A low crosstalk composite shielded high speed ethernet cable and method of making same

By partitioning and controlling the surface of aromatic organic pigments and titanium dioxide, the problem of inconsistent cell morphology and dielectric properties of the insulating core wire caused by different pigments was solved, and stable transmission performance of low crosstalk composite shielded high-speed Ethernet cable was achieved.

CN123120419APending Publication Date: 2026-11-17HANGZHOU LINAN GUANGDA CABLE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611619582.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-10-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

When using different pigments to identify the core wires in existing skin-foam-skin polyethylene insulated high-speed Ethernet cables, the differences in the surface properties, particle size, and dispersion state of the pigments lead to fluctuations in the pore morphology, equivalent dielectric properties, and electrical balance of the insulated core wires, affecting propagation delay and crosstalk performance.

Method used

By partitioning and surface-tuning aromatic organic pigments and titanium dioxide, long-chain alkyl interfaces are formed on the polyethylene side. Combined with the same polyethylene base material and basic nucleation system, the dispersion of cell structure and dielectric properties between different colored insulating cores and along the length direction is reduced.

Benefits of technology

It reduces the differences in cell density, size, and morphology between insulated cores of different colors and along the same core length, thereby reducing the dispersion of the equivalent dielectric constant and capacitance per unit length, reducing propagation delay difference and capacitance imbalance to ground, and reducing return loss and crosstalk performance fluctuations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application provides a low-crosstalk composite shielding high-speed Ethernet cable and a preparation method thereof, and belongs to the technical field of cables. In view of the problem that the differences in surface properties of different pigments interfere with polyethylene crystallization and foaming nucleation, and cause the fluctuations of the cell morphology, dielectric properties and electrical balance of the colored insulating core wires, the aromatic organic pigments are treated by using a pyrene-based long-chain alkyl interface regulator, and the titanium dioxide is treated by using octadecyl phosphonic acid, so that the long-chain alkyl interfaces of the two types of pigments are formed to face the polyethylene; the same polyethylene base material and calcite type calcium carbonate nucleation system are matched to form a skin-bubble-skin insulating core wire and a cable. The partition anchoring and the common outer interface can effectively weaken the different influences of different pigments on the adsorption, crystallization and cell nucleation of the polyethylene chain segment, reduce the discreteness of the cell structure and dielectric properties of the colored core wires and the length direction thereof, reduce the propagation delay difference and the imbalance of the ground capacitance, and improve the stable margin of the return loss and crosstalk performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of cable technology and relates to a low crosstalk composite shielded high-speed Ethernet cable and its preparation method. Background Technology

[0002] High-speed Ethernet cables typically consist of insulated cores, stranded pairs, a shield, and a sheath. As transmission frequencies increase, in addition to conductor resistance and shielding integrity, the impedance, propagation delay, and uniformity of capacitance to ground of each insulated core also affect return loss and crosstalk performance. Sheet-foam-sheet polyethylene insulation, by incorporating a foam layer between the solid inner and outer sheaths, reduces the equivalent dielectric constant of the insulation while maintaining surface integrity and mechanical strength, thus making it suitable for high-speed data communication cables.

[0003] To distinguish different wire pairs and their polarities, insulated core wires are typically marked with colors such as blue, orange, green, brown, and white. The pigments used for these different colors differ in chemical structure, surface properties, particle size, and dispersion state. After entering the polyethylene foam layer, the pigments not only serve a coloring function, but their particle surfaces may also participate in polyethylene crystallization and heterogeneous bubble nucleation. Existing processes typically adjust insulation performance by controlling parameters such as resin ratio, pigment dosage, foaming gas injection amount, extrusion temperature, and foaming degree. However, these adjustments mainly target the average state of the foam layer, making it difficult to eliminate nucleation differences caused by different pigments, and also difficult to ensure foam stability along the length of the same core wire. Composite shielding can suppress electromagnetic interference between wire pairs and from the external environment, but it cannot eliminate electrical imbalances caused by fluctuations in the dielectric properties of the insulation material itself.

[0004] Therefore, the technical problem to be solved in this application is that existing skin-foam-skin polyethylene insulated high-speed Ethernet cables require the use of different colored pigments to identify the core wires. The surface properties, particle size and dispersion state of different pigments have different effects on the polyethylene foaming nucleation system, making it difficult to maintain the effective nucleation density, cell size and longitudinal and transverse morphology of the insulated core wires of different colors under the same extrusion conditions. This directly causes fluctuations in the equivalent dielectric properties and electrical balance between different core wires and in the same core wire length direction, thereby increasing the propagation delay difference and ground capacitance imbalance, and compressing the stability margin of return loss and crosstalk performance. Summary of the Invention

[0005] The purpose of this invention is to provide a low-crosstalk composite shielded high-speed Ethernet cable and its preparation method. Addressing the issue that different colored pigments have varying surface properties, effective particle size due to agglomeration, and dispersion states, resulting in different effects on polyethylene crystallization and foaming nucleation, and consequently causing fluctuations in the cell morphology, equivalent dielectric properties, and electrical balance of the insulated cores of different colors, this invention reduces the dispersion of cell structure and dielectric properties between different colored insulated cores and along their length by using a partitioned surface control of aromatic organic pigments and titanium dioxide. This ensures that different types of colorants have long-chain alkyl interfaces on the polyethylene-facing side, and by using the same polyethylene base material and basic nucleation system.

[0006] To achieve this objective, the present invention adopts the following technical solution: In a first aspect, the present invention provides a low crosstalk composite shielded high-speed Ethernet cable, comprising multiple pairs of wires formed by twisting together sheath-foam-sheath polyethylene insulated core wires, each of the wires having a separate shielding layer on the outside, and a total shielding layer and a sheath layer being sequentially provided on the outside of the multiple pairs of wires.

[0007] The sheath-foam-sheath polyethylene insulated core wire includes a conductor and an inner sheath layer, an intermediate foam layer, and an outer sheath layer sequentially disposed on the outside of the conductor. The intermediate foam layer includes polyethylene base material, uncoated calcite-type calcium carbonate, and long-chain alkylated colorant.

[0008] The long-chain alkylated colorant is a long-chain alkylated organic pigment or a long-chain alkylated titanium dioxide. The long-chain alkylated organic pigment is an aromatic organic pigment with an interface modifier containing pyrene and octadecyl groups adsorbed on its surface; the long-chain alkylated titanium dioxide is titanium dioxide with octadecylphosphonic acid loaded on its surface.

[0009] Preferably, the interface modifier is a product obtained by reacting pyrene-1-carboxylic acid with octadecylamine after activation by N,N′-carbonyldiimidazole.

[0010] Preferably, the aromatic organic pigment is selected from at least one of CI Pigment Blue 15:3, CI Pigment Yellow 180 and CI Pigment Orange 73.

[0011] Preferably, the polyethylene base material includes high-density polyethylene and low-density polyethylene, and both the inner skin layer and the outer skin layer include high-density polyethylene.

[0012] Preferably, the sub-shielding layer is an aluminum foil sub-shielding layer, and the total shielding layer includes a total aluminum foil shielding layer and a metal braided shielding layer disposed on the outside of the total aluminum foil shielding layer.

[0013] Secondly, the present invention provides a method for preparing a low-crosstalk composite shielded high-speed Ethernet cable, the method comprising: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran and reacted under nitrogen protection; octadecylamine was added to continue the reaction; after the reaction solution was cooled, anhydrous methanol was added to precipitate the product; the product was filtered, washed with anhydrous methanol and dried under vacuum to obtain the interface regulator. S2: After drying CI pigment blue 15:3, CI pigment yellow 180 and CI pigment orange 73 respectively, they were added to a toluene solution of the interface modifier for treatment. The mother liquor was separated by hot separation, and after washing and vacuum drying, long-chain alkylated pigment blue, long-chain alkylated pigment yellow and long-chain alkylated pigment orange were obtained respectively. S3: After drying, titanium dioxide is added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid for treatment. After filtration and pre-drying, it is heat-treated under vacuum conditions, then washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: The long-chain alkylated pigment blue, long-chain alkylated pigment yellow, long-chain alkylated pigment orange and long-chain alkylated titanium dioxide are melt-mixed with high-density polyethylene to obtain the corresponding color masterbatch; the color masterbatch is mixed with high-density polyethylene, low-density polyethylene and uncoated calcite-type calcium carbonate to obtain a cell layer mixture. S5: High-density polyethylene is used as the inner and outer solid skin layer material, and the foam layer mixture is used as the middle foam layer material for three-layer co-extrusion of skin-foam-skin. Nitrogen gas is injected into the middle foam layer melt and cooled to obtain skin-foam-skin polyethylene insulated core wire. S6: Twist the polyethylene insulated core wires of different colors into pairs, and set an aluminum foil shielding layer on the outside of each wire. Then, bundle the multiple pairs into a cable, and set an aluminum foil shielding layer, a metal braided shielding layer and a sheath layer on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

[0014] Preferably, in step S1, the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole is 1:(1.05-1.10), and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran is 1g:(8-20)mL, and the reaction is carried out under nitrogen protection and at 20-35℃ for 1-3h; the molar ratio of octadecylamine to pyrene-1-carboxylic acid is (1.10-1.15):1, and the reaction is carried out at 55-66℃ for 4-10h after the addition of octadecylamine.

[0015] Preferably, in step S2, the mass ratio of the interface modifier to the corresponding organic pigment is (0.5-5.0):100, the mass-volume ratio of the organic pigment to toluene is 1g:(5-15)mL, the treatment temperature is 70-100℃, and the treatment time is 1-4h.

[0016] Preferably, in step S3, the mass ratio of octadecylphosphonic acid to titanium dioxide is (0.3-3.0):100, the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran is 1g:(3-20)mL, the treatment temperature is 45-60℃, and the treatment time is 2-6h; the heat treatment temperature is 110-140℃, and the time is 1-3h.

[0017] Preferably, in step S4, when preparing the color masterbatch corresponding to the organic pigment, the long-chain alkylated organic pigment is 10-25 parts by mass, the high-density polyethylene is 75-90 parts by mass, and the total amount of the two is 100 parts by mass; when preparing the color masterbatch corresponding to titanium dioxide, the long-chain alkylated titanium dioxide is 25-50 parts by mass, the high-density polyethylene is 50-75 parts by mass, and the total amount of the two is 100 parts by mass; the melting and mixing temperature is 150-180℃.

[0018] Preferably, in step S4, the ingredients are prepared according to a total of 100 parts by mass of all high-density polyethylene and low-density polyethylene, wherein the total high-density polyethylene is 80-95 parts by mass and the low-density polyethylene is 5-20 parts by mass; the total high-density polyethylene includes separately added high-density polyethylene and carrier high-density polyethylene in the color masterbatch; the effective addition amount of the long-chain alkylated organic pigment is 0.05-0.50 parts by mass, or the effective addition amount of the long-chain alkylated titanium dioxide is 0.30-1.50 parts by mass, and the addition amount of uncoated calcite-type calcium carbonate is 0.05-0.20 parts by mass.

[0019] Preferably, in step S5, the temperature of the three-layer co-extrusion of skin-foam-skin is 150-200℃; the mass ratio of nitrogen to the total amount of high-density polyethylene and low-density polyethylene in step S4 is (0.05-0.30):100; the thickness ratio of the inner skin layer, the intermediate foam layer and the outer skin layer is (5-10):(80-90):(5-10), and the foaming degree of the intermediate foam layer is 25-45%.

[0020] Upon contact between the carboxyl group of pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole, an acylimidazole reactive intermediate is formed, releasing carbon dioxide and imidazole. The primary amino group in octadecylamine undergoes nucleophilic attack on the acyl carbon, forming an amide linkage structure via addition and imidazole departure, resulting in an interface modifier possessing pyrene, amide, and octadecyl groups simultaneously. Precipitation and washing separate the imidazole, unreacted octadecylamine, and residual activators from the interface modifier. Vacuum drying limits the entry of moisture and solvents into subsequent pigment processing and the polyethylene melting system.

[0021] CI Pigment Blue 15:3, CI Pigment Yellow 180, and CI Pigment Orange 73 possess conjugated aromatic structures, but their molecular skeletons, crystal stacking methods, and exposed crystal faces differ, resulting in varying effects on the adsorption of polyethylene segments and on crystallization and heterogeneous bubble nucleation. Treating the three organic pigments separately allows the interface modifier to adsorb independently on their respective pigment surfaces, avoiding competitive allocation due to differences in surface adsorption capacity when different pigments coexist. The pyrene group in the interface modifier can approach the conjugated aromatic region on the organic pigment surface and adsorb onto the pigment surface through π-π interactions and dispersion; on exposed crystal faces containing carbonyl groups, nitrogen-containing groups, or other polar sites, the amide group can also participate in hydrogen bonding. The octadecyl group, located away from the pigment surface, tends to enter the non-polar environment composed of polyethylene methylene segments. Hot separation mother liquor can remove unadsorbed interface modifiers from the solution beforehand, reducing the solvent contact required for subsequent washing and thus limiting the desorption of adsorbed interface modifiers into the washing liquid. Washing and vacuum drying further reduce residual mother liquor, free interface modifiers and solvents, so that the interfacial behavior in subsequent melt mixing mainly comes from the adsorption layer retained on the pigment surface.

[0022] Titanium dioxide has hydroxyl groups and coordinatingly unsaturated titanium sites on its surface, and its surface chemistry differs from that of aromatic organic pigments. When octadecylphosphonic acid (OPA) comes into contact with titanium dioxide, phosphonic acid groups can accumulate on the titanium dioxide surface through hydrogen bonding and coordination. Some of these phosphonic acid groups can undergo dehydration bonding with surface hydroxyl groups, forming Ti-OP type surface bonds. Pre-drying reduces the obstruction of excessive physically adsorbed water to the phosphonic acid groups' access to surface sites. Vacuum heat treatment promotes the removal of interfacial water and residual solvent, and further bonds the phosphonic acid groups that can undergo dehydration bonding to the titanium dioxide surface, reducing the desorption of the surface bond layer during subsequent solvent contact and melt shearing processes. The resulting surface layer can contain different coordination forms and uncondensed phosphonic acid groups, and is not limited to a single octagonal structure. Anhydrous methanol washing reduces octadecylphosphonic acid that is not bonded to the titanium dioxide surface, limiting the transfer of free phosphonic acid to the calcite-type calcium carbonate surface during subsequent mixing. The octadecyl groups retained on the titanium dioxide surface are distributed towards the polyethylene phase, resulting in a contact region on the outer side of the titanium dioxide surface dominated by hydrocarbon chains.

[0023] When long-chain alkylated organic pigments and long-chain alkylated titanium dioxide are melt-mixed with high-density polyethylene (HDPE), melt shearing disperses secondary pigment agglomerates and promotes the spread of HDPE melt onto the treated pigment surface. Dispersion occurs between the octadecyl groups on the pigment surface and the methylene segments of the polyethylene, and these segments flow with the melt into the spaces between adjacent segments. This dispersion facilitates the spread of the polyethylene melt on the treated pigment surface and reduces the polarity difference between the pigment surface and the polyethylene phase. Using HDPE as the color masterbatch carrier ensures that the masterbatch, after entering the porous layer matrix composed of HDPE and LPE, does not introduce carrier phases of different chemical types, limiting the formation of polar carrier-rich regions or independent phase regions around the pigment. Different pigments are adsorbed on the inner side by pyrene groups or loaded on the phosphonic acid surface, while the outer side is in contact with polyethylene via octadecyl groups, thus minimizing the differences between organic pigments and titanium dioxide in melt wetting, localized segment adsorption, and interfacial friction.

[0024] High-density polyethylene (HDPE) forms a semi-crystalline continuous phase within the cell layer. The long-branched structure of low-density polyethylene (LDPE) increases the long-term relaxation component in the melt, leading to strain hardening and increased melt strength during tensile flow caused by gas evolution and cell expansion. This limits excessive cell wall thinning and rupture. Nitrogen dissolves and disperses in the pressurized polyethylene melt. After leaving the die, the melt becomes supersaturated due to pressure drop, generating bubble nuclei in localized polymer fluctuation regions and at solid particle interfaces. Uncoated calcite-type calcium carbonate provides heterogeneous nucleation interfaces with similar composition and surface type in each color cell layer. After the original crystal faces of the pigment are partially obscured by the octadecyl-containing surface layer, the direct contact between the pigment core surface and the polyethylene chain segments decreases, thus weakening its color dependence on the polyethylene crystallization initiation position and bubble nucleation position. The relative nucleation contribution of calcite-type calcium carbonate tends to converge in different color systems.

[0025] After cell formation, nitrogen diffuses into the bubble nuclei and promotes cell growth, while the cell walls simultaneously undergo stretching, polyethylene chain segment orientation, and crystallization. As the influence of different pigments on the local crystallization rate and cell wall viscosity decreases, the number of bubble nuclei formed, the gas competition between adjacent bubbles, and the cell wall solidification process in each color system become similar, and the color differences in cell density, cell size, and longitudinal and transverse morphology decrease accordingly. During skin-cell-skin co-extrusion, the inner and outer solid high-density polyethylene layers form boundary constraints on the radial expansion of the intermediate cell layer and limit surface cell rupture and changes in insulation outer diameter during cooling. As the fluctuations in cell nucleation and growth state decrease in the continuous extrusion direction, the range of variation in the local density and gas phase volume fraction of the intermediate cell layer along the core length narrows accordingly.

[0026] The equivalent dielectric properties of the intermediate foam layer depend on the volume distribution, local density, and crystalline state of the polyethylene phase and the foam gas phase. When the differences in foam density, foam size, foaming degree, and crystalline state among the colored core wires decrease, the difference in their equivalent dielectric constant and capacitance per unit length also decreases. When the fluctuations in the foam structure along the length of the same core wire decrease, the sudden changes in local impedance and the resulting signal reflections decrease. The similar dielectric states of the two insulated core wires in a wire pair reduce the capacitance difference between the two conductors and the shielding layer and ground reference surface, limiting the conversion between common mode and differential mode. The reduced difference in propagation speed between different wire pairs reduces the propagation delay difference. The aluminum foil shielding layers on the outer sides of each wire pair limit the extension of the electric field from the wire pair to adjacent wire pairs. The overall aluminum foil shielding layer and the metal braided shielding layer limit the entry of external electromagnetic fields into the cable interior. Under this shielding boundary, the reduction in dielectric fluctuations and electrical imbalances in the insulation layer reduces the fluctuations in echo reflections and crosstalk coupling between wire pairs.

[0027] Compared with the prior art, the beneficial effects of the present invention are as follows: To address the different surface chemical properties of aromatic organic pigments and titanium dioxide, two anchoring pathways are employed: pyrene adsorption and phosphonic acid surface loading. Simultaneously, both types of colorants exhibit an octadecyl interface on the polyethylene side. This reduces the differences in wetting, chain segment adsorption, and interfacial friction of different colored pigments in the polyethylene melt, avoiding the problem of difficulty in simultaneously adapting organic and inorganic pigments using the same surface treatment agent.

[0028] In the interface modifier, the pyrene group is used to adsorb aromatic organic pigments, while the octadecyl group is used to contact polyethylene segments. Octadecylphosphonic acid retains the octadecyl interface by adsorption, coordination, and dehydration of the phosphonic acid group with the titanium dioxide surface. Both treatment methods allow the octadecyl-containing surface layer to partially cover the original exposed crystal faces of the pigment, reducing direct contact between the pigment core surface and the polyethylene segments. This reduces the influence of the original pigment surface state on crystallization and bubble nucleation, weakens the differential interference of different pigments on polyethylene crystallization and heterogeneous bubble nucleation, and makes the relative nucleation contributions of the same calcite-type calcium carbonate in various color systems tend to be similar.

[0029] Once the nucleation sources of different colored foam layers become consistent, the differences in foam density, foam size, longitudinal and transverse morphology, and local foaming degree between different colored insulating cores and along the same core length direction will decrease accordingly. This will reduce the dispersion of equivalent dielectric constant, capacitance per unit length, and impedance, decrease propagation delay difference and ground capacitance imbalance, and reduce echo reflection and crosstalk coupling fluctuations caused by local impedance abrupt changes and electrical imbalance of wire pairs. Detailed Implementation

[0030] The technical solution of the present invention will be described in detail below with reference to specific embodiments. The embodiments described herein are specific implementations of the present invention and are used to illustrate the concept of the present invention; these descriptions are explanatory and exemplary and should not be construed as limiting the implementation of the present invention or the scope of protection of the present invention. In addition to the embodiments described herein, those skilled in the art can also adopt other obvious technical solutions based on the content disclosed in the claims and the specification of this application. These technical solutions include technical solutions that employ any obvious substitutions and modifications made to the embodiments described herein.

[0031] Example 1 This embodiment provides a low-crosstalk composite shielded high-speed Ethernet cable and its manufacturing method. The manufacturing method specifically includes the following steps: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran, wherein the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole was 1:1.05, and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran was 1 g:16 mL. The reaction was carried out under nitrogen protection and at 30 °C for 3 h. Octadecylamine was added, wherein the molar ratio of octadecylamine to pyrene-1-carboxylic acid was 1.10:1, and the reaction was carried out at 55 °C for 8 h. After the reaction solution was cooled, anhydrous methanol was added to precipitate the product. The product was filtered, washed with anhydrous methanol, and dried under vacuum to obtain the interface modifier. S2: Organic pigments CI Pigment Blue 15:3, CI Pigment Yellow 180, and CI Pigment Orange 73 were dried separately and then added to a toluene solution of an interface modifier, wherein the mass ratio of the interface modifier to the corresponding organic pigment was 2.0:100 and the mass-to-volume ratio of the organic pigment to toluene was 1 g:15 mL. The solutions were treated at 80 °C for 1 h. After treatment, the mother liquor was separated by hot separation, washed, and vacuum dried to obtain long-chain alkylated organic pigments, namely long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange. S3: After drying, titanium dioxide was added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid, wherein the mass ratio of octadecylphosphonic acid to titanium dioxide was 3.0:100, and the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran was 1g:8mL. The solution was treated at 50℃ for 5h; after filtration and pre-drying, it was heat-treated at 110℃ under vacuum for 2.5h, then rapidly washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: Long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange are respectively mixed with high-density polyethylene, wherein the long-chain alkylated organic pigment is 10 parts by mass and the high-density polyethylene is 90 parts by mass; long-chain alkylated titanium dioxide is mixed with high-density polyethylene, wherein the long-chain alkylated titanium dioxide is 40 parts by mass and the high-density polyethylene is 60 parts by mass; they are melt-mixed separately at 170°C to obtain the corresponding color masterbatches; the total amount of all high-density polyethylene and low-density polyethylene is 100 parts by mass, wherein all high-density polyethylene is 95 parts by mass and low-density polyethylene is 5 parts by mass; the all high-density polyethylene includes the separately added high-density polyethylene and the carrier high-density polyethylene in the color masterbatch; the color masterbatch is added so that the effective addition amount of long-chain alkylated organic pigment is 0.32 parts by mass, or the effective addition amount of long-chain alkylated titanium dioxide is 1.50 parts by mass, and then 0.10 parts by mass of uncoated calcite-type calcium carbonate is added, and after mixing evenly, a foam layer mixture is obtained; S5: High-density polyethylene is used as the inner and outer solid skin layer material, and the foam layer mixture is used as the intermediate foam layer material for three-layer co-extrusion of skin-foam-skin. The co-extrusion temperature is 165℃. Nitrogen is injected into the intermediate foam layer melt, and the mass ratio of nitrogen to the total amount of high-density polyethylene and low-density polyethylene in S4 is 0.12:100, so that the thickness ratio of the inner skin layer, intermediate foam layer and outer skin layer is 5:85:10. The foaming degree of the intermediate foam layer is controlled to be 32%. After cooling, the skin-foam-skin polyethylene insulated core wire is obtained. S6: Different colored polyethylene insulated core wires are twisted into pairs, and aluminum foil shielding layers are set on the outside of each wire. The multi-component shielded pairs are then cabled, and an overall aluminum foil shielding layer, a metal braided shielding layer, and a sheath layer are set on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

[0032] Example 2 This embodiment provides a low-crosstalk composite shielded high-speed Ethernet cable and its manufacturing method. The manufacturing method specifically includes the following steps: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran, wherein the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole was 1:1.15, and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran was 1 g:8 mL. The reaction was carried out under nitrogen protection and at 25 °C for 2.5 h. Octadecylamine was added, wherein the molar ratio of octadecylamine to pyrene-1-carboxylic acid was 1.12:1. The reaction was carried out at 62 °C for 10 h. After the reaction solution was cooled, anhydrous methanol was added to precipitate the product. The product was filtered, washed with anhydrous methanol, and dried under vacuum to obtain the interface modifier. S2: Organic pigments CI Pigment Blue 15:3, CI Pigment Yellow 180, and CI Pigment Orange 73 were dried separately and then added to a toluene solution of an interface modifier, wherein the mass ratio of the interface modifier to the corresponding organic pigment was 5.0:100 and the mass-to-volume ratio of the organic pigment to toluene was 1 g:8 mL. The solutions were treated at 70 °C for 3 h. After treatment, the mother liquor was separated by hot separation, washed, and vacuum dried to obtain long-chain alkylated organic pigments, namely long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange. S3: After drying, titanium dioxide was added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid, wherein the mass ratio of octadecylphosphonic acid to titanium dioxide was 0.3:100, and the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran was 1g:20mL. The solution was treated at 55℃ for 2h. After filtration and pre-drying, the solution was heat-treated at 130℃ under vacuum for 3h. Then, it was rapidly washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: Long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange are respectively mixed with high-density polyethylene, wherein the long-chain alkylated organic pigment is 25 parts by mass and the high-density polyethylene is 75 parts by mass; long-chain alkylated titanium dioxide is mixed with high-density polyethylene, wherein the long-chain alkylated titanium dioxide is 25 parts by mass and the high-density polyethylene is 75 parts by mass; they are melt-mixed separately at 150°C to obtain the corresponding color masterbatches; the total amount of all high-density polyethylene and low-density polyethylene is 100 parts by mass, wherein all high-density polyethylene is 90 parts by mass and low-density polyethylene is 10 parts by mass; the all high-density polyethylene includes the separately added high-density polyethylene and the carrier high-density polyethylene in the color masterbatch; the color masterbatch is added so that the effective addition amount of long-chain alkylated organic pigment is 0.05 parts by mass, or the effective addition amount of long-chain alkylated titanium dioxide is 0.70 parts by mass, and then 0.20 parts by mass of uncoated calcite-type calcium carbonate is added, and after mixing evenly, a cell layer mixture is obtained; S5: High-density polyethylene is used as the inner and outer solid skin layer material, and the foam layer mixture is used as the intermediate foam layer material for three-layer co-extrusion of skin-foam-skin. The co-extrusion temperature is 185℃. Nitrogen gas is injected into the intermediate foam layer melt, wherein the mass ratio of nitrogen gas to the total amount of high-density polyethylene and low-density polyethylene in S4 is 0.30:100, so that the thickness ratio of the inner skin layer, intermediate foam layer and outer skin layer is 10:85:5, and the foaming degree of the intermediate foam layer is controlled to be 45%. After cooling, the skin-foam-skin polyethylene insulated core wire is obtained. S6: Different colored polyethylene insulated core wires are twisted into pairs, and aluminum foil shielding layers are set on the outside of each wire. The multi-component shielded pairs are then cabled, and an overall aluminum foil shielding layer, a metal braided shielding layer, and a sheath layer are set on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

[0033] Example 3 This embodiment provides a low-crosstalk composite shielded high-speed Ethernet cable and its manufacturing method. The manufacturing method specifically includes the following steps: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran, wherein the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole was 1:1.12, and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran was 1 g:20 mL. The reaction was carried out under nitrogen protection and at 20 °C for 1.5 h. Octadecylamine was added, wherein the molar ratio of octadecylamine to pyrene-1-carboxylic acid was 1.15:1. The reaction was carried out at 58 °C for 4 h. After the reaction solution was cooled, anhydrous methanol was added to precipitate the product. The product was filtered, washed with anhydrous methanol, and dried under vacuum to obtain the interface modifier. S2: Organic pigments CI Pigment Blue 15:3, CI Pigment Yellow 180, and CI Pigment Orange 73 were dried separately and then added to a toluene solution of an interface modifier, wherein the mass ratio of the interface modifier to the corresponding organic pigment was 0.5:100 and the mass-to-volume ratio of the organic pigment to toluene was 1 g:12 mL. The solutions were treated at 100 °C for 2 h. After treatment, the mother liquor was separated by hot separation, washed, and vacuum dried to obtain long-chain alkylated organic pigments, namely long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange. S3: After drying, titanium dioxide was added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid, wherein the mass ratio of octadecylphosphonic acid to titanium dioxide was 1.2:100, and the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran was 1 g:3 mL. The solution was treated at 45 °C for 6 h. After filtration and pre-drying, the solution was heat-treated at 140 °C under vacuum for 1 h, and then rapidly washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: Long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange are respectively mixed with high-density polyethylene, wherein the long-chain alkylated organic pigment is 15 parts by mass and the high-density polyethylene is 85 parts by mass; long-chain alkylated titanium dioxide is mixed with high-density polyethylene, wherein the long-chain alkylated titanium dioxide is 50 parts by mass and the high-density polyethylene is 50 parts by mass; they are melt-mixed separately at 160°C to obtain the corresponding color masterbatches; the total amount of all high-density polyethylene and low-density polyethylene is 100 parts by mass, wherein all high-density polyethylene is 80 parts by mass and low-density polyethylene is 20 parts by mass; the all high-density polyethylene includes the separately added high-density polyethylene and the carrier high-density polyethylene in the color masterbatch; the color masterbatch is added so that the effective addition amount of long-chain alkylated organic pigment is 0.50 parts by mass, or the effective addition amount of long-chain alkylated titanium dioxide is 0.30 parts by mass, and then 0.15 parts by mass of uncoated calcite-type calcium carbonate is added, and after mixing evenly, a foam layer mixture is obtained; S5: High-density polyethylene is used as the inner and outer solid skin material, and the foam layer mixture is used as the intermediate foam layer material for three-layer co-extrusion of skin-foam-skin. The co-extrusion temperature is 150℃. Nitrogen is injected into the intermediate foam layer melt, wherein the mass ratio of nitrogen to the total amount of high-density polyethylene and low-density polyethylene in S4 is 0.05:100, so that the thickness ratio of the inner skin layer, intermediate foam layer and outer skin layer is 10:80:10, and the foaming degree of the intermediate foam layer is controlled to be 25%. After cooling, the skin-foam-skin polyethylene insulated core wire is obtained. S6: Different colored polyethylene insulated core wires are twisted into pairs, and aluminum foil shielding layers are set on the outside of each wire. The multi-component shielded pairs are then cabled, and an overall aluminum foil shielding layer, a metal braided shielding layer, and a sheath layer are set on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

[0034] Example 4 This embodiment provides a low-crosstalk composite shielded high-speed Ethernet cable and its manufacturing method. The manufacturing method specifically includes the following steps: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran, wherein the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole was 1:1.11, and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran was 1 g:12 mL. The reaction was carried out under nitrogen protection and at 35 °C for 1 h. Octadecylamine was added, wherein the molar ratio of octadecylamine to pyrene-1-carboxylic acid was 1.13:1, and the reaction was carried out at 66 °C for 6 h. After the reaction solution was cooled, anhydrous methanol was added to precipitate the product. The product was filtered, washed with anhydrous methanol, and dried under vacuum to obtain the interface modifier. S2: Organic pigments CI Pigment Blue 15:3, CI Pigment Yellow 180, and CI Pigment Orange 73 were dried separately and then added to a toluene solution of an interface modifier, wherein the mass ratio of the interface modifier to the corresponding organic pigment was 3.5:100 and the mass-to-volume ratio of the organic pigment to toluene was 1 g:5 mL. The solutions were treated at 90 °C for 4 h. After treatment, the mother liquor was separated by hot separation, washed, and vacuum dried to obtain long-chain alkylated organic pigments, namely long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange. S3: After drying, titanium dioxide was added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid, wherein the mass ratio of octadecylphosphonic acid to titanium dioxide was 2.1:100, and the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran was 1 g:14 mL. The solution was treated at 60 °C for 3 h. After filtration and pre-drying, the solution was heat-treated at 120 °C under vacuum for 1.5 h. Then, it was rapidly washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: Long-chain alkylated pigment blue, long-chain alkylated pigment yellow, and long-chain alkylated pigment orange are respectively mixed with high-density polyethylene, wherein the long-chain alkylated organic pigment is 20 parts by mass and the high-density polyethylene is 80 parts by mass; long-chain alkylated titanium dioxide is mixed with high-density polyethylene, wherein the long-chain alkylated titanium dioxide is 35 parts by mass and the high-density polyethylene is 65 parts by mass; they are melt-mixed at 180°C to obtain the corresponding color masterbatches; the total amount of all high-density polyethylene and low-density polyethylene is 100 parts by mass, wherein all high-density polyethylene is 85 parts by mass and low-density polyethylene is 15 parts by mass; the all high-density polyethylene includes the separately added high-density polyethylene and the carrier high-density polyethylene in the color masterbatch; the color masterbatch is added so that the effective addition amount of long-chain alkylated organic pigment is 0.18 parts by mass, or the effective addition amount of long-chain alkylated titanium dioxide is 1.10 parts by mass, and then 0.05 parts by mass of uncoated calcite-type calcium carbonate is added, and after mixing evenly, a foam layer mixture is obtained; S5: High-density polyethylene is used as the inner and outer solid skin layer material, and the foam layer mixture is used as the intermediate foam layer material for three-layer co-extrusion of skin-foam-skin. The co-extrusion temperature is 200℃. Nitrogen is injected into the intermediate foam layer melt, wherein the mass ratio of nitrogen to the total amount of high-density polyethylene and low-density polyethylene in S4 is 0.22:100, so that the thickness ratio of the inner skin layer, intermediate foam layer and outer skin layer is 5:90:5, and the foaming degree of the intermediate foam layer is controlled to be 38%. After cooling, the skin-foam-skin polyethylene insulated core wire is obtained. S6: Different colored polyethylene insulated core wires are twisted into pairs, and aluminum foil shielding layers are set on the outside of each wire. The multi-component shielded pairs are then cabled, and an overall aluminum foil shielding layer, a metal braided shielding layer, and a sheath layer are set on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

[0035] Comparative Example 1 This comparative example provides a low crosstalk composite shielded high-speed Ethernet cable and its preparation method. The difference from Example 1 is that no interface modifier is added in S2, CI pigment blue 15:3, CI pigment yellow 180 and CI pigment orange 73 are added to toluene for the same treatment, and in S4, the corresponding organic pigments obtained in S2 are used to replace the long-chain alkylated pigment blue, long-chain alkylated pigment yellow and long-chain alkylated pigment orange by equal mass. Other operation steps and process parameters are exactly the same as in Example 1.

[0036] Comparative Example 2 This comparative example provides a low crosstalk composite shielded high-speed Ethernet cable and its preparation method. The difference from Example 1 is that in S2, an equal mass of octadecylamine is used to replace the interface modifier, and the resulting treated organic pigments are used in S4 to prepare the corresponding color masterbatches. Since the interface modifier is no longer used, S1 is cancelled accordingly. Other operation steps and process parameters are exactly the same as in Example 1.

[0037] Comparative Example 3 This comparative example provides a low crosstalk composite shielded high-speed Ethernet cable and its preparation method. The difference from Example 1 is that no interface modifier is added to toluene in S2. CI pigment blue 15:3, CI pigment yellow 180 and CI pigment orange 73, which have undergone the same treatment, are used in S4 to prepare the corresponding color masterbatches. The interface modifier is added directly during the melting and mixing in S4. The mass ratio of the interface modifier to the corresponding organic pigment is 2.0:100. Other operation steps and process parameters are exactly the same as in Example 1.

[0038] Comparative Example 4 This comparative example provides a low crosstalk composite shielded high-speed Ethernet cable and its preparation method. The difference from Example 1 is that octadecylphosphonic acid is not added in S3, and the titanium dioxide undergoes the same treatment as before. In S4, the long-chain alkylated titanium dioxide is replaced by the same mass of the titanium dioxide obtained in S3. Other operation steps and process parameters are exactly the same as in Example 1.

[0039] Comparative Example 5 This comparative example provides a method for preparing a low crosstalk composite shielded high-speed Ethernet cable. The difference between this method and Example 1 is that after filtration and pre-drying in S3, heat treatment under vacuum conditions is not performed. Instead, the cable is directly washed with anhydrous methanol and dried under vacuum. The resulting long-chain alkylated titanium dioxide is used to prepare the corresponding color masterbatch in S4. Other process parameters and operating conditions are exactly the same as in Example 1.

[0040] The performance of the low crosstalk composite shielded high-speed Ethernet cables of Examples 1-4 and Comparative Examples 1-5 was tested, and the specific process is as follows: Color-to-color crystallization peak temperature range: Tested according to GB / T 19466.3-2025. Blue, yellow, orange, and titanium dioxide colored core wires were cut from three batches of sheath-foam-sheath polyethylene insulated core wires. The conductors and inner and outer solid sheaths were removed, and 6.0±0.5mg samples were cut from the middle foam layer. Three samples of each color were tested. Using a differential scanning calorimeter, with a nitrogen flow rate of 50mL / min, the samples were heated from 25℃ to 200℃ at a rate of 10℃ / min and held for 5min, then cooled to 25℃ at a rate of 10℃ / min. The crystallization peak temperatures of the cooling curves were recorded, and the average values ​​for each color were calculated. The color-to-color crystallization peak temperature range was obtained by subtracting the minimum value from the maximum value. The unit is ℃.

[0041] Extreme differences in cross-sectional cell density between colors: For each example or comparative example, three batches of insulated core wires were taken. From each batch, core wires of four different colors were cut and cross-sectional samples with a thickness of 1.0 mm were prepared. The intermediate cell layer was observed using an optical microscope at 100x magnification. A 0.50 mm × 0.50 mm field of view was selected at 0°, 90°, 180°, and 270° circumference, and the number of cells within each of the four fields of view was counted. The total number of cells was divided by 1.00 mm. 2 The cross-sectional cell number density is obtained, in cells / mm². 2 The average values ​​of three batches of samples for the four coloring systems were calculated respectively, and the maximum value was subtracted from the minimum value to obtain the range of cross-sectional cell density between colors.

[0042] The effective relative permittivity range between colors: For each example or comparative example, three batches of unstranded insulated core wires were taken. From each batch, one segment of each of the four colored core wires was cut, with each segment being 1.20m long. A water electrode test system was constructed using a precision LCR bridge and a sodium chloride aqueous solution with a concentration of 10.0g / L and a temperature of 20±1℃. The capacitances C1 and C2 of the core wires were measured at 1kHz and 1.0V when immersed in the wires for 0.40m and 0.80m, respectively. The capacitance per unit length C′ was calculated as (C2-C1) / 0.40m. The outer diameter D of the insulation and the diameter d of the conductor were measured, and the effective relative permittivity was calculated. The average values ​​for the four coloring systems were calculated, and the effective relative permittivity range between colors was obtained by subtracting the minimum value from the maximum value.

[0043] Impedance range between wire pairs: Tested according to GB / T 18015.1-2017 and GB / T 18015.5-2025. For each embodiment or comparative example, three finished cables with an effective length of 100.0m were used. A time-domain reflectometry (TD-RS) tester with a 100Ω balanced differential port was employed for measurement. The rise time of the differential step signal was 500ps. The far end of the tested wire pair was terminated with a 100Ω differential load. Starting 5m from the nearest end of the cable, one characteristic impedance value was recorded every 1m, ending at 95m. The average characteristic impedance of each wire pair was calculated. The impedance range between wire pairs was obtained by subtracting the minimum value from the maximum value of the average characteristic impedance of the four wire pairs for the same cable. The arithmetic mean of the results for each group of three cables was taken, in Ω.

[0044] Propagation delay difference: Tested according to GB / T 18015.1-2017 and GB / T 18015.5-2025. Three finished cables with an effective length of 100.0m were used in each group. A cable network analyzer with a 100Ω balanced port was used to perform a 1601-point linear frequency sweep within the range of 1MHz to 500MHz, measuring the phase propagation delay of each of the four wire pairs. At each frequency, the delay difference was calculated by subtracting the minimum value from the maximum propagation delay of the four wire pairs, and the maximum value among all sweep points was taken as the propagation delay difference of that cable. The arithmetic mean of the results for each group of three cables was taken, with units of ns / 100m.

[0045] Results of capacitance imbalance to ground: For each group, three finished cables with an effective length of 100.0m were used for testing using a precision LCR bridge at 1kHz and 1.0V. Each shielding layer and the non-tested conductor were connected to the low-potential end of the bridge. The capacitance to ground of each conductor in the same wire pair was measured, and the absolute value of the difference was taken as the capacitance imbalance to ground for that wire pair. This process was repeated for all four wire pairs, and the maximum value was taken as the capacitance imbalance result for that cable. The arithmetic mean of the results for each group of three cables was taken, expressed in pF / 100m.

[0046] Near-end crosstalk minimum test margin and near-end crosstalk power and minimum test margin: Tests were conducted according to GB / T 18015.1-2017 and GB / T 18015.5-2025. Three finished cables with an effective length of 100.0m were used for each group. A multi-port cable network analyzer with a 100Ω balanced differential port was used to perform a 1601-point linear frequency sweep in the range of 1MHz to 500MHz. Each wire pair was terminated with a 100Ω differential load at its far end. Near-end crosstalk was measured from both ends of the cable for six different wire pair combinations formed by four wire pairs. The instrument then summed the near-end crosstalk power of the other three wire pairs corresponding to the same interfered wire pair. The test margin is calculated by subtracting the corresponding frequency limit for Category 6A cables in GB / T 18015.5-2025 from the measured value. The minimum value is taken from all wire pairs, both test ends, and all frequency sweep points to obtain the minimum near-end crosstalk test margin and the near-end crosstalk power and minimum test margin. The arithmetic mean of the results of 3 cables in each group is taken, and the unit is dB.

[0047] The test results are shown in Table 1.

[0048] Table 1: Performance test results of low crosstalk composite shielded high-speed Ethernet cables in Examples 1-4 and Comparative Examples 1-5 As can be seen from the test results of Example 1 and Comparative Example 1 in Table 1, when the organic pigments were not treated with interface modifiers, the original surface polarity, crystal energy and agglomeration tendency of different organic pigments were not regulated by the long-chain alkyl adsorption layer. The differences in their wetting, dispersion and heterogeneous nucleation behavior in polyethylene melt increased, resulting in a greater difference in the crystallization peak temperature between colors and a greater difference in the cross-sectional cell number density between colors. The difference in cell content and distribution of different colored insulating core wires increased the difference in the equivalent relative permittivity between colors, and further increased the difference in impedance between wire pairs, the difference in propagation delay, and the imbalance of capacitance to ground. The minimum test margin for near-end crosstalk and the near-end crosstalk power and minimum test margin decreased accordingly.

[0049] As shown in Table 1, the test results of Example 1 and Comparative Example 2 reveal that when octadecylamine is used as an interface modifier, although it can introduce long-chain alkyl groups, it lacks the pyrene planar structure found in interface modifiers and cannot form the same aromatic conjugated adsorption relationship. Therefore, it is more prone to desorption or migration into the polyethylene continuous phase during melt mixing, resulting in differences in the degree of surface conditioning for different organic pigments. Consequently, the differences in crystallization peak temperature and cross-sectional pore density between colors increase, leading to increased differences in equivalent relative permittivity, impedance between line pairs, propagation delay, and capacitance-to-ground imbalance between colors. This, in turn, reduces the minimum test margin for near-end crosstalk, near-end crosstalk power, and minimum test margin.

[0050] As shown in Table 1, the test results of Example 1 and Comparative Example 3 indicate that when the interface modifier is directly added to the cell layer mixture without pretreatment of the organic pigments, the interface modifier is diluted in the polyethylene melt. Its long-chain alkyl groups tend to enter the polyethylene phase, making it difficult for the interface modifier to preferentially accumulate on the surface of each organic pigment before entering the polyethylene melt. At the same time, the free interface modifier also participates in the crystallization and bubble nucleation process of polyethylene. The surface differences of different organic pigments are therefore not sufficiently mitigated, which increases the difference in crystallization peak temperature between colors and the difference in cross-sectional cell number density between colors. The resulting cell differences increase the difference in equivalent relative permittivity between colors, the difference in impedance between line pairs, the difference in propagation delay, and the imbalance in capacitance to ground, and decrease the minimum test margin for near-end crosstalk, as well as the near-end crosstalk power and the minimum test margin.

[0051] As shown in Table 1, the test results of Example 1 and Comparative Example 4 reveal that without octadecylphosphonic acid treatment, the hydroxyl groups and polar sites on the titanium dioxide surface are directly exposed, resulting in decreased wettability with the non-polar polyethylene melt and increased susceptibility to particle aggregation and local heterogeneous nucleation. This leads to differences in the crystallization, nucleation, and cell growth behaviors between the titanium dioxide coloring system and the organic pigment coloring system. Consequently, the differences in crystallization peak temperature and cross-sectional cell density between colors increase, as does the difference in equivalent relative permittivity between colors. This further increases the differences in impedance between line pairs, propagation delay, and capacitance to ground imbalance, while decreasing the minimum test margin for near-end crosstalk, near-end crosstalk power, and minimum test margin.

[0052] As can be seen from the test results of Example 1 and Comparative Example 5 in Table 1, after the vacuum heat treatment is cancelled, the process of promoting interfacial dehydration and improving the surface layer's resistance to washing and melt shearing by the heat treatment is no longer present. Consequently, the differences in crystallization and foaming between the titanium dioxide coloring system and the organic pigment coloring system increase, making desorption and migration more likely to occur during subsequent washing and melt shearing processes, thus reducing the coverage of long-chain alkyl groups on the titanium dioxide surface. This increased difference in crystallization and foaming between the titanium dioxide coloring system and the organic pigment coloring system manifests as a greater difference in the crystallization peak temperature, the greater difference in cross-sectional cell density, and the greater difference in equivalent relative permittivity between colors. Correspondingly, the differences in impedance between line pairs, the difference in propagation delay, and the imbalance in capacitance to ground increase, while the minimum test margin for near-end crosstalk and the near-end crosstalk power and minimum test margin decrease.

[0053] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A low crosstalk composite shielded high speed Ethernet cable, characterized by, The device comprises multiple pairs of wires formed by stranding polyethylene insulated core wires in a sheath-foam-sheath configuration. Each wire has a separate shielding layer on the outside, and a total shielding layer and a sheath layer are sequentially arranged on the outer sides of the multiple pairs of wires. The intermediate foam layer of the sheath-foam-sheath polyethylene insulated core wire comprises polyethylene base material, uncoated calcite-type calcium carbonate, and long-chain alkylated colorants. The intermediate foam layers of the sheath-foam-sheath polyethylene insulated core wires of different colors contain corresponding long-chain alkylated colorants. The long-chain alkylated colorants include at least aromatic organic pigments with pyrene and octadecyl interface modifiers adsorbed on their surfaces, and titanium dioxide with a surface treatment layer formed by octadecylphosphonic acid bonded to its surface.

2. The low crosstalk, composite shielded, high speed Ethernet cable of claim 1, wherein, The interface modifier is a product obtained by reacting pyrene-1-carboxylic acid with octadecylamine after activation by N,N′-carbonyldiimidazole.

3. The low crosstalk, composite shielded, high speed Ethernet cable of claim 1, wherein, The aromatic organic pigment is selected from at least one of CI Pigment Blue 15:3, CI Pigment Yellow 180 and CI Pigment Orange 73.

4. The low crosstalk, composite shielded, high speed Ethernet cable of claim 1, wherein, The polyethylene base material includes high-density polyethylene and low-density polyethylene, and both the inner and outer sheaths of the sheath-foam-sheath polyethylene insulated core wire include high-density polyethylene.

5. The low crosstalk, composite shielded, high speed Ethernet cable of claim 1, wherein, The sub-shielding layer is an aluminum foil sub-shielding layer, and the total shielding layer includes a total aluminum foil shielding layer and a metal braided shielding layer disposed on the outside of the total aluminum foil shielding layer.

6. A method of making a low crosstalk, composite shielded high speed Ethernet cable as claimed in any one of claims 1-5, characterized in that, Includes the following steps: S1: Pyrene-1-carboxylic acid and N,N′-carbonyldiimidazole were added to anhydrous tetrahydrofuran and reacted under nitrogen protection; octadecylamine was added to continue the reaction; after the reaction solution was cooled, anhydrous methanol was added to precipitate the product; the product was filtered, washed with anhydrous methanol and dried under vacuum to obtain the interface regulator. S2: After drying CI pigment blue 15:3, CI pigment yellow 180 and CI pigment orange 73 respectively, they were added to a toluene solution of the interface modifier for treatment. The mother liquor was separated by hot separation, and after washing and vacuum drying, long-chain alkylated pigment blue, long-chain alkylated pigment yellow and long-chain alkylated pigment orange were obtained respectively. S3: After drying, titanium dioxide is added to an anhydrous tetrahydrofuran solution of octadecylphosphonic acid for treatment. After filtration and pre-drying, it is heat-treated under vacuum conditions, then washed with anhydrous methanol and vacuum dried to obtain long-chain alkylated titanium dioxide. S4: The long-chain alkylated pigment blue, long-chain alkylated pigment yellow, long-chain alkylated pigment orange and long-chain alkylated titanium dioxide are melt-mixed with high-density polyethylene to obtain the corresponding color masterbatch; the color masterbatch is mixed with high-density polyethylene, low-density polyethylene and uncoated calcite-type calcium carbonate to obtain a cell layer mixture. S5: High-density polyethylene is used as the inner and outer solid skin layer material, and the foam layer mixture is used as the middle foam layer material for three-layer co-extrusion of skin-foam-skin. Nitrogen gas is injected into the middle foam layer melt and cooled to obtain skin-foam-skin polyethylene insulated core wire. S6: Twist the polyethylene insulated core wires of different colors into pairs, and set an aluminum foil shielding layer on the outside of each wire. Then, bundle the multiple pairs into a cable, and set an aluminum foil shielding layer, a metal braided shielding layer and a sheath layer on the outside in sequence to obtain a low crosstalk composite shielded high-speed Ethernet cable.

7. The preparation method according to claim 6, characterized in that, In step S1, the molar ratio of pyrene-1-carboxylic acid to N,N′-carbonyldiimidazole is 1:(1.05-1.10), and the mass-to-volume ratio of pyrene-1-carboxylic acid to anhydrous tetrahydrofuran is 1g:(8-20)mL. The reaction is carried out under nitrogen protection and at 20-35℃ for 1-3h. The molar ratio of octadecylamine to pyrene-1-carboxylic acid is (1.10-1.15):

1. After the addition of octadecylamine, the reaction is carried out at 55-66℃ for 4-10h.

8. The preparation method according to claim 6, characterized in that, In step S2, the mass ratio of the interface modifier to the corresponding organic pigment is (0.5-5.0):100, the mass-volume ratio of the organic pigment to toluene is 1g:(5-15)mL, the treatment temperature is 70-100℃, and the treatment time is 1-4h.

9. The preparation method according to claim 6, characterized in that, In step S3, the mass ratio of octadecylphosphonic acid to titanium dioxide is (0.3-3.0):100, the mass-volume ratio of titanium dioxide to anhydrous tetrahydrofuran is 1g:(3-20)mL, the treatment temperature is 45-60℃, and the treatment time is 2-6h; the heat treatment temperature is 110-140℃, and the time is 1-3h.

10. The preparation method according to claim 6, characterized in that, In step S4, when preparing the color masterbatches corresponding to each organic pigment, the long-chain alkylated pigment blue, long-chain alkylated pigment yellow, or long-chain alkylated pigment orange is 10-25 parts by mass, and high-density polyethylene is 75-90 parts by mass, with the total amount of both being 100 parts by mass; when preparing the color masterbatches corresponding to titanium dioxide, the long-chain alkylated titanium dioxide is 25-50 parts by mass, and high-density polyethylene is 50-75 parts by mass, with the total amount of both being 100 parts by mass; when preparing the above color masterbatches, the melting and mixing temperature is 150-180℃.