A shielding layer structure and braiding process for high-voltage cables in new energy vehicles
By employing a double-layer reverse braided structure and a low-temperature conductive hot melt adhesive penetration and curing method, the problems of increased porosity of the braided layer and insulation layer damage caused by welding fixation under dynamic bending of high-voltage cables for new energy vehicles have been solved, thereby improving electromagnetic shielding effectiveness and stability.
Patent Information
- Application Number
- CN202611470429.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-21
- Publication Date
- 2026-11-17
AI Technical Summary
The porosity of the braided layer of high-voltage cables for new energy vehicles increases under dynamic bending, and the welding and fixing of the drain wire can cause thermal damage to the insulation layer and fatigue fracture of the solder joint.
The shielding layer adopts a double-layer reverse braided structure with an angle difference of ≥10° between the inner and outer braids. Combined with low-temperature conductive hot melt adhesive penetration and curing, it forms a deep mechanical interlock, replacing the traditional welding fixation.
Maintaining the overall porosity of the shielding layer avoids thermal damage to the insulation layer, reduces the risk of fatigue fracture of the drain wire, and maintains the electromagnetic shielding effectiveness and stability.
Smart Images

Figure CN123120406A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of wire and cable manufacturing technology, and in particular to a shielding layer structure and braiding process for high-voltage cables for new energy vehicles. Background Technology
[0002] High-voltage cables for new energy vehicles generate strong electromagnetic interference during operation. Therefore, a metal braided shielding layer needs to be installed on the outside of the insulation layer to limit electromagnetic radiation, and a drain line needs to be configured to ensure reliable grounding of the shielding layer.
[0003] Existing metal braided shielding layers mostly adopt a single-layer or double-layer braided structure at the same angle. During actual vehicle operation, high-voltage cables are under dynamic bending and vibration conditions for a long time. When subjected to repeated stress, the metal wires of the conventional braided structure will slip relative to each other, causing the braided mesh to gradually enlarge and the structure to loosen. This increase in porosity will cause the overall braiding density of the shielding layer to decrease, affecting the shielding effect of electromagnetic waves and making it difficult to meet the electromagnetic compatibility requirements of the vehicle system.
[0004] Regarding the connection and forming of the drain wire, the industry currently uses metal spot welding or ultrasonic welding to directly fix the drain wire to the metal shielding mesh. The local high temperature generated by the welding process can penetrate the braided mesh and be conducted to the inner insulation layer, causing thermal damage or slight melting of the insulation material, which poses an electrical safety hazard. In addition, the welding fixing method will form a rigid connection point between the drain wire and the shielding layer. When the cable undergoes long-term mechanical deformation and alternating hot and cold cycles with the vehicle body, stress concentration will occur at the connection point, resulting in metal fatigue fracture. This will lead to a reduction in the contact area between the drain wire and the shielding layer and an increase in contact resistance, thereby affecting the stability of shielding and draining. Summary of the Invention
[0005] The purpose of this invention is to provide a shielding layer structure and braiding process for high-voltage cables for new energy vehicles, which solves the problems that the porosity of the braided layer of high-voltage cables for new energy vehicles will increase under dynamic bending, and that the welding and fixing of the lead wire will cause thermal damage to the insulation layer and fatigue fracture of the solder joint.
[0006] To achieve the above objectives, the present invention provides the following technical solution:
[0007] In a first aspect, the present invention provides a shielding layer structure for high-voltage cables in new energy vehicles, employing the following technical solution:
[0008] A shielding layer structure for a high-voltage cable of a new energy vehicle, comprising, from the inside out: an inner semiconductive layer disposed on the outer surface of an insulating layer, used to uniform the electric field and prevent partial discharge; and a braided shielding layer disposed on the outer surface of the inner semiconductive layer. The braided shielding layer adopts a double-layer reverse braiding structure, including an inner braided layer braided in a clockwise direction and an outer braided layer braided in a counterclockwise direction. The braiding angle of the inner braided layer relative to the cable axis is a first braiding angle, and the braiding angle of the outer braided layer relative to the cable axis is a second braiding angle. The absolute value of the difference between the first braiding angle and the second braiding angle is ≥10°, which is used to maintain the braided porosity without a sharp increase and keep the total braiding density ≥85% during dynamic bending of the cable through a double-layer differential angle misalignment complementary mechanism.
[0009] An outer semiconductive layer is disposed on the outer surface of the braided shielding layer to fill the pores of the braided shielding layer and improve shielding efficiency. A guide wire is disposed between the braided shielding layer and the outer semiconductive layer along the cable axis. The guide wire includes a guide wire baseline and a low-temperature conductive hot melt adhesive covering the outer surface of the guide wire baseline. The low-temperature conductive hot melt adhesive is forcibly penetrated into the interlacing gaps of the outer braided layer by in-situ melting and curing to form a deep mechanical interlock between the guide wire and the braided shielding layer, maintaining low contact resistance and high thermal cycling stability. The low-temperature conductive hot melt adhesive is made of the following components in parts by weight: 40 to 60 parts of copolyamide hot melt resin, 10 to 15 parts of rosin pentaerythritol ester, 150 to 200 parts of flake silver powder, and 10 to 20 parts of multi-walled carbon nanotubes.
[0010] This invention, through the combination of physical and mechanical structural design and interface conductive connection, mainly functions in the following aspects:
[0011] Under dynamic bending stress, due to the difference in weaving angle between the inner and outer braided layers being greater than or equal to 10°, the sliding displacement of the two braided layers exhibits asymmetrical characteristics when sliding occurs under axial and radial forces. During the stretching and pore expansion process of the outer braided mesh, the displacement of the braided wires can effectively fill the pores of the inner braided mesh that have expanded due to torsion. The physical misalignment and superposition of the two mesh layers can, to a certain extent, block the straight-line penetration path of electromagnetic waves and maintain the stability of the total weaving density.
[0012] In the extrusion process, the copolyamide hot melt resin matrix is liquefied by utilizing the ambient heat and melt pressure of the extruder head. The liquid conductive adhesive overcomes the surface tension of the fluid and penetrates microscopically in three dimensions along the cylindrical surface of the outer braided filaments, filling the gaps in the mesh. Subsequent cooling causes the hot melt adhesive to undergo a phase change and solidify, establishing a deep mechanical interlock between the lead wire and the outer braided layer, replacing the traditional rigid welding points, thereby avoiding localized heat concentration damage caused by welding.
[0013] In terms of conductive structure molding, the large aspect ratio sheet-like silver powder inside the copolyamide matrix constructs a two-dimensional conductive framework through surface contact. Multi-walled carbon nanotubes, with their aspect ratio advantage, interweave and overlap between the distant silver powder sheets to form a one-dimensional conductive bridge. The combination of the two forms a three-dimensional conductive network, which helps to reduce the resistivity of the cured hot melt adhesive layer and ensures low contact resistance between the lead wire and the braided layer.
[0014] Preferably, the low-temperature conductive hot melt adhesive further contains a silane coupling agent, wherein the silane coupling agent is γ-aminopropyltriethoxysilane, and the amount is 1.0 to 2.0 parts; the flake silver powder and multi-walled carbon nanotubes in the low-temperature conductive hot melt adhesive are pretreated as follows: the flake silver powder and multi-walled carbon nanotubes are added to anhydrous ethanol, the silane coupling agent is added dropwise, and after ultrasonic dispersion, filtration and vacuum drying, a modified composite conductive filler is obtained, which is then mixed with copolyamide hot melt resin and rosin pentaerythritol ester.
[0015] Surface chemical reactions are used to improve the interfacial compatibility between inorganic conductive fillers and organic polymer matrices.
[0016] Specifically, the three ethoxy groups at the ends of the γ-aminopropyltriethoxysilane molecule undergo hydrolysis in anhydrous ethanol and trace moisture environments to generate an active intermediate containing three silanol groups. The active silanol groups undergo dehydration condensation reactions with the hydroxyl groups at the defects on the surface of multi-walled carbon nanotubes and the hydroxyl groups in the metal oxide layer on the surface of flake silver powder, forming covalent bonds. Amino functional groups are grafted onto the surface of the composite conductive filler. During the subsequent hot melt mixing and curing process, the amino functional groups grafted onto the filler surface generate hydrogen bond intermolecular forces with the amide bonds in the copolyamide hot melt resin matrix. This largely avoids secondary physical agglomeration of silver powder and carbon nanotubes in the polymer melt and helps maintain a uniform distribution of the conductive phase during the extrusion rheological process.
[0017] Preferably, the outer semiconductive layer is made of raw materials comprising the following parts by weight: 54 to 90 parts of ethylene-vinyl acetate copolymer; 20 to 30 parts of polyolefin elastomer; 0.5 to 1.5 parts of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate); 1.0 to 3.0 parts of zinc stearate; 30 to 50 parts of acetylene black; and 1.0 to 2.5 parts of dicumyl peroxide.
[0018] The blend system of ethylene-vinyl acetate copolymer and polyolefin elastomer can be used as a base material to give the cable surface the corresponding mechanical flexibility. Acetylene black, as a conductive medium, is distributed in the matrix to provide semi-conductive properties. Combined with dicumyl peroxide, it initiates the cross-linking reaction of polymer macromolecular chains to improve the overall temperature resistance. At the same time, the introduction of zinc stearate as a lubricant helps to reduce extrusion friction resistance.
[0019] Preferably, the baseline of the drainage line has a cross-sectional area of 0.5 to 1.5 mm². 2 The low-temperature conductive hot melt adhesive contains multi-strand stranded tin-plated copper wire; the average radial dimension D50 of the flake silver powder is 2.0 to 3.0 μm, and the thickness is 0.1 to 0.3 μm; the outer diameter of the multi-walled carbon nanotube is 10 to 20 nm, and the length is 10 to 20 μm; the weight-average molecular weight of the copolyamide hot melt resin is 20,000 to 30,000, and the ring and ball softening point is 110°C to 130°C.
[0020] By rationally setting the spatial size parameters of the conductive filler, it is beneficial for carbon nanotubes with an outer diameter of 10 to 20 nm to be filled into the gaps between stacked sheet-like silver powders of 2.0 to 3.0 μm. The copolyamide hot melt resin is set with a softening point of 110°C to 130°C, so that it has basic structural stability under the normal operating temperature of the cable, and can quickly enter the viscous flow state under the heating conditions of extrusion processing to meet the processing requirements.
[0021] Preferably, the first weaving angle is 40° to 50°, the second weaving angle is 25° to 35°, and the absolute value of the difference between the first weaving angle and the second weaving angle is 15°; the weaving density of the inner weaving layer is 40% to 50%, and the weaving density of the outer weaving layer is 40% to 50%.
[0022] The first braiding angle is set at 40° to 50° primarily to provide radial compressive strength, while the second braiding angle is set at 25° to 35° to provide axial tensile strength to the cable. The set absolute difference of 15° is beneficial for the formation of a relatively stable staggered distribution of the inner and outer mesh layers.
[0023] Secondly, the present invention provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, comprising the following steps:
[0024] S1. Provide a cable core with an internal conductor and an insulation layer and an inner semi-conductive layer.
[0025] S2. Feed the cable core into the first braiding machine and perform the first braiding on the surface of the inner semiconductive layer to form an inner braided mesh, and control the braiding angle relative to the cable axis to the first braiding angle.
[0026] S3. The wire core is continuously fed into the second braiding machine, and a second reverse braiding is performed on the surface of the inner braided mesh to form the outer braided mesh. The braiding angle relative to the cable axis is controlled to be the second braiding angle, and the absolute value of the difference between the first braiding angle and the second braiding angle is controlled to be ≥10°.
[0027] S4. Monitor the light transmittance of the two-layer woven mesh in real time and perform closed-loop adjustment to ensure that the total woven density after the double-layer staggered superposition is constant at ≥85%;
[0028] S5. After the outer layer is woven, the pre-coated lead wire with the surface covered with low-temperature conductive hot melt adhesive is attached straight along the cable axis to the outer surface of the outer layer woven mesh.
[0029] S6. The wire harness is fed into the extruder as a whole. An extrusion mold is used to extrude the semi-conductive polymer material for preparing the outer semi-conductive layer onto the outside of the outer braided mesh and the pre-coated lead wire. The ambient heat provided by the die head during the extrusion process causes the low-temperature conductive hot melt adhesive on the surface of the pre-coated lead wire to liquefy instantly. The melt pressure in the extrusion mold drives the liquefied conductive hot melt adhesive to forcefully penetrate into the interlacing gaps of the outer braided mesh.
[0030] S7. Cool the extruded composite cable to cure the conductive hot melt adhesive and the outer semiconductive layer, and complete the physical interlocking bonding of the outer braided mesh of the lead wire and the braided shielding layer with the outer semiconductive layer.
[0031] By utilizing the heat carried by the polymer melt during extrusion at the extruder head, the hot melt adhesive on the surface of the pre-coated lead wire is liquefied and penetrated under the pressure inside the extrusion die. The sheath forming and lead wire fixing are completed in one extrusion process, eliminating the need for a separate lead wire welding process. This can largely avoid the risk of thermal stress damaging the insulation layer and improve process continuity.
[0032] Preferably, after the outer layer is braided, the step of attaching pre-coated lead wires, with their surfaces covered in low-temperature conductive hot melt adhesive, straight along the cable axis to the outer surface of the outer braided mesh includes: attaching lead wires with a cross-sectional area of 0.5 to 1.5 mm² to the outer surface of the outer braided mesh. 2 Multi-strand stranded tinned copper wire is used as the baseline of the lead wire and is inserted into the wire extrusion molding machine. At an extrusion temperature of 140°C to 150°C, the molten low-temperature conductive hot melt adhesive is uniformly coated on the outer surface of the lead wire baseline with a radial thickness of 0.1 mm to 0.3 mm. After cooling, the pre-coated lead wire is collected and then attached to the outer surface of the outer braided mesh in a straight line along the cable axis.
[0033] Pre-coating the guide wire baseline surface with hot melt adhesive at a radial thickness of 0.1mm to 0.3mm provides a relatively suitable hot melt adhesive volume, avoiding poor contact due to insufficient adhesive seeping into the mesh gaps, or local abrupt changes in outer diameter due to excessive adhesive, which helps maintain the flatness of the extruded outer surface.
[0034] Preferably, the wire harness is fed into an extruder as a whole, and an extrusion die is used to extrude the semi-conductive polymer material for preparing the outer semi-conductive layer onto the outer braided mesh and the pre-coated lead wire. The ambient heat provided by the extruder head during the extrusion process causes the low-temperature conductive hot melt adhesive on the surface of the pre-coated lead wire to liquefy instantaneously, and the melt pressure in the extrusion die drives the liquefied conductive hot melt adhesive to forcefully penetrate into the interlacing gaps of the outer braided mesh. The steps include: setting the extruder head temperature to 150°C to 180°C, establishing and maintaining a continuous melt pressure of 15MPa to 25MPa inside the extrusion die; and the extrusion temperature of the semi-conductive polymer material is higher than the softening point of the low-temperature conductive hot melt adhesive.
[0035] The set temperature of 150℃ to 180℃ provides the melting heat for the hot melt adhesive, and the continuous melt pressure of 15MPa to 25MPa drives the liquid conductive adhesive to flow, which can overcome the surface friction resistance of the metal braided wire to a certain extent, and promote the conductive filler and resin to be squeezed into the mesh pores for filling.
[0036] Preferably, the steps of feeding the cable core into a first braiding machine to perform a first braid on the surface of the inner semiconductive layer to form an inner braided mesh, and controlling the braiding angle relative to the cable axis to be a first braiding angle, and feeding the core continuously into a second braiding machine to perform a second reverse braid on the surface of the inner braided mesh to form an outer braided mesh, controlling the braiding angle relative to the cable axis to be a second braiding angle, and controlling the absolute value of the difference between the first braiding angle and the second braiding angle to be ≥10°, both include:
[0037] The steps for maintaining a constant single-spindle wire tension between 5N and 10N, and for real-time monitoring of the light transmittance of the two-layer woven mesh and performing closed-loop adjustment to ensure that the total woven density after the double-layer misaligned superposition is constant at ≥85%, include: real-time monitoring of the light transmittance of the two-layer mesh after misaligned superposition using an online visual inspection instrument, and closed-loop adjustment of the traction speed and spindle tension to change the rotational speed ratio between the traction wheel and the spindle disc, so that the macroscopic light transmittance after the physical misalignment of the double-layer woven mesh remains below 15%.
[0038] The visual inspection instrument characterizes the superposition state of two mesh layers by light transmittance. When the light transmittance parameter exceeds the set threshold, the number of braided intersections within a unit axial length of the cable is changed by adjusting the rotational speed ratio between the traction wheel and the spindle disc, thereby achieving active compensation adjustment of porosity.
[0039] Preferably, the step of cooling the extruded composite cable to solidify the conductive hot melt adhesive and the outer semiconductive layer, and completing the physical interlocking bonding of the lead wire, the outer braided mesh of the braided shielding layer and the outer semiconductive layer, includes: immediately immersing the extruded composite cable in a circulating water tank with a water temperature of 20°C to 40°C for rapid cooling.
[0040] Rapid water cooling causes the rearrangement of polymer macromolecular chains to stop, and the hot melt adhesive gradually changes from a liquid state to a solid state as it cools, which can better maintain its permeation state within the woven mesh and complete the fixation.
[0041] In summary, the present invention has at least one of the following beneficial technical effects:
[0042] 1. This invention employs a double-layer reverse braiding structure and controls the absolute value of the difference between the inner and outer braiding angles to be ≥10°. When the cable undergoes dynamic bending or torsion, the braided strands of the inner and outer layers will generate asymmetrical displacement during the force-induced slippage process. This causes the stretched and enlarged mesh to physically misalign and overlap with the braided strands of the other layer. This helps maintain the overall porosity of the shielding layer under external stress, keeping the total braiding density above 85%, thereby ensuring the electromagnetic shielding effectiveness of the high-voltage cable under long-term dynamic operating conditions.
[0043] 2. This invention coats the baseline surface of the lead wire with low-temperature conductive hot melt adhesive. Utilizing the ambient heat and melt pressure provided by the extrusion head during the extrusion of the outer semi-conductive layer, the hot melt adhesive is driven to penetrate into the interlacing gaps of the outer braided mesh and cool and solidify. This integrates the fixation of the lead wire with the outer sheath extrusion process, replacing traditional metal spot welding or ultrasonic welding steps, and avoiding localized thermal damage to the internal insulation layer of the cable caused by high welding temperatures. At the same time, the deep mechanical interlocking structure formed after the hot melt adhesive solidifies has good flexibility, which can alleviate stress concentration and reduce the risk of fatigue fracture of the lead wire during long-term alternating hot and cold cycles.
[0044] 3. The low-temperature conductive hot melt adhesive of the present invention uses flake silver powder and multi-walled carbon nanotubes as composite conductive fillers, and pre-modifies the surface with a silane coupling agent. After modification, the amino functional groups grafted on the surface of the filler generate hydrogen bonding forces with the copolyamide hot melt resin matrix, which can effectively prevent the inorganic conductive filler from secondary agglomeration during heating, melting and extrusion rheology. This helps the flake silver powder and carbon nanotubes to be evenly dispersed in the resin matrix and overlap to form a three-dimensional conductive network, thereby reducing the volume resistivity of the cured adhesive layer and maintaining a low contact resistance between the lead wire and the shielding layer. Attached Figure Description
[0045] Figure 1 This is a cross-sectional view of the present invention;
[0046] Figure 2 This is a differential scanning calorimetry (DSC) endothermic curve of the present invention.
[0047] Figure 3 This is a graph showing the viscosity and temperature rheological properties of the present invention.
[0048] Figure 4The image shows the macroscopic transmittance test curves of the cable braided shielding layer sample of the present invention at different bending angles.
[0049] Figure 5 This is a comparison diagram of the shielding effectiveness of the cable of the present invention before and after dynamic bending;
[0050] Figure 6 This is a thermal cycling drift curve of the contact resistance of the cable sample of the present invention.
[0051] Figure 7 This is a partial enlarged view of the contact resistance drift in Embodiments 1 to 5 of the present invention;
[0052] Figure 8 This is a phase distribution diagram of the discharge pulse in the partial discharge test of the present invention;
[0053] Figure 9 This is a bar chart showing the voltage breakdown test results of the present invention.
[0054] Among them, 1. conductor; 2. insulating layer; 3. inner semiconductive layer; 4. braided shielding layer; 5. outer semiconductive layer. Detailed Implementation
[0055] The following is in conjunction with the appendix Figure 1 -Appendix Figure 9 The present invention will be further described in detail below.
[0056] The main raw materials and reagents used in the following examples and comparative examples have the following sources and specifications. Reagents not specifically mentioned are all commercially available analytical grade or higher grade products.
[0057] Ethylene-vinyl acetate copolymer (CAS No.: 24937-78-8), random copolymer, weight-average molecular weight 100,000 to 150,000, molecular weight distribution index 2.5 to 3.5, vinyl acetate mass fraction 28%, melt flow rate 3.0 g / 10 min (tested at 190℃ / 2.16 kg), density 0.95 g / cm³. 3 The Vicat softening point is 42℃.
[0058] The polyolefin elastomer is an ethylene-octene copolymer prepared by metallocene-catalyzed solution polymerization. It belongs to the category of linear short-chain copolymers, with a weight-average molecular weight of 80,000 to 120,000, an octene mass fraction of 38%, a crystallinity of 15%, and a density of 0.87 g / cm³. 3 The Mooney viscosity ML(1+4) at 121℃ is 10, and the glass transition temperature is -52℃.
[0059] Acetylene black (CAS No.: 1333-86-4), with a primary particle size of 35 nm and a specific surface area of 75 m². 2 / g, iodine uptake value is 95g / kg, and dibutyl ester uptake value is 250cm. 3 / 100g, with a volume resistivity of 0.05Ω·cm.
[0060] Copolyamide hot melt resin is formed by random copolymerization and condensation of caprolactam, adipic acid, hexamethylenediamine, and dodecanoic acid, with a weight-average molecular weight of 20,000 to 30,000 and a density of 0.98 g / cm³. 3 The melt flow rate was 25 g / 10 min (tested at 160℃ / 2.16 kg), the softening point by the ring and ball method was 120℃, and the glass transition temperature was -15℃.
[0061] Flake silver powder (CAS No.: 7440-22-4), chemical purity ≥99.9%, average radial dimension D50 of 2.5μm, thickness of 0.2μm, and bulk density of 1.5g / cm³. 3 The tap density is 2.8 g / cm³. 3 Its specific surface area is 1.2 m². 2 / g.
[0062] Multi-walled carbon nanotubes (CAS No.: 308068-56-6), with a carbon content ≥95%, an outer diameter of 15 nm, a length of 10 to 20 μm, and a specific surface area of 250 m² / g. 2 / g, the volume resistivity of the powder is 0.12Ω·cm.
[0063] In this invention, the units of measurement for all materials and solvents are uniformly referred to as parts by weight.
[0064] Reference Figure 1 The shielding structure of the high-voltage cable for new energy vehicles, from the inside out, includes:
[0065] The inner semiconducting layer 3 is disposed on the outer surface of the insulating layer 2 to uniform electric field and prevent partial discharge.
[0066] A braided shielding layer 4 is disposed on the outer surface of the inner semiconductive layer 3. The braided shielding layer 4 adopts a double-layer reverse braided structure, including an inner braided layer braided in a clockwise direction and an outer braided layer braided in a counterclockwise direction. The braiding angle of the inner braided layer relative to the cable axis is the first braiding angle, and the braiding angle of the outer braided layer relative to the cable axis is the second braiding angle. The absolute value of the difference between the first braiding angle and the second braiding angle is ≥10°. This is used to maintain the braided porosity without a sharp increase during dynamic bending of the cable through the double-layer differential angle misalignment complementary mechanism, and to maintain the total braiding density ≥85%.
[0067] An outer semiconductive layer 5 is disposed on the outer surface of the braided shielding layer 4 and is used to fill the pores of the braided shielding layer 4 to improve shielding efficiency.
[0068] The lead wire is disposed between the braided shielding layer 4 and the outer semiconductive layer 5 along the cable axis. The lead wire includes a lead wire baseline and a low-temperature conductive hot melt adhesive covering the outer surface of the lead wire baseline. The low-temperature conductive hot melt adhesive is forcibly penetrated into the interlacing gaps of the outer braided layer by in-situ melting and curing, which is used to form a deep mechanical interlock between the lead wire and the braided shielding layer 4 to maintain low contact resistance and high thermal cycling stability.
[0069] Preparation Example 1:
[0070] This preparation example provides a method for preparing a semiconductive polymer material, including the following steps:
[0071] 80 parts of ethylene-vinyl acetate copolymer, 20 parts of polyolefin elastomer, 1.0 part of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and 2.0 parts of zinc stearate were added to a high-speed mixer and mixed at 70°C for 12 minutes; then 40 parts of acetylene black were slowly added in three batches and the mixture was continued to mix for 25 minutes.
[0072] The premixed material is fed into a co-rotating twin-screw extruder, and the temperatures of each zone of the extruder are set as follows: Zone 1 95℃, Zone 2 110℃, Zone 3 115℃, and Die head 120℃. 1.5 parts of liquefied dicumyl peroxide are injected into the liquid inlet in the middle section of the twin-screw extruder through a metering pump. The extruded material is granulated by a water ring pelletizer, and after dehydration and drying, semi-conductive polymer material particles are obtained. These semi-conductive polymer material particles are named semi-conductive polymer material A.
[0073] Preparation Example 2:
[0074] This preparation example provides a method for preparing a semiconductive polymer material, including the following steps:
[0075] 54 parts of ethylene-vinyl acetate copolymer, 27 parts of polyolefin elastomer, 0.5 parts of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and 1.0 parts of zinc stearate were added to a high-speed mixer and mixed at 60°C for 10 minutes; then 30 parts of acetylene black were slowly added in three batches and the mixture was continued to mix for 20 minutes.
[0076] The premixed material is fed into a co-rotating twin-screw extruder, and the temperatures of each zone of the extruder are set as follows: Zone 1 90℃, Zone 2 105℃, Zone 3 110℃, and Die Head 115℃. At the liquid inlet in the middle section of the twin-screw extruder, 1.0 part of liquefied dicumyl peroxide is injected through a metering pump. The extruded material is granulated by a water ring pelletizer, and after dehydration and drying, semi-conductive polymer material particles are obtained. These semi-conductive polymer material particles are named semi-conductive polymer material B.
[0077] Preparation Example 3:
[0078] This preparation example provides a method for preparing a semiconductive polymer material, including the following steps:
[0079] 90 parts of ethylene-vinyl acetate copolymer, 30 parts of polyolefin elastomer, 1.5 parts of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate) and 3.0 parts of zinc stearate were added to a high-speed mixer and mixed at 80°C for 15 minutes; then 50 parts of acetylene black were slowly added in three batches and the mixture was continued to mix for 30 minutes.
[0080] The premixed material is fed into a co-rotating twin-screw extruder, and the temperatures of each zone of the extruder are set as follows: Zone 1 100℃, Zone 2 115℃, Zone 3 120℃, and Die Head 125℃. 2.5 parts of liquefied dicumyl peroxide are injected into the liquid inlet in the middle section of the twin-screw extruder through a metering pump. The extruded material is granulated by a water ring pelletizer, and after dehydration and drying, semi-conductive polymer material particles are obtained. These semi-conductive polymer material particles are named semi-conductive polymer material C.
[0081] Preparation Example 4:
[0082] This preparation example provides a method for preparing a pre-coated drainage wire, including the following steps:
[0083] 170 parts of flake silver powder and 15 parts of multi-walled carbon nanotubes were added to anhydrous ethanol, and 1.5 parts of γ-aminopropyltriethoxysilane were added dropwise. After ultrasonic dispersion for 40 minutes, the mixture was filtered and vacuum dried (80℃, 2 hours) to obtain the modified composite conductive filler.
[0084] 50 parts of copolyamide hot melt resin and 12 parts of rosin pentaerythritol ester were put into a mixer and mixed at 140°C until completely melted; modified composite conductive filler was added in batches, the speed was controlled at 50 rpm, and the mixture was mixed for 25 minutes to obtain low-temperature conductive hot melt adhesive.
[0085] The low-temperature conductive hot melt adhesive is transferred into the wire extrusion molding machine, and a cross-sectional area of 1.0 mm² is selected. 2 Using multi-strand stranded tin-plated copper wire as the baseline of the lead wire, at an extrusion temperature of 145°C, low-temperature conductive hot melt adhesive is wrapped around the outer surface of the lead wire baseline with a radial thickness of 0.2 mm. After cooling, the pre-coated lead wire is obtained. This pre-coated lead wire is named pre-coated lead wire A.
[0086] Preparation Example 5:
[0087] This preparation example provides a method for preparing a pre-coated drainage wire, including the following steps:
[0088] 200 parts of flake silver powder and 20 parts of multi-walled carbon nanotubes were added to anhydrous ethanol, and 2.0 parts of γ-aminopropyltriethoxysilane were added dropwise. After ultrasonic dispersion for 50 minutes, the mixture was filtered and vacuum dried (80℃, 2 hours) to obtain the modified composite conductive filler.
[0089] 40 parts of copolyamide hot melt resin and 10 parts of rosin pentaerythritol ester were put into a mixer and mixed at 130°C until completely melted; modified composite conductive filler was added in batches, the speed was controlled at 60 rpm, and the mixture was mixed for 20 minutes to obtain low-temperature conductive hot melt adhesive.
[0090] The low-temperature conductive hot melt adhesive is transferred into the wire extrusion molding machine, and a cross-sectional area of 0.5mm² is selected. 2 Using multi-strand stranded tin-plated copper wire as the baseline of the lead wire, at an extrusion temperature of 140℃, low-temperature conductive hot melt adhesive is wrapped around the outer surface of the lead wire baseline with a radial thickness of 0.1mm. After cooling, the pre-coated lead wire is obtained. This pre-coated lead wire is named pre-coated lead wire B.
[0091] Preparation Example 6:
[0092] This preparation example provides a method for preparing a pre-coated drainage wire, including the following steps:
[0093] 150 parts of flake silver powder and 10 parts of multi-walled carbon nanotubes were added to anhydrous ethanol, and 1.0 part of γ-aminopropyltriethoxysilane was added dropwise. After ultrasonic dispersion for 30 minutes, the mixture was filtered and vacuum dried (80℃, 2 hours) to obtain the modified composite conductive filler.
[0094] 60 parts of copolyamide hot melt resin and 15 parts of rosin pentaerythritol ester were put into a mixer and mixed at 150°C until completely melted; modified composite conductive filler was added in batches, the speed was controlled at 40 rpm, and the mixture was mixed for 35 minutes to obtain low-temperature conductive hot melt adhesive.
[0095] The low-temperature conductive hot melt adhesive is transferred into the wire extrusion molding machine, and a cross-sectional area of 1.5mm² is selected. 2 Using multi-strand stranded tin-plated copper wire as the baseline of the lead wire, at an extrusion temperature of 150°C, low-temperature conductive hot melt adhesive is wrapped around the outer surface of the lead wire baseline with a radial thickness of 0.3 mm. After cooling, the pre-coated lead wire is obtained. This pre-coated lead wire is named pre-coated lead wire C.
[0096] Example 1:
[0097] This embodiment provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, including the following steps:
[0098] S1. Provide a cable core that has been covered with inner insulation layer 2 and inner semiconductive layer 3. Set the number of braiding spindles of the first and second series braiding machines to 24 spindles each. Each spindle is configured with 6 tin-plated copper wires with a single wire diameter of 0.15mm. The single spindle wire tension is constant at 8N.
[0099] S2. Feed the cable core into the first braiding machine and braid it on the surface of the inner semiconductive layer 3. Control the speed ratio between the traction wheel speed and the spindle speed so that the first braiding angle is 45° to form the inner braided mesh. Control the braiding density of this single layer to 45%.
[0100] S3. The core wires continuously enter the second braiding machine and are braided a second time on the surface of the inner braided mesh. The speed ratio is adjusted so that the second braiding angle is 30° to form the outer braided mesh. The braiding density of this outer layer is controlled to be 45%. At this time, the absolute value of the difference between the first braiding angle and the second braiding angle is 15°.
[0101] S4. Monitor the light transmittance of the two layers of mesh in real time using an online visual inspection instrument, and adjust the traction speed and spindle tension in a closed loop to ensure that the total weaving density after the double-layer misalignment is constant at ≥85%;
[0102] S5. After the outer layer is woven, before entering the extruder head of the outer sheath, the pre-coated lead wire A is attached to the outer surface of the outer layer woven mesh in a straight axial direction at the same linear speed as the cable core through the guide wheel device.
[0103] S6. Feed the entire wire harness into the extruder and use an extrusion die to extrude the semi-conductive polymer material A as the outer semi-conductive layer 5. Set the extruder head temperature to 170°C and generate a melt pressure of 20MPa inside the extrusion die. The heat of 170°C is instantly conducted to the pre-coated lead wire, causing the low-temperature conductive hot melt adhesive on the surface to liquefy and be forced to penetrate into the interwoven gaps of the outer braided mesh under the pressure of 20MPa.
[0104] S7. The extruded composite cable is immediately placed in a circulating water tank at a temperature of 30°C for cooling. The conductive hot melt adhesive is cured, completing the fixation and bonding of the lead wire, the outer braided mesh and the outer semi-conductive layer 5.
[0105] Example 2:
[0106] This embodiment provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, including the following steps:
[0107] S1. Provide a cable core that has been covered with inner insulation layer 2 and inner semiconductive layer 3. Set the number of braiding spindles of the two series braiding machines to 16, and configure each spindle with 4 tinned copper wires with a single wire diameter of 0.15mm. The single spindle wire tension is constant at 5N.
[0108] S2. Feed the cable core into the first braiding machine, control the speed ratio so that the first braiding angle is 40° to form the inner braided mesh, and control the braiding density of this single layer to 40%;
[0109] S3. The core yarn continuously enters the second braiding machine. The speed ratio is adjusted so that the second braiding angle is 25° to form the outer braided mesh. The braiding density of this outer layer is controlled to be 40%. At this time, the absolute value of the difference between the first braiding angle and the second braiding angle is 15°.
[0110] S4. Real-time monitoring using an online visual inspection device ensures that the total weaving density after double-layer misalignment is constant at ≥85%;
[0111] S5. After the outer layer is woven, attach the pre-coated guide wire B straight along the axial direction to the outer surface of the outer woven mesh.
[0112] S6. Feed the wire harness into the extruder and use an extrusion die to extrude the semi-conductive polymer material B as the outer semi-conductive layer 5. Set the extruder head temperature to 165℃ and generate a melt pressure of 18MPa inside the extrusion die. The conductive hot melt adhesive liquefies and penetrates into the interwoven gaps of the outer braided mesh under pressure.
[0113] S7. The extruded composite cable is cooled in a circulating water tank at a temperature of 20°C. The conductive hot melt adhesive is cured, and the lead wire, outer braided mesh and outer semi-conductive layer 5 are fixedly bonded.
[0114] Example 3:
[0115] This embodiment provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, including the following steps:
[0116] S1. Provide a cable core that has been covered with inner insulation layer 2 and inner semiconductive layer 3. Set the number of braiding spindles of the two series braiding machines to 32 spindles each. Each spindle is configured with 8 tinned copper wires with a single wire diameter of 0.15mm. The single spindle wire tension is constant at 10N.
[0117] S2. Feed the cable core into the first braiding machine, control the speed ratio so that the first braiding angle is 50° to form the inner braided mesh, and control the braiding density of this single layer to be 50%;
[0118] S3. The core yarn continuously enters the second braiding machine. The speed ratio is adjusted so that the second braiding angle is 35° to form the outer braided mesh. The braiding density of this outer layer is controlled to be 50%. At this time, the absolute value of the difference between the first braiding angle and the second braiding angle is 15°.
[0119] S4. Real-time monitoring using an online visual inspection device ensures that the total weaving density after double-layer misalignment is constant at ≥85%;
[0120] S5. After the outer layer is woven, attach the pre-coated guide wire C straight along the axial direction to the outer surface of the outer woven mesh.
[0121] S6. Feed the wire harness into the extruder and use an extrusion die to extrude the semi-conductive polymer material C as the outer semi-conductive layer 5. Set the extruder head temperature to 180℃ and generate a melt pressure of 25MPa inside the extrusion die. The conductive hot melt adhesive liquefies and penetrates into the interwoven gaps of the outer braided mesh under pressure.
[0122] S7. The extruded composite cable is cooled in a circulating water tank at a temperature of 40°C, and the conductive hot melt adhesive is cured to complete the fixing and bonding.
[0123] Example 4:
[0124] This embodiment provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, including the following steps:
[0125] S1. Provide a cable core that has been covered with inner insulation layer 2 and inner semiconductive layer 3. Set the number of braiding spindles of the two series braiding machines to 24 spindles each. Each spindle is configured with 6 tin-plated copper wires with a single wire diameter of 0.15mm. The single spindle wire tension is constant at 8N.
[0126] S2. Feed the cable core into the first braiding machine, control the speed ratio so that the first braiding angle is 45° to form the inner braided mesh, and control the braiding density of this single layer to 45%;
[0127] S3. The core yarn continuously enters the second braiding machine. The speed ratio is adjusted so that the second braiding angle is 35° to form the outer braided mesh. The braiding density of this outer layer is controlled to be 45%. At this time, the absolute value of the difference between the first braiding angle and the second braiding angle is 10°.
[0128] S4. Real-time monitoring using an online visual inspection device ensures that the total weaving density after double-layer misalignment is constant at ≥85%;
[0129] S5. After the outer layer is woven, attach the pre-coated guide wire A straight along the axial direction to the outer surface of the outer woven mesh.
[0130] S6. Feed the wire harness into the extruder and use an extrusion die to extrude the semi-conductive polymer material A as the outer semi-conductive layer 5. Set the extruder head temperature to 170℃ and generate a melt pressure of 20MPa inside the extrusion die. The conductive hot melt adhesive liquefies and penetrates into the interwoven gaps of the outer braided mesh under pressure.
[0131] S7. The extruded composite cable is cooled in a circulating water tank at a temperature of 30°C, and the conductive hot melt adhesive is cured to complete the fixing and bonding.
[0132] Example 5:
[0133] This embodiment provides a braiding process for the shielding layer of a high-voltage cable for new energy vehicles, including the following steps:
[0134] S1. Provide a cable core that has been covered with inner insulation layer 2 and inner semiconductive layer 3. Set the number of braiding spindles of the two series braiding machines to 24 spindles each. Each spindle is configured with 6 tin-plated copper wires with a single wire diameter of 0.15mm. The single spindle wire tension is constant at 8N.
[0135] S2. Feed the cable core into the first braiding machine, control the speed ratio so that the first braiding angle is 45° to form the inner braided mesh, and control the braiding density of this single layer to 45%;
[0136] S3. The yarn cores continuously enter the second braiding machine. The speed ratio is adjusted so that the second braiding angle is 30° to form the outer braided mesh. The braiding density of this outer layer is controlled to be 45%. At this time, the absolute value of the difference between the first braiding angle and the second braiding angle is 15°.
[0137] S4. Real-time monitoring using an online visual inspection device ensures that the total weaving density after double-layer misalignment is constant at ≥85%;
[0138] S5. After the outer layer is woven, attach the pre-coated guide wire A straight along the axial direction to the outer surface of the outer woven mesh.
[0139] S6. Feed the wire harness into the extruder and use an extrusion die to extrude the semi-conductive polymer material A as the outer semi-conductive layer 5. Set the extruder head temperature to 150℃ and generate a melt pressure of 15MPa inside the extrusion die. The conductive hot melt adhesive liquefies and penetrates into the interwoven gaps of the outer braided mesh under pressure.
[0140] S7. The extruded composite cable is cooled in a circulating water tank at a temperature of 20°C, and the conductive hot melt adhesive is cured to complete the fixing and bonding.
[0141] Comparative Example 1:
[0142] Compared with Example 1, the difference is that: no double-layer weaving is performed, only single-layer weaving is performed, the single-layer weaving angle is controlled at 45°, and by increasing the number of spindles and the number of strands per spindle, the single-layer weaving density directly reaches 85%, and the rest are the same.
[0143] Comparative Example 2:
[0144] Compared with Example 1, the difference is that the speed ratio between the traction wheel speed and the spindle disc speed is controlled so that the first weaving angle of the first weaving machine and the second weaving angle of the second weaving machine are the same, both being 45°, that is, the absolute value of the difference between the first weaving angle and the second weaving angle is 0°, and all other aspects are the same.
[0145] Comparative Example 3:
[0146] Compared with Example 1, the difference is that in S5, the pre-coated guide wire A is not used, but instead a wire with a cross-sectional area of 1.0 mm² is used directly. 2 The multi-strand stranded bare tin-plated copper wire is used as the lead wire. No conductive hot melt adhesive is applied to the surface. It is directly and straight along the axial direction and attached to the outer surface of the outer braided mesh. Everything else is the same.
[0147] Comparative Example 4:
[0148] Compared with Example 1, the difference is that in S6, the extrusion die of the extruder is replaced with a conventional tube extrusion die. Under this die structure, high melt pressure cannot be established inside, and the liquefied conductive hot melt adhesive cannot undergo forced pressure penetration. Everything else is the same.
[0149] Comparative Example 5:
[0150] The difference compared to Example 1 is that, in S5, a pre-coated guide wire A is not used; instead, a wire with a cross-sectional area of 1.0 mm² is used. 2 Multi-strand stranded bare tinned copper wire is used as the lead wire, and the lead wire is directly spot-welded to the outer braided mesh at certain intervals using conventional resistance spot welding process, and the rest is the same.
[0151] Test Example 1:
[0152] The low-temperature conductive hot melt adhesive on the surface of the pre-coated guide wire A in Preparation Example 4 was taken as the first sample; the semi-conductive polymer material A particles prepared in Preparation Example 1 were taken as the second sample.
[0153] Using a differential scanning calorimeter, under a nitrogen protective atmosphere, with the gas flow rate set to 50 mL / min, approximately 8.5 mg of the first and second samples were weighed and placed in an aluminum standard crucible. The test temperature program was set to heat from 80 °C to 200 °C at a heating rate of 10 °C / min. The heat flow rate change data during the heating process were recorded to obtain the endothermic and exothermic peak values and the phase transition temperature range.
[0154] Using a rotational rheometer with a 25mm parallel plate clamp, the first and second samples were pre-pressed into 1.5mm thick discs with a gap of 1.0mm. The test was conducted in strain control mode with a constant shear frequency of 1Hz, a strain amplitude of 1% (within the linear viscoelastic region), a test temperature range of 80℃ to 200℃, and a heating rate of 3℃ / min. The rheological response data of the complex viscosity of the samples as a function of temperature were continuously recorded.
[0155] Table 1. Thermodynamic and rheological test data of low-temperature conductive hot melt adhesives and semiconductive polymer materials:
[0156] Test temperature (°C) Hot melt adhesive heat flow rate (W / g) Heat flow rate of semiconductive materials (W / g) Complex viscosity of hot melt adhesive (Pa·s) Complex viscosity of semiconductive materials (Pa·s) 80 0.126 0.852 518423.5 26541.2 90 0.141 3.214 310542.1 11452.6 100 0.203 1.156 185421.8 8321.4 110 0.652 0.312 86452.3 6105.8 120 3.784 0.245 542.7 5014.3 130 0.812 0.211 92.4 4512.7 140 0.218 0.185 44.6 4125.1 150 0.176 0.162 27.9 3841.5 160 0.142 0.141 22.1 3582.6 170 0.138 0.126 17.5 4153.2 180 0.131 -0.542 14.8 9241.7 190 0.125 -1.315 12.3 23154.5 200 0.119 -1.824 11.6 58462.1
[0157] According to Table 1 and Figure 2 and Figure 3 The test results show that the endothermic melting peak of the low-temperature conductive hot melt adhesive appears around 120℃, while the melting peak of the matrix resin of the semiconductive material A is around 90℃. In the range of 160℃ to 180℃, the complex viscosity of the semiconductive material A increases and the heat flow rate turns negative, indicating that a polymer crosslinking reaction initiated by dicumyl peroxide has occurred. At this time, the complex viscosity of the conductive hot melt adhesive in liquid state has dropped to below 30 Pa·s.
[0158] Rheological and thermodynamic data confirm that, under the set extrusion process of 170℃, the semiconductive polymer material A remains in an extrudable viscoelastic state and begins to crosslink and solidify, while the conductive hot melt adhesive attached to the outside is in a low-viscosity liquefied state. The viscosity difference formed between the liquid hot melt adhesive and the semiconductive material melt, combined with the melt pressure provided inside the extrusion die, can drive the hot melt adhesive to fill the gaps in the woven mesh, establishing a continuous conductive path at the microscale without causing excessive flow or pyrolysis of the semiconductive layer material. This confirms that the in-situ extrusion thermodynamic parameter settings and melt penetration mechanism in this scheme are technologically feasible.
[0159] Test Example 2:
[0160] Cable cores after the first and second braiding processes in Example 1, Comparative Example 1, and Comparative Example 2 were cut as test samples, with a single sample cut length of 500 mm.
[0161] The test sample is fixed between the movable and fixed clamps of the dynamic bending test machine. A parallel laser emitter is placed on the outer arc side of the sample where bending deformation occurs, and an integrating sphere photodetector is placed on the opposite side that passes through the center of the sample. The working area of the test machine is enclosed with a light-absorbing partition to shield ambient light.
[0162] The dynamic bending tester is controlled to run at a constant speed, so that the bending angle of the test sample gradually increases from 0° to 120°. The transmitted light intensity signal received by the integrating sphere photodetector is continuously collected, and the ratio of the transmitted light intensity to the initial light intensity of the transmitter is calculated. The macroscopic transmittance values of each sample at different bending angles are recorded.
[0163] Table 2. Test data on the light transmittance of cable braided shielding layer 4 at different bending angles:
[0164] Bending angle (°) Example 1: Light transmittance (%) Comparative Example 1: Light transmittance (%) Comparative Example 2: Light transmittance (%) 0 10.42 14.15 11.23 15 10.87 15.68 12.16 30 11.41 18.24 14.58 45 11.23 21.05 17.11 60 12.35 24.31 19.85 75 13.06 27.52 21.64 90 12.78 29.84 23.47 105 13.82 32.19 25.12 120 14.35 34.62 27.85
[0165] According to Table 2 and Figure 4The test results show that when the single-layer woven mesh of Comparative Example 1 and the double-layer woven mesh of Comparative Example 2 are bent, the light transmittance increases with the increase of the bending angle. This reflects that when the cable is subjected to axial tensile stress on the outside of the bend, the diamond-shaped mesh with a single angle distribution expands, causing the porosity to exceed the control threshold of 15%.
[0166] In Example 1, the light transmittance of the test sample remained within the range of 10% to 14.5% during dynamic bending from 0° to 120° without any sudden increase. The first weaving angle of 45° and the second weaving angle of 30° used in Example 1 have a difference of 15°. The outer and inner meshes have different stretching and compression ratios when responding to deformation. The area where the outer mesh expands due to stretching is blocked by the inner metal wire with different deformation profile. The physical misalignment of the woven mesh limits the increase in overall porosity. The test shows that the differential angle double-layer woven structure can maintain a constant overall weaving density under bending conditions.
[0167] Test Example 3:
[0168] The composite cable products prepared in Examples 1 to 5, as well as Comparative Examples 1 and 2, were cut as test samples. The length of each sample was 3000 mm. The outer sheath was removed from both ends of the sample to expose the shielding layer for connection to the test fixture.
[0169] Initial shielding effectiveness was tested using a vector network analyzer in conjunction with a three-coaxial test tube. The test frequency range was set from 30MHz to 1GHz, and the initial shielding effectiveness values of each sample at 100MHz were recorded.
[0170] The samples that have completed the initial test are mounted on a cable dynamic bending fatigue testing machine. The bending radius is set to 5 times the outer diameter of the cable, and the bending rate is set to 30 times / minute. The testing machine is controlled to perform 100,000 continuous reciprocating bends on all samples.
[0171] After the bending process is completed, the test sample is removed and reconnected to the vector network analyzer and the three coaxial test tube. Under the same test conditions, the shielding effectiveness value at 100MHz frequency is read, and the shielding effectiveness attenuation before and after bending is calculated.
[0172] Table 3. Test data on shielding effectiveness of cables before and after dynamic bending in the examples and comparative examples:
[0173] Sample number Initial shielding effectiveness (dB) Shielding effectiveness after bending (dB) Shielding effectiveness attenuation (dB) Example 1 78.42 76.15 2.27 Example 2 75.86 74.21 1.65 Example 3 81.24 79.52 1.72 Example 4 79.18 76.84 2.34 Example 5 78.65 76.51 2.14 Comparative Example 1 77.53 62.47 15.06 Comparative Example 2 78.11 65.38 12.73
[0174] According to Table 3 and Figure 5The test results show that the shielding effectiveness values of Examples 1 to 5 and Comparative Examples 1 to 2 are similar in the initial state, all within the range of 75dB to 82dB. After 100,000 dynamic reciprocating bends, the shielding effectiveness of the single-layer braided structure of Comparative Example 1 and the double-layer braided structure of Comparative Example 2 at the same angle shows a decreasing trend, with attenuation reaching 15.06dB and 12.73dB respectively. The attenuation of Examples 1 to 5 under the same conditions remains between 1.65dB and 2.34dB, and the shielding performance shows high stability.
[0175] When conventional single-layer and double-layer braided networks are subjected to cyclic bending stress, the metal wires on the outer arc side of the bend undergo synchronous axial stretching and radial contraction, causing irreversible expansion of the mesh aperture. This increases the leakage channels for high-frequency electromagnetic waves, leading to a decrease in shielding effectiveness. The embodiment adopts a design where the difference between the first and second braiding angles is greater than or equal to 10°. Under stress, the deformation profiles of the inner and outer meshes are misaligned. This asynchronous geometric deformation causes the two meshes to form physical barriers and mutual compensation in the bending deformation zone, maintaining the overall shielding coverage of the cable shielding layer and exhibiting better fatigue resistance and shielding retention capabilities.
[0176] Test Example 4:
[0177] The composite cable products prepared in Examples 1 to 5, Comparative Example 3 and Comparative Example 4 were used as test samples. The length of a single sample was 1000 mm. The outer sheath and the outer semiconductive layer 5 were removed from both ends of the sample to expose the pre-coated lead wire (or bare copper lead wire) and the outer braided mesh. The test lead wire was fixed to both ends of the lead wire and the outer braided mesh with conductive silver paste to prepare a four-terminal contact resistance test circuit.
[0178] The initial contact resistance of each test circuit was measured using a high-precision micro-resistance meter at room temperature (25°C), and the data was recorded as the baseline value for zero cycles.
[0179] The test sample with the leads connected was placed in the high and low temperature alternating damp heat test chamber. The thermal cycling program was set as follows: each cycle consisted of maintaining a constant temperature of -40℃ for 30 minutes, followed by raising the temperature to 125℃ within 5 minutes and maintaining it for 30 minutes. The total number of cycle tests was set to 100.
[0180] During the thermal cycling test, the sample was returned to room temperature every 20 cycles, and the contact resistance between the drain wire and the outer braided mesh was remeasured using a micro resistance meter. The resistance drift data at different cycling stages were recorded, and the change in contact resistance was calculated after 100 cycles.
[0181] Table 4. Contact resistance data during the thermal cycling test of the cables in the examples and comparative examples:
[0182] Sample number 0 times / initial (mΩ) 20 times (mΩ) 40 times (mΩ) 60 times (mΩ) 80 times (mΩ) 100 times (mΩ) Example 1 2.14 2.18 2.21 2.24 2.28 2.31 Example 2 2.45 2.51 2.56 2.62 2.68 2.74 Example 3 1.98 2.01 2.05 2.11 2.13 2.19 Example 4 2.67 2.71 2.78 2.82 2.88 2.95 Example 5 3.12 3.25 3.32 3.41 3.55 3.68 Comparative Example 3 16.42 28.53 41.22 57.81 76.45 92.18 Comparative Example 4 8.76 11.24 15.68 21.34 28.91 36.42
[0183] According to Table 4 and Figure 6 and Figure 7 The test results show that the initial contact resistance of Examples 1 to 5 remained in the low range of 1.98mΩ to 3.12mΩ, and after 100 cycles of alternating heat from -40℃ to 125℃, the change in resistance value did not exceed 0.6mΩ, demonstrating high electrical connection stability. Comparative Example 3 used a bare copper lead wire without adhesive, and its initial contact resistance was higher. After thermal cycling, due to the difference in the coefficients of thermal expansion and contraction between the metal and the polymer matrix, the contact points became physically loose, and the contact resistance rose to 92.18mΩ.
[0184] Comparative Example 4, due to the use of an extrusion die, failed to establish melt pressure during extrusion. The liquefied conductive hot melt adhesive failed to penetrate into the interwoven gaps of the woven mesh, remaining only on the surface of the mesh to form weak point adhesions. Under the action of thermal shock stress, microscopic peeling occurred at the adhesion interface, and the contact resistance showed a continuous upward trend with the number of cycles. The embodiment solution maintained a melt pressure of 15MPa to 25MPa in the extrusion die, driving the low-viscosity hot melt adhesive into the micropores of the woven mesh. After curing, an axial continuous surface contact interface based on micro-mechanical interlocking was constructed. This structure not only increases the actual conductive contact area to reduce the initial resistance, but also resists the interface loosening caused by thermal strain by relying on the deep interlocking effect, confirming the role of the in-situ melt penetration process in improving the reliability of the drain wire connection.
[0185] Test Example 5:
[0186] The finished cable products prepared in Examples 1 to 5 and Comparative Example 5 were used as test samples. Each sample was cut into a standard length of 1200mm. The outer sheath and outer semiconductive layer 5 with a length of 150mm were removed from one end of the test sample to expose the internal drain wire and braided shielding mesh. The other end was kept structurally intact and the end was insulated and sealed.
[0187] Using a microcomputer-controlled electronic universal testing machine, the complete end of the sample is fixed to the lower clamp, and the peeled end of the drain wire is fixed to the upper clamp. The tensile rate is set to 50 mm / min, and the axial tension is increased until the drain wire is peeled off or broken from the surface of the braided mesh. The peak value of the maximum pull-out force captured by the sensor is recorded.
[0188] The test sample is placed in a shielded room and connected to the circuit of the partial discharge test transformer and the partial discharge detector. An AC power frequency voltage is applied between the conductor 1 of the sample and the shielding layer, and the voltage is gradually increased to the test standard voltage (set to 2.5 times the rated voltage U0). The voltage is held for 5 minutes, and the apparent partial discharge quantity under this voltage is recorded by the detector. The discharge pulse spectrum in the power frequency phase range from 0° to 360° is also collected.
[0189] After the partial discharge test is completed, the sample is moved into the insulating oil tank of the high-voltage breakdown test bench to prevent end surface flashover. The power frequency AC voltage is continued to be applied to the sample at a constant voltage increase rate of 1kV / s until the instrument detects a sudden change in leakage current and a momentary drop in voltage. The breakdown voltage value at this time is recorded.
[0190] Table 5. Test data of pull-out force and high-voltage electrical performance of cable samples from the examples and comparative examples:
[0191] Sample number Axial tensile strength (N) Apparent partial discharge quantity (pC) Breakdown voltage (kV) Example 1 128.4 2.1 48.5 Example 2 122.3 2.7 46.2 Example 3 134.1 1.8 51.4 Example 4 125.6 2.4 47.8 Example 5 129.8 2.9 49.1 Comparative Example 5 145.2 134.8 23.6
[0192] According to Table 5 and Figure 8 and Figure 9 The test results show that the axial pull-out strength of Examples 1 to 5 is in the range of 122N to 134N, the partial discharge is maintained below 3pC, and the breakdown voltage is higher than 46kV, which meets the mechanical adhesion and electrical insulation standards of high-voltage cables. Comparative Example 5 adopts the traditional spot welding process, and its axial pull-out strength reaches 145.2N due to the metallurgical bond formed by metal melting; however, in the partial discharge test spectrum, characteristic discharge pulses with peak values exceeding 130pC appear in the first quadrant (around 75°) and the third quadrant (around 255°), respectively, and the overall breakdown voltage drops to 23.6kV.
[0193] Spot welding generates a high-temperature electric arc at the moment of contact. This heat is rapidly conducted inward through the woven shielding mesh, exceeding the thermal degradation temperature of the bottom semi-conductive polymer layer and the insulating layer 2. This causes localized thermodynamic damage at the insulation interface, forming microscopic pores or carbonization points. Under the action of a high-voltage alternating electric field, electric field distortion occurs at these micro-defects, triggering strong ionization discharge and ultimately causing premature failure of dielectric strength.
[0194] The embodiment scheme uses the ambient temperature (150°C to 180°C) provided outside the extrusion molding head to liquefy the hot melt adhesive and rely on fluid pressure for penetration. This low-temperature, distributed heat conduction process acts as a thermal buffer, avoiding local thermal stress concentration. While establishing physical interlocking adhesion, it ensures the integrity of the internal insulation structure of the cable. Test data confirms the advantages of the in-situ hot melt penetration process over traditional welding processes in avoiding material damage from a macroscopic performance perspective.
[0195] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A shielding layer structure for high-voltage cables in new energy vehicles, characterized in that, The shielding layer structure of the high-voltage cable for new energy vehicles comprises, from the inside out: An inner semiconductive layer (3) is disposed on the outer surface of the insulating layer (2) to uniform electric field and avoid partial discharge; A braided shielding layer (4) is disposed on the outer surface of the inner semiconductive layer (3). The braided shielding layer (4) adopts a double-layer reverse braiding structure, including an inner braided layer braided in a clockwise direction and an outer braided layer braided in a counterclockwise direction. The braiding angle of the inner braided layer relative to the cable axis is the first braiding angle, and the braiding angle of the outer braided layer relative to the cable axis is the second braiding angle. The absolute value of the difference between the first braiding angle and the second braiding angle is ≥10°. This is used to maintain the braided porosity without a sharp increase and keep the total braiding density ≥85% by the double-layer differential angle misalignment complementary mechanism when the cable is dynamically bent. An outer semiconductive layer (5) is disposed on the outer surface of the braided shielding layer (4) to fill the pores of the braided shielding layer (4) to improve shielding efficiency; The drain wire is disposed between the braided shielding layer (4) and the outer semiconductive layer (5) along the cable axis. The drain wire includes a drain wire baseline and a low-temperature conductive hot melt adhesive covering the outer surface of the drain wire baseline. The low-temperature conductive hot melt adhesive is forcibly penetrated into the interlacing gap of the outer braided layer by in-situ melting and solidification, which is used to form a deep mechanical interlock between the drain wire and the braided shielding layer (4) to maintain low contact resistance and high thermal cycling stability. The low-temperature conductive hot melt adhesive is made of the following components in parts by weight: 40 to 60 parts of copolyamide hot melt resin, 10 to 15 parts of rosin pentaerythritol ester, 150 to 200 parts of flake silver powder, and 10 to 20 parts of multi-walled carbon nanotubes.
2. The shielding layer structure for high-voltage cables of new energy vehicles according to claim 1, characterized in that, The outer semiconductive layer (5) is made of raw materials comprising the following parts by weight: 54 to 90 parts of ethylene-vinyl acetate copolymer; 20 to 30 parts of polyolefin elastomer; 0.5 to 1.5 parts of pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate); Zinc stearate 1.0 to 3.0 parts; 30 to 50 parts of acetylene black; 1.0 to 2.5 parts of dicumyl peroxide.
3. The shielding layer structure for high-voltage cables of new energy vehicles according to claim 1, characterized in that, The baseline of the drainage line has a cross-sectional area of 0.5 to 1.5 mm². 2 The low-temperature conductive hot melt adhesive contains multi-strand stranded tin-plated copper wire; the average radial dimension D50 of the flake silver powder is 2.0 to 3.0 μm, and the thickness is 0.1 to 0.3 μm; the outer diameter of the multi-walled carbon nanotube is 10 to 20 nm, and the length is 10 to 20 μm; the weight-average molecular weight of the copolyamide hot melt resin is 20,000 to 30,000, and the ring and ball softening point is 110°C to 130°C.
4. The shielding layer structure for high-voltage cables of new energy vehicles according to claim 1, characterized in that, The low-temperature conductive hot melt adhesive also contains a silane coupling agent, which is γ-aminopropyltriethoxysilane, and the amount used is 1.0 to 2.0 parts. The flake silver powder and multi-walled carbon nanotubes in the low-temperature conductive hot melt adhesive are pre-treated as follows: the flake silver powder and multi-walled carbon nanotubes are added to anhydrous ethanol, the silane coupling agent is added dropwise, and after ultrasonic dispersion, filtration and vacuum drying, a modified composite conductive filler is obtained, which is then mixed with copolyamide hot melt resin and rosin pentaerythritol ester.
5. The shielding layer structure for high-voltage cables of new energy vehicles according to claim 1, characterized in that, The first weaving angle is 40° to 50°, the second weaving angle is 25° to 35°, and the absolute value of the difference between the first weaving angle and the second weaving angle is 15°; the weaving density of the inner weaving layer is 40% to 50%, and the weaving density of the outer weaving layer is 40% to 50%.
6. A braiding process for a high-voltage cable shielding layer for new energy vehicles according to any one of claims 1-5, characterized in that, Includes the following steps: S1. A cable core with an internal conductor (1) and an insulation layer (2) and an inner semiconductive layer (3) is provided; S2. The cable core is fed into the first braiding machine, and the first braid is performed on the surface of the inner semiconductive layer (3) to form an inner braided mesh. The braiding angle relative to the cable axis is controlled to be the first braiding angle. S3. The wire core is continuously fed into the second braiding machine, and a second reverse braiding is performed on the surface of the inner braided mesh to form the outer braided mesh. The braiding angle relative to the cable axis is controlled to be the second braiding angle, and the absolute value of the difference between the first braiding angle and the second braiding angle is controlled to be ≥10°. S4. Monitor the light transmittance of the two-layer woven mesh in real time and perform closed-loop adjustment to ensure that the total woven density after the double-layer staggered superposition is constant at ≥85%; S5. After the outer layer is woven, the pre-coated lead wire with the surface covered with low-temperature conductive hot melt adhesive is attached straight along the cable axis to the outer surface of the outer layer woven mesh. S6. The wire harness is fed into the extruder as a whole. Using an extrusion mold, the semi-conductive polymer material for preparing the outer semi-conductive layer (5) is extruded onto the outer braided mesh and the pre-coated lead wire. The ambient heat provided by the die head during the extrusion process causes the low-temperature conductive hot melt adhesive on the surface of the pre-coated lead wire to liquefy instantly. The melt pressure in the extrusion mold drives the liquefied conductive hot melt adhesive to forcefully penetrate into the interlacing gaps of the outer braided mesh. S7. Cool the extruded composite cable to solidify the conductive hot melt adhesive and the outer semiconductive layer (5), and complete the physical interlocking bonding of the outer braided mesh of the lead wire and the braided shielding layer (4) with the outer semiconductive layer (5).
7. The braiding process for the shielding layer of high-voltage cables for new energy vehicles according to claim 6, characterized in that, The step of attaching the pre-coated lead wire, whose surface is covered with low-temperature conductive hot melt adhesive, straight along the cable axis to the outer surface of the outer braided mesh after the outer layer is woven includes: The cross-sectional area is 0.5 to 1.5 mm. 2 Multi-strand stranded tinned copper wire is used as the baseline of the lead wire and is inserted into the wire extrusion molding machine. At an extrusion temperature of 140°C to 150°C, the molten low-temperature conductive hot melt adhesive is uniformly coated on the outer surface of the lead wire baseline with a radial thickness of 0.1 mm to 0.3 mm. After cooling, the pre-coated lead wire is collected and then attached to the outer surface of the outer braided mesh in a straight line along the cable axis.
8. The braiding process for the shielding layer of high-voltage cables for new energy vehicles according to claim 6, characterized in that, The steps of feeding the wire harness as a whole into an extruder, using an extrusion die to extrude the semi-conductive polymer material for preparing the outer semi-conductive layer (5) onto the outer braided mesh and the pre-coated lead wire, utilizing the ambient heat provided by the die head during the extrusion process to instantly liquefy the low-temperature conductive hot melt adhesive on the surface of the pre-coated lead wire, and using the melt pressure in the extrusion die to force the liquefied conductive hot melt adhesive to penetrate into the interlacing gaps of the outer braided mesh include: The extruder head temperature is set to 150°C to 180°C, and a continuous melt pressure of 15MPa to 25MPa is established and maintained inside the extrusion mold; the extrusion temperature of the semi-conductive polymer material is higher than the softening point of the low-temperature conductive hot melt adhesive.
9. The braiding process for the shielding layer of high-voltage cables for new energy vehicles according to claim 6, characterized in that, The steps of feeding the cable core into the first braiding machine, performing the first braiding on the surface of the inner semiconductive layer (3) to form an inner braided mesh, and controlling the braiding angle relative to the cable axis to the first braiding angle; The steps of continuously feeding the wire cores into a second braiding machine, performing a second reverse braiding on the surface of the inner braided mesh to form an outer braided mesh, controlling the braiding angle relative to the cable axis as a second braiding angle, and controlling the absolute value of the difference between the first braiding angle and the second braiding angle to be ≥10°, all include: The single-spindle wire feeding tension is constantly controlled between 5N and 10N; The steps for real-time monitoring of the light transmittance of the superimposed mesh of the two layers of woven mesh, and closed-loop adjustment to ensure that the total weaving density after the double-layer staggered superposition remains constant at ≥85% include: The transmittance of the two layers of mesh after misalignment and superposition is monitored in real time by an online visual inspection instrument. The traction speed and spindle tension are adjusted in a closed loop to change the rotational speed ratio between the traction wheel and the spindle disc, so that the macroscopic transmittance of the double-layer woven mesh after physical misalignment and superposition is always kept below 15%.
10. The braiding process for the shielding layer of the high-voltage cable for new energy vehicles according to claim 6, characterized in that, The steps of cooling the extruded composite cable to solidify the conductive hot melt adhesive and the outer semiconductive layer (5), and completing the physical interlocking bonding of the outer braided mesh of the drain wire and the braided shielding layer (4) with the outer semiconductive layer (5) include: The extruded composite cable is immediately placed into a circulating water tank with a water temperature of 20°C to 40°C for rapid cooling.