or more, and even more preferably 100 or more. When the ratio (selectivity) of the etching rates is 50 or more, the success rate of pattern correction of the light-absorbing film by dry etching using an electron beam activated fluorine gas is improved.

[0109] Furthermore, the light-absorbing film preferably has a structure that can be corrected solely by dry etching using an electron beam-activated fluorine-based gas. For example, when the light-absorbing film is a multilayer formed from two or more materials with different etching properties, two or more different types of etching are required when forming and correcting the pattern of the light-absorbing film. As a result, stepped portions are likely to appear in the cross-section of the pattern of the light-absorbing film. If the pattern of the light-absorbing film has stepped portions, the possibility of inaccuracy or error during pattern transfer increases. Therefore, such stepped patterns cannot cope with the miniaturization of patterns. In the cross-section of the pattern of the light-absorbing film, from the viewpoint of preventing the formation of stepped portions and from the viewpoint of obtaining a shape more perpendicular to the main surface of the substrate, the light-absorbing film is formed only from a material preferably containing platinum (Pt) and ruthenium (Ru), more preferably a material containing platinum (Pt) and ruthenium (Ru) with a total content of platinum (Pt) and ruthenium (Ru) of 96 atomic% or more, and even more preferably a material composed of platinum (Pt) and ruthenium (Ru).

[0110] In this invention, the light-absorbing film is a phase-shifting film. A phase-shifting light-absorbing film is a film that absorbs a portion of the exposure light and reflects the remainder of the exposure light by changing (shifting) its phase relative to the phase of the exposure light reflected from the multilayer reflective film. Thus, the phase-shifting function is obtained by the phase difference between the light reflected from the multilayer reflective film and the light reflected from the light-absorbing film.

[0111] The reflective photomask blank and reflective photomask of the present invention can be referred to as a reflective photomask blank with phase-shifting function (reflective phase-shifting photomask blank) and a reflective photomask with phase-shifting function (reflective phase-shifting photomask), respectively.

[0112] The light-absorbing film (phase-shifting film) with phase-shifting function has a reflectance of preferably 3% or more, more preferably 4% or more, and preferably 10% or less, more preferably 8% or less, to exposure light in the extreme ultraviolet region. This reflectance is the relative reflectance relative to the portion where the light-absorbing film is not formed, specifically the ratio between the reflectance of light reflected from the light-absorbing film formed on the substrate via the multilayer reflective film and the protective film, and the reflectance of light reflected from the multilayer reflective film and the protective film formed on the substrate.

[0113] The light-absorbing film (phase-shifting film) with phase-shifting function has a phase difference of preferably 200 degrees or more, more preferably 205 degrees or more, and preferably 230 degrees or less, more preferably 225 degrees or less, relative to the exposure light in the extreme ultraviolet region. This phase difference is the relative phase difference with respect to the portion where the light-absorbing film is not formed, specifically, the difference between the phase of the light reflected from the multilayer reflective film and protective film formed on the substrate and the phase of the light reflected from the light-absorbing film formed on the substrate via the multilayer reflective film and protective film.

[0114] From the viewpoint of ensuring light absorption and phase shift functions as well as reducing the impact of the shielding effect, the thickness of the light-absorbing film is preferably 35 nm or more, more preferably 36 nm or more, and preferably 40 nm or less, more preferably 38 nm or less.

[0115] In the manufacturing process of reflective photomasks, the light-absorbing film is exposed to cleaning with sulfuric acid or alkali. Furthermore, when using reflective photomasks or during pattern correction, the pattern of the light-absorbing film is exposed to cleaning with sulfuric acid or alkali. When the light-absorbing film of the present invention is contacted with an aqueous solution containing sulfuric acid, such as a sulfuric acid-hydrogen peroxide mixture (SPM), specifically, when cleaned with a sulfuric acid-hydrogen peroxide mixture (a mixed solution of sulfuric acid:hydrogen peroxide = 3:1 (volume ratio)) (100°C, 30 min), the change in the thickness of the light-absorbing film is preferably 0.5 nm or less, more preferably 0.3 nm or less. Furthermore, when the light-absorbing film of the present invention is contacted with an aqueous solution containing alkali, specifically, when cleaned with an aqueous alkali solution (ammonia, H2SO4 concentration: 6000 ppm) (80°C, 50 min), the change in the thickness of the light-absorbing film is preferably 0.5 nm or less, more preferably 0.3 nm or less.

[0116] A hard mask is a film that acts as an etching mask during the etching of an absorbing film. Hard masks are typically formed in contact with an absorbing film. Hard masks can consist of a single layer or multiple layers (e.g., 2 to 5 layers). Furthermore, hard masks can be films with a gradient composition.

[0117] When patterning an absorbing film using dry etching with fluorine-based gases, the hard mask preferably acts as an etching mask. The hard mask is preferably formed of a material resistant to dry etching using fluorine-based gases (SF6, CF4, etc.) (fluorine-based dry etching), such as dry etching using a mixture of SF6 and helium (He). Furthermore, the hard mask is preferably formed of a material capable of being etched using dry etching with chlorine-based gases (e.g., chlorine alone, or a mixture of chlorine (Cl2) and oxygen (O2)) (chlorine-based dry etching), particularly dry etching using a mixture of chlorine (Cl2) and oxygen (O2).

[0118] The material used to form the hard mask film is preferably a chromium (Cr)-containing material. The material used to form the hard mask film is preferably free of both platinum (Pt) and ruthenium (Ru). The material used to form the hard mask film may contain one or more light elements selected from oxygen (O), nitrogen (N), carbon (C), and boron (B). Specific examples of materials used for hard mask films include chromium oxide (CrO), chromium nitride (CrN), chromium oxynitride (CrON), chromium carbide (CrC), chromium oxycarbide (CrCO), chromium carbonitride (CrCN), and chromium oxynitride carbide (CrONC).

[0119] If the hard mask film is too thin, it may lose its function as an etching mask during the etching of the light-absorbing film, and may also reduce the defect inspection sensitivity of the hard mask film. Therefore, the thickness of the hard mask film is preferably 2 nm or more, more preferably 4 nm or more. Furthermore, when the hard mask film is removed by dry etching, the protective film is usually also exposed to the dry etching process. In this case, if the hard mask film is too thick, the amount of protective film loss increases. Therefore, the thickness of the hard mask film is preferably 14 nm or less, more preferably 10 nm or less.

[0120] The conductive film is preferably formed in contact with a substrate. The conductive film preferably has a sheet resistance of less than 100 Ω / square, and its material is not particularly limited. Examples of materials for the conductive film include those containing tantalum (Ta) or chromium (Cr). Furthermore, materials containing tantalum (Ta) or chromium (Cr) may contain one or more light elements selected from oxygen (O), nitrogen (N), carbon (C), and boron (B). The thickness of the conductive film is not particularly limited, as long as it acts as an electrostatic chuck, but is typically around 20 to 300 nm.

[0121] The resist film is preferably formed in contact with a light-absorbing film or a hard mask film. In this invention, the resist film can be an electron beam resist drawn by an electron beam or a photoresist drawn by light, but is preferably a chemically amplified resist. The chemically amplified resist can be a positive or negative resist. Examples of chemically amplified resists include resists containing a base resin such as a hydroxyl-styrene resin or a (meth)acrylic resin and an acid-generating agent, and, if necessary, a crosslinking agent, a quencher, and / or a surfactant.

[0122] The thickness of the resist film is preferably 150 nm or less. From the viewpoint that the resist pattern used to form fine auxiliary patterns is less likely to collapse due to the impact of the developing fluid or pure water during the rinsing process in the development step of forming the resist pattern, the thickness is preferably 100 nm or less. There is no lower limit to the thickness of the resist film, as long as the film thickness is sufficient to act as an etching mask during etching, that is, sufficient to leave a resist pattern on the entire surface of the film to be etched after etching. The thickness is not particularly limited, but is preferably 50 nm or more, more preferably 70 nm or more.

[0123] The formation of the multilayer reflective film, protective film, light-absorbing film, hard mask film, and conductive film of the present invention is not particularly limited, but since films with predetermined properties can be formed with good controllability, they are preferably formed by sputtering. Examples of applicable sputtering systems include, but are not limited to, DC sputtering and RF sputtering.

[0124] When a multilayer reflective film consisting of a molybdenum (Mo) layer and a silicon (Si) layer is formed, a molybdenum (Mo) target and a silicon (Si) target can be used as sputtering targets.

[0125] When the protective film is formed from a material containing rhodium (Rh), a rhodium (Rh) target can be used as a sputtering target.

[0126] When the light-absorbing film is formed from a material containing platinum (Pt) and ruthenium (Ru), platinum (Pt) targets and ruthenium (Ru) targets can be used as sputtering targets, and niobium (Nb) targets can be used if necessary.

[0127] When the hard mask film is formed of a material containing chromium (Cr), a chromium (Cr) target can be used as a sputtering target.

[0128] When the conductive film is formed from a material containing tantalum (Ta) or chromium (Cr), a tantalum (Ta) target or a chromium (Cr) target can be used as a sputtering target.

[0129] Depending on factors such as the size of the sputtering target, cooling efficiency, and controllability of the film formation, the electrical power supplied to the sputtering target can be appropriately set. Typically, the electrical power per unit area of ​​the sputtering surface of the target can be set from 50 to 3000 W / cm². 2 Furthermore, rare gases such as helium (He gas), neon (Ne gas), or argon (Ar gas) are used as sputtering gases. In cases where only the elements of the target material form the film (the layers constituting the film), only rare gases can be used as sputtering gases.

[0130] When the film (the layers constituting the film) is formed of a material containing one or more light elements selected from oxygen (O), nitrogen (N), and carbon (C), reactive sputtering is preferred as the sputtering method. Rare gases such as helium (He), neon (Ne), or argon (Ar) and reactive gases are used as the sputtering gases for reactive sputtering.

[0131] When a membrane (constituting the membrane layer) is formed from an oxygen-containing (O) material, oxygen gas (O2 gas) can be used as the reactive gas. When a membrane (constituting the membrane layer) is formed from a nitrogen-containing (N) material, nitrogen gas (N2 gas) can be used as the reactive gas. When a membrane (constituting the membrane layer) is formed from materials containing both nitrogen (N) and oxygen (O), the reactive gas can be suitably selected from oxygen gas (O2 gas), nitrogen gas (N2 gas), and nitrogen oxide gases such as nitric oxide gas (NO gas), nitrogen dioxide gas (NO2 gas), and nitrous oxide gas (N2O gas). When a membrane (constituting the membrane layer) is formed from a carbon-containing material, carbon-containing gases such as methane gas (CH4), carbon monoxide gas (CO gas), or carbon dioxide gas (CO2 gas) can be used as the reactive gas. For example, when a membrane (a layer constituting the membrane) is formed from a material containing nitrogen (N), oxygen (O) and carbon (C), oxygen (O2 gas), nitrogen (N2 gas) and carbon dioxide (CO2) gas can be used simultaneously as reactive gases.

[0132] Furthermore, when forming a film from a material containing boron (B), a target with added boron (B) can be used.

[0133] The pressure during membrane formation (of the membrane layers) can be appropriately set considering factors such as membrane stress, chemical resistance, and washability. The pressure is preferably 0.01 Pa or more, more preferably 0.03 Pa or more, and preferably 1 Pa or less, more preferably 0.3 Pa or less, to particularly improve chemical resistance. Furthermore, the gas flow rate can be appropriately set to provide the desired composition, typically from 0.1 to 100 sccm.

[0134] In the manufacturing process of a reflective photomask preform, before forming the resist film, the substrate, or the substrate and the film formed on the substrate, can be subjected to heat treatment. When performing heat treatment, it is preferable to apply the heat treatment while the surface of the light-absorbing film is not exposed. As a method for heat treatment, infrared heating or resistance heating can be used, for example, and the treatment conditions are not particularly limited. The heat treatment can be performed, for example, in a gas atmosphere containing oxygen (O). The concentration of the oxygen (O) gas is not particularly limited. In the case of oxygen (O2 gas), the gas content can be, for example, from 1 volume% to 100 volume%. The heat treatment temperature is preferably 200°C or higher, more preferably 400°C or higher.

[0135] Furthermore, during the fabrication of a reflective photomask preform, before forming the resist film, the film formed on the substrate, excluding the light-absorbing film, can be subjected to treatments such as ozone or plasma. There are no particular limitations on the treatment conditions. Any treatment can be applied to increase the oxygen concentration at the surface of the film. In this case, the treatment conditions can be appropriately controlled to obtain a predetermined oxygen concentration. It should be noted that when forming the film by sputtering, the oxygen concentration at the surface of the film can be increased by controlling the ratio of rare gases to oxygen-containing gases (oxidizing gases) such as oxygen (O2), carbon monoxide (CO), or carbon dioxide (CO2) in the sputtering gas.

[0136] Additionally, during the manufacturing process of reflective photomask preforms, a cleaning process can be performed before forming the resist film to remove defects present on the substrate or on the surface of the film formed on the substrate. Cleaning can be performed using one or both of ultrapure water and functional water, where the functional water contains, for example, ozone gas (O3 gas) or hydrogen gas (H2 gas). When applying the cleaning process to the light-absorbing film, it is preferable not to use functional water containing ozone gas (O3 gas). Furthermore, after cleaning with ultrapure water containing surfactants, additional cleaning can be performed using one or both of ultrapure water and functional water. If necessary, cleaning can be performed simultaneously with or in combination with UV light irradiation.

[0137] There are no particular restrictions on the methods used to form the resist film (coating the resist), and known methods such as spin coating can be applied.

[0138] The reflective photomask blank of the present invention can be used to manufacture a reflective photomask having a pattern of a substrate, a multilayer reflective film, a protective film and a light-absorbing film.

[0139] In the fabrication of reflective photomasks, when no resist film is formed on the reflective photomask blank, a resist film is formed by contacting the side of the reflective photomask blank that is furthest from the substrate, such as the light-absorbing film or hard mask film furthest from the substrate.

[0140] Then, using a resist pattern obtained by patterning a resist film or a film pattern obtained by patterning a film such as a hard mask film as an etching mask, a dry etching method appropriately selected from, for example, chlorine-based dry etching and fluorine-based dry etching, is applied to pattern or remove the film according to the etching characteristics of the material used to form the respective films. In this way, reflective photomasks can be fabricated. In the fabrication of reflective photomasks, the resist pattern can be removed using a sulfuric acid-hydrogen peroxide mixture (SPM).

[0141] Next, with reference to the accompanying drawings, an example of a method for manufacturing a reflective photomask from the reflective photomask blank of the present invention will be specifically described. Figure 6Includes a cross-sectional view for explaining the steps of manufacturing a reflective photomask according to the second aspect of the invention from a reflective photomask blank according to the second aspect of the invention.

[0142] First, such as Figure 6 As shown in (A), a resist film 7 is formed by contacting the side of the hard mask film 5 furthest from the substrate of the reflective photomask blank 102 (step (A)).

[0143] Subsequently, as Figure 6 As shown in (B), the resist film 7 is patterned to form a resist pattern 7a (step (B)).

[0144] Subsequently, as Figure 6 As shown in (C), the hard mask film 5 is patterned by using a resist pattern 7a as an etching mask and dry etching with chlorine gas to form the pattern 5a of the hard mask film (step (C)).

[0145] Subsequently, as Figure 6 As shown in (D), remove the resist pattern 7a (step (D)).

[0146] Subsequently, as Figure 6 As shown in (E), the pattern 5a of the hard mask film is used as an etching mask, and the light-absorbing film 4 is patterned by dry etching with fluorine gas to form the pattern 4a of the light-absorbing film (step (E)).

[0147] Next, as Figure 6 As shown in (F), the pattern 5a of the hard mask film is removed by dry etching with chlorine gas (step (F)) to obtain a reflective photomask 202.

[0148] Example

[0149] The present invention is described in detail below with reference to embodiments and comparative examples, but the present invention is not limited to the following embodiments.

[0150] Examples 1 to 13, Comparative Examples 1 to 3

[0151] like Figure 2 As shown, multiple layers of reflective film, protective film, light-absorbing film and hard mask film are sequentially stacked on one of the main surfaces of a quartz substrate with a square diameter of 152 mm and a thickness of about 6 mm, and a conductive film is formed on the other main surface of the quartz substrate to manufacture a reflective photomask preform (a reflective photomask preform of the second type).

[0152] First, using molybdenum (Mo) and silicon (Si) targets, and argon (Ar) gas as the sputtering gas, sputtering from the molybdenum (Mo) target and sputtering from the silicon (Si) target are performed alternately by controlling the electrical power applied to the targets and the flow rate of the sputtering gas to form a multilayer reflective film (thickness: 280 nm) of alternating molybdenum (Mo) and silicon (Si) layers on a quartz substrate (one of the main surfaces), i.e., a multilayer reflective film (reflectivity of 65% for light at a wavelength of 13.5 nm). The cycle consisting of stacked molybdenum (Mo) and silicon (Si) layers is repeated for 40 cycles (40 molybdenum (Mo) layers and 40 silicon (Si) layers).

[0153] Subsequently, a rhodium (Rh) target was used as the target and argon (Ar gas) was used as the sputtering gas. Sputtering was performed by controlling the electrical power to be applied to the target and controlling the flow rate of the sputtering gas to form a protective film on the multilayer reflective film, namely, a film formed of elemental rhodium (thickness: 2nm).

[0154] Subsequently, a tantalum (Ta) target was used as the target and argon (Ar gas) and nitrogen (N2 gas) were used as sputtering gases. Sputtering was performed by controlling the electrical power to be applied to the target and controlling the flow rate of the sputtering gases to form a conductive film on a quartz substrate (another main surface), namely, a film formed of tantalum nitride (TaN) (thickness: 70 nm).

[0155] Subsequently, using platinum (Pt) and ruthenium (Ru) targets as targets and argon (Ar gas) as sputtering gas, sputtering was performed by controlling the electrical power applied to the targets and controlling the flow rate of the sputtering gas to form a light-absorbing film with phase-shifting function on the protective film, namely, a film formed of platinum and ruthenium (PtRu).

[0156] By varying the power applied to each target over time, the light-absorbing film exhibits:

[0157] The composition changes, wherein from the side of the light-absorbing film furthest from the substrate towards the substrate side, along the thickness direction of the light-absorbing film, the platinum (Pt) content continuously decreases and the ruthenium (Ru) content continuously increases, and from the center of the thickness direction of the light-absorbing film to the side closest to the substrate, the platinum (Pt) content and the ruthenium (Ru) content become constant, or

[0158] The composition changes, wherein from the side of the light-absorbing film furthest from the substrate to the side closest to the substrate, along the thickness direction of the light-absorbing film, the platinum (Pt) content continuously decreases and the ruthenium (Ru) content continuously increases.

[0159] Subsequently, using a chromium (Cr) target and argon (Ar), oxygen (O2), nitrogen (N2), and carbon dioxide (CO2) gases as sputtering gases, sputtering was performed by controlling the electrical power applied to the target and the flow rate of the sputtering gases to form a hard mask film on the light-absorbing film. Specifically, a film formed of chromium oxynitride carbide (CrONC) (thickness: 10 nm, chromium (Cr) content: 38 atomic%, oxygen (O) content: 34 atomic%, nitrogen (N) content: 18 atomic%, and carbon (C) content: 10 atomic%) was obtained in this manner. A reflective photomask preform was thus obtained.

[0160] Compare Examples 4 and 5

[0161] The reflective photomask blank was obtained in the same manner as in Example 1, except that in the formation of the phase-shifting light-absorbing film, the electrical power to be applied to each target was kept constant over time to form the phase-shifting light-absorbing film. In the composition of the light-absorbing film, the contents of platinum (Pt) and ruthenium (Ru) along the thickness direction of the light-absorbing film from the side furthest from the substrate to the side closest to the substrate are constant, that is, there is no change in composition.

[0162] Comparative Example 6

[0163] The reflective photomask preform was obtained in the same manner as in Example 1, except that in the formation of the protective film, a ruthenium (Ru) target and a niobium (Nb) target were used as targets, and argon gas (Ar gas) was used as sputtering gas. Sputtering was performed by controlling the electrical power to be applied to the target and controlling the flow rate of the sputtering gas to form a protective film on the multilayer reflective film, that is, a film formed of ruthenium and niobium (RuNb) (thickness: 2nm).

[0164] For each reflective photomask preform, the composition (average value of the entire film, the side furthest from the substrate (top), the center in the thickness direction (center), and the side closest to the substrate (bottom)) and thickness of the absorbing film, as well as the reflectivity (relative reflectivity to the multilayer reflective film and the protective film) and phase difference (relative phase difference to the multilayer reflective film and the protective film) for light with a wavelength of 13.5 nm are shown in Table 1. Note that the composition of the absorbing film was measured using X-ray photoelectron spectroscopy. Furthermore, the thickness of the absorbing film was measured using an X-ray diffractometer via X-ray reflectance (the same applies to the film thickness measurements below). As for reflectivity, the reflectivity for light with an incident angle of 6 degrees was measured using a reflectometer. Additionally, the refractive index n and extinction coefficient k were measured using a refractive index / extinction coefficient measuring device, and the phase difference was calculated from these measured values.

[0165] Table 1

[0166]

[0167] Next, using the obtained reflective photomask preform, fabrication is carried out on... Figure 5 The reflective photomask shown is a second type of reflective photomask.

[0168] First, a positive chemical amplification electron beam resist is spin-coated onto a hard mask to form a resist film with a thickness of 150 nm (step (A)).

[0169] Subsequently, an electron beam mapping device was used at 100 µC / cm. 2 The dose was used to create a line-space pattern (long side dimension 1000 nm, number of line patterns: 100,000). The width of the line pattern and the spacing pattern were each 100 nm. Subsequently, a heat treatment was performed at 110 °C for 14 minutes using a heat treatment apparatus (PEB: post-exposure baking). Then, a development process was performed by immersion development for 40 seconds to form the resist pattern (step (B)).

[0170] Subsequently, using the obtained resist pattern as an etching mask, the hard mask film is dry etched under the following conditions using a chlorine-based gas to form the pattern of the hard mask film (step (C)).

[0171] <Conditions for dry etching using chlorine-based gases>

[0172] Equipment: ICP (Inductively Coupled Plasma) system

[0173] Etching gases: Cl2 and O2

[0174] Gas pressure: 3.0 mTorr (0.40 Pa)

[0175] ICP power: 350 W

[0176] Subsequently, the residual resist pattern is removed by washing with a sulfuric acid-hydrogen peroxide mixture (a mixture of sulfuric acid and hydrogen peroxide solution (sulfuric acid: hydrogen peroxide solution = 3:1 (volume ratio))) (step (D)).

[0177] Subsequently, using the pattern of the obtained hard mask film as an etching mask, dry etching with fluorine-based gas is applied under the following conditions to form the pattern of the light-absorbing film (step (E)).

[0178] <Conditions for dry etching using fluorine-based gases>

[0179] Equipment: ICP (Inductively Coupled Plasma) system

[0180] Gas: SF6 gas + He gas

[0181] Gas pressure: 4.0 mTorr (0.53 Pa)

[0182] ICP power: 400 W

[0183] Subsequently, under the above conditions, the pattern of the hard mask film is dry etched using chlorine gas (step (F)) and the pattern of the hard mask film is removed to obtain a reflective photomask.

[0184] For each of the obtained reflective photomasks, the thickness of the pattern of the light-absorbing film was measured to obtain the difference between the thickness of the light-absorbing film and that of the reflective photomask blank (the reduction before and after manufacturing). The results are shown in Table 2.

[0185] Subsequently, the cleaning of the reflective photomask with a sulfuric acid-hydrogen peroxide mixture (a mixed solution of sulfuric acid and hydrogen peroxide in a volume ratio of 3:1) was repeated 5 times (100°C, 6 minutes). The thickness of the pattern of the light-absorbing film was measured to obtain the difference (reduction) before and after cleaning with the sulfuric acid-hydrogen peroxide mixture. The results are shown in Table 2.

[0186] Subsequently, the reflective photomask was cleaned five times with an alkaline aqueous solution (ammonia, H2SO4 concentration: 6000ppm) (80℃, 10min). The thickness of the light-absorbing film pattern was measured to obtain the difference (reduction) before and after cleaning with the alkaline aqueous solution. The results are shown in Table 2.

[0187] Furthermore, using each of the obtained reflective photomasks, the dry etching process using electron beam-activated fluorine gas, employed in correcting the pattern of the light-absorbing film of the reflective photomask, was applied to each of the light-absorbing film pattern and the protective film under the following conditions, and the etching amount (thickness) and etching time were measured. The etching rate was calculated from these, and the ratio of the etching rate of the light-absorbing film to the etching rate of the protective film was calculated as a selectivity. The results are shown in Table 2.

[0188] <Conditions for dry etching using electron beam-activated fluorine gases>

[0189] Apparatus: Electron beam correction device (MeRiT, manufactured by Carl Zeiss)

[0190] Gas: XeF2 gas

[0191] Table 2

[0192]

[0193] It should be noted that the present invention is not limited to the embodiments described above. The embodiments described above are examples, and any content having the same or substantially the same structure as the technical concept of the present invention, performing the same or similar functions and effects, is included within the technical scope of the present invention.

Claims

1. A reflective photomask preform, comprising a substrate, a multilayer reflective film formed on the substrate and reflecting exposure light as extreme ultraviolet (EUV) light, a protective film formed on the multilayer reflective film for protecting the multilayer reflective film, and a light-absorbing film formed on the protective film in contact with the protective film, which absorbs exposure light and has a phase-shifting function, wherein, The light-absorbing film has a thickness of 35 nm or more and 40 nm or less. The light-absorbing film is formed of a material containing platinum (Pt) and ruthenium (Ru). As the overall average value in the light-absorbing film, the content of platinum (Pt) is 40 atomic% or more and less than 60%, the content of ruthenium (Ru) is greater than 40 atomic% and less than 60 atomic%, and the total content of platinum (Pt) and ruthenium (Ru) is 96 atomic% or more. The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is greater than 50 atomic% and less than 90 atomic%. In a portion or all of the light-absorbing film, along the thickness direction of the film, from the side of the film furthest from the substrate toward the substrate side, the platinum (Pt) content decreases intermittently or continuously, and The light-absorbing film has a reflectivity of 3% or more and 10% or less for the exposed light and a phase difference of 200 degrees or more and 230 degrees or less for the exposed light.

2. The reflective photomask preform according to claim 1, wherein, The platinum (Pt) content on the side of the light-absorbing film closest to the substrate is 40 atomic% or more and 50 atomic% or less.

3. The reflective photomask blank according to claim 1 or 2, wherein, The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is 52 atomic% or more.

4. The reflective photomask blank according to claim 1 or 2, wherein, When the protective film and the light-absorbing film are etched under the same conditions by dry etching using an electron beam-activated fluorine gas, the ratio of the etching rate of the light-absorbing film to the etching rate of the protective film is 50 or more.

5. The reflective photomask blank according to claim 1 or 2, wherein, The protective film is formed from a material containing rhodium (Rh).

6. The reflective photomask preform according to claim 1 or 2, further comprising a hard mask film formed on the light-absorbing film in contact with the light-absorbing film.

7. The reflective photomask preform according to claim 6, wherein, The hard mask is formed of a material that is resistant to fluorine-based dry etching and can be etched by chlorine-based dry etching.

8. The reflective photomask blank according to claim 7, wherein, The hard mask film is formed of a chromium (Cr)-containing material and has a thickness of more than 2 nm and less than 14 nm.

9. A reflective photomask, comprising a substrate, a multilayer reflective film formed on the substrate and reflecting exposure light as extreme ultraviolet (EUV) light, a protective film formed on the multilayer reflective film for protecting the multilayer reflective film, and a pattern of a light-absorbing film formed on the protective film in contact with the protective film, which absorbs exposure light and has a phase-shifting function, wherein... The light-absorbing film has a thickness of 35 nm or more and 40 nm or less. The light-absorbing film is formed of a material containing platinum (Pt) and ruthenium (Ru). As the overall average value in the light-absorbing film, the content of platinum (Pt) is greater than 40 atomic% and less than 60%, the content of ruthenium (Ru) is greater than 40 atomic% and less than 60 atomic%, and the total content of platinum (Pt) and ruthenium (Ru) is greater than 96 atomic%. The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is greater than 50 atomic% and less than 90 atomic%. In part or all of the light-absorbing film, along the thickness direction of the film, from the side of the film furthest from the substrate toward the substrate side, the content of platinum (Pt) decreases intermittently or continuously. The light-absorbing film has a reflectivity of 3% or more and 10% or less for the exposed light and a phase difference of 200 degrees or more and 230 degrees or less for the exposed light.

10. The reflective photomask according to claim 9, wherein the platinum (Pt) content on the side of the light-absorbing film closest to the substrate is 40 atomic% or more and 50 atomic% or less.

11. The reflective photomask according to claim 9 or 10, wherein, The platinum (Pt) content on the side of the light-absorbing film furthest from the substrate is 52 atomic% or more.

12. The reflective photomask according to claim 9 or 10, wherein, When a protective film and a light-absorbing film are etched under the same conditions using dry etching with an electron beam activated fluorine gas, the ratio of the etching rate of the light-absorbing film to the etching rate of the protective film is 50 or more.

13. The reflective photomask according to claim 9 or 10, wherein, The protective film is formed from a material containing rhodium (Rh).

14. A method for manufacturing a reflective photomask comprising a pattern of a light-absorbing film from a reflective photomask preform according to any one of claims 6 to 8, the method comprising the steps of: (A) Forming a resist film that contacts the side of the hard mask film furthest from the substrate. (B) Patterning the resist film to form a resist pattern. (C) Using a resist pattern as an etching mask, a hard mask film is patterned by dry etching with chlorine-based gases to form the pattern of the hard mask film. (D) Remove the resist pattern. (E) Using the pattern of the hard mask film as an etching mask, the light-absorbing film is patterned by dry etching with fluorine-based gases to form the pattern of the light-absorbing film, and (F) The pattern of the hard mask film is removed by dry etching using chlorine-based gases.

Citation Information

Patent Citations

  • Reflective mask blank and reflective mask, and manufacturing methods for reflective mask and semiconductor device

    JP2024142177A