A high-temperature resistant insulating enameled wire and its preparation method

By coating the surface of the conductor with polyimide varnish and wrapping it with aramid fiber, then impregnating it with epoxy resin to form a nylon layer and a polyamide layer, and then fusing the layers through a stepped heating sintering process, the problems of insulation peeling, insufficient corona resistance and insufficient mechanical strength of traditional enameled wires under high temperature environments are solved, and the high adhesion, corona resistance and mechanical strength are improved.

CN123120437APending Publication Date: 2026-11-17GUANGDONG JINGXUN LIYA SPECIAL WIRE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611319768.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-08-28
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Traditional enameled wires suffer from problems such as easy peeling of the insulation varnish layer, insufficient corona resistance, insufficient mechanical strength, and susceptibility to internal defects under high-temperature environments.

Method used

The process involves coating the surface of the conductor with polyimide varnish and wrapping it with aramid fiber, then impregnating it with epoxy resin to form a nylon layer and a polyamide layer. The layers are then fused together using a stepped heating sintering process. The combination of silane coupling agent and nano-inorganic filler enhances the interlayer adhesion and thermal conductivity.

Benefits of technology

It improves interlayer adhesion, corona resistance, and mechanical strength, avoids internal defects, and meets the high-temperature requirements of new energy vehicles and high-end industrial motors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention discloses a high-temperature resistant insulated enameled wire and its preparation method, relating to the field of enameled wire technology. The method includes: coating the surface of a conductor with polyimide varnish and drying it to form a polyimide varnish layer; wrapping aramid fibers around the outside of the polyimide varnish layer and impregnating it with epoxy resin; sequentially coating the outside of the aramid fibers with nylon and polyamide materials to form nylon and polyamide layers respectively; and subjecting the coated conductor to high-temperature sintering to fuse the coating layers and wrapping layers, forming the high-temperature resistant insulated enameled wire. This method, through multi-layer insulation structure composite and high-temperature sintering, ensures tight bonding between the layers, effectively improving the high-temperature resistance and insulation reliability of the enameled wire.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of enameled wire technology, specifically to a high-temperature resistant insulating enameled wire and its preparation method. Background Technology

[0002] Enameled wire is one of the main winding materials widely used in motors, transformers, electrical appliances, and electronic equipment. With the rapid development of new energy vehicles (especially 800V and above high-voltage platforms), wind power generation, solar energy equipment, and high-end industrial motors, extremely stringent requirements have been placed on the high-temperature resistance, corona resistance, mechanical strength, and service life of enameled wire.

[0003] Traditional enameled wires typically use a single insulating varnish coating for insulation. However, in high-temperature operating environments (above 200°C), they exhibit the following significant problems: First, due to the difference in thermal expansion coefficients between the metal conductor and the insulating varnish layer, frequent thermal expansion and contraction can easily cause the varnish layer to peel off from the conductor. Second, in high-frequency, high-voltage environments (such as variable frequency motors), the corona resistance and thermal conductivity of traditional polyimide and other insulating varnishes are insufficient, easily leading to localized overheating and corona breakdown. Third, the mechanical strength and abrasion resistance of a single varnish layer or simple fiber wrapping structure are insufficient, making it prone to fiber breakage or varnish layer scratches during automated high-speed winding processes. Fourth, traditional high-temperature sintering processes often involve heating to extremely high temperatures in a single step, which can cause severe evaporation of the solvent inside the insulation layer, resulting in microcracks or bubbles and creating a potential for insulation failure.

[0004] Therefore, developing a method for preparing high-temperature insulating enameled wires that combines excellent interlayer adhesion, high corona resistance, ultra-high mechanical strength, and dense, defect-free properties has become a pressing technical problem to be solved in this field. Summary of the Invention

[0005] The purpose of this invention is to provide a solution to the technical problems mentioned in the background section.

[0006] To achieve the above objectives, the present invention provides the following technical solution: A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: A polyimide varnish is coated onto the surface of the conductor and dried to form a polyimide varnish layer; Aramid fibers are wrapped around the outside of the polyimide coating and impregnated with epoxy resin; A nylon material is coated on the outer side of the aramid fiber to form a nylon layer; A polyamide material is coated on the outside of the nylon layer to form a polyamide layer; The coated conductor is subjected to high-temperature sintering to fuse the coating layers and the wrapping layer, forming the high-temperature resistant insulated enameled wire.

[0007] Preferably, the conductor is a copper conductor; Before coating the surface of the conductor with polyimide varnish, the process also includes an annealing and softening treatment of the conductor.

[0008] After the annealing and softening treatment and before applying the polyimide varnish, the method further includes a step of coating the surface of the conductor with a silane coupling agent to form an interfacial bonding transition layer.

[0009] Preferably, the polyimide paint is a modified polyimide paint doped with nano-inorganic fillers; Preferably, the nano-inorganic filler is one or more of nano-boron nitride, nano-alumina, or nano-silica, and its mass accounts for 1% to 5% of the total mass of the polyimide paint; Preferably, when forming the polyimide paint layer, the thickness of the polyimide paint layer is controlled to be 0.1 to 0.2 mm.

[0010] Preferably, when wrapping aramid fibers around the outside of the polyimide coating, a double-layer reverse cross-wrapping process is adopted, with the inner aramid fibers and the outer aramid fibers wrapped in opposite directions.

[0011] Preferably, when coating the outer side of the aramid fiber with nylon material, the coated nylon material is impregnated with epoxy resin. The thickness of the nylon layer is 0.1 to 0.3 mm.

[0012] Preferably, the thickness of the polyamide layer is 0.05 to 0.15 mm.

[0013] Preferably, when forming the nylon layer and the polyamide layer, each layer of material is individually baked and dried after coating.

[0014] Preferably, the high-temperature sintering employs a stepped heating sintering process, comprising the following steps: The first preheating stage involves maintaining a temperature of 200–250℃. The second curing stage, maintained at 280–320℃; and The third fusion stage involves heat preservation at 350–400℃.

[0015] A high-temperature resistant insulating enameled wire is prepared by the method described above.

[0016] Compared with the prior art, the beneficial effects of the present invention are: 1. A silane coupling agent is introduced into the interfacial bonding transition layer between the conductor and the polyimide enamel layer. Through chemical bonding, the interlayer adhesion is greatly improved, effectively solving the problem of insulation layer peeling off the enameled wire under high temperature above 200℃ and severe thermal expansion and contraction conditions.

[0017] 2. By uniformly doping nano-inorganic fillers into the polyimide coating, the thermal conductivity of the insulation layer is not only significantly improved, which can quickly dissipate the heat of the conductor, but also the corona breakdown resistance is significantly enhanced, perfectly meeting the stringent requirements of 800V high-voltage platform motors for new energy vehicles.

[0018] 3. The double-layer reverse cross-wrapping process is adopted, which enables the aramid fibers to form a self-locking mesh reinforcement skeleton inside the insulation layer, fundamentally eliminating the phenomenon of fiber stranding and greatly improving the tensile and abrasion resistance of the enameled wire in the high-speed automated winding assembly process.

[0019] 4. A three-stage stepped heating sintering process of preheating, curing, and fusing is adopted to avoid the violent evaporation of internal solvents caused by a one-time high-temperature impact. The tiny bubbles in the insulation system are slowly expelled, ultimately forming an extremely dense, micro-crack-free integrated insulation structure, which greatly extends the service life of the enameled wire. Detailed Implementation

[0020] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0021] Example 1 A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: Oxygen-free copper rods for electrical applications were continuously drawn into round copper wires with a diameter of 1.0 mm using multiple drawing dies. The copper wires were placed in a tubular annealing furnace, and high-purity nitrogen (≥99.99%) was introduced as a protective atmosphere. The temperature was increased to 350℃ at a rate of 5℃ / min, and held for annealing for 2 hours to fully soften the copper wires and eliminate processing stress. After annealing, the wires were cooled to room temperature in the furnace and then removed for use. γ-aminopropyltriethoxysilane (KH-550) was dissolved in a mixed solvent of water and anhydrous ethanol (water to ethanol volume ratio 1:1) to form a 2% (w / w) solution. The pH of the solution was adjusted to 4.5 with glacial acetic acid, and the solution was hydrolyzed and stirred at room temperature for 30 min to obtain the silane coupling agent working solution. The annealed copper wires were immersed in the above working solution using the dip-coating method for 10 minutes. The pulling speed was controlled at 23 mm / s. After being taken out, the wires were placed in a forced-air drying oven and dried at 100°C for 10 minutes to form a silane coupling agent interfacial bonding transition layer with a thickness of about 12 μm on the surface of the copper wires.

[0022] A modified polyimide varnish doped with nano-inorganic fillers was coated onto the surface of a copper conductor forming an interfacial bonding transition layer and then dried to form a polyimide varnish layer. A homopolymer polyimide varnish with a solid content of 20% (solvent: N-methylpyrrolidone) was selected. Nano-boron nitride powder with a particle size of 30-80 nm was added to the varnish at a ratio of 4% of the total mass of the polyimide varnish. The mixture was first pre-dispersed at 2000 r / min for 20 min using a high-speed disperser, and then ground three times using a three-roll mill to ensure that the nano-fillers were evenly distributed in the varnish without agglomeration. A vertical coating machine is used for coating, with 10 coats applied. After each coat, the coating passes through a 6m long vertical baking oven. The oven temperature is divided into three zones: 200℃ at the entrance, 250℃ in the middle, and 280℃ at the exit. The line speed is 8m / min. Each coat forms a paint film with a thickness of approximately 0.018mm. After 10 coats, the total thickness of the polyimide paint layer is approximately 0.18mm, forming a dense and uniform nano-modified polyimide paint layer.

[0023] Aramid fibers are wrapped around the outer side of the polyimide varnish layer using a double-layer reverse cross-wrapping process, with the inner and outer aramid fibers wrapped in opposite directions. Para-aramid fibers with a linear density of 22.2 dtex (heat resistance ≥427℃) are selected and wrapped on a horizontal double-head wrapping machine. The first layer is wrapped in a left-handed direction at a wrapping angle of 30°, with an overlap of 55%. The second layer is wrapped in a right-handed direction in the opposite direction to the first layer at a wrapping angle of 35°, with an overlap of 55%. The total overlap of the two layers is approximately 80%, forming a tightly interlocked mesh structure. During the wrapping process, the aramid fibers first pass through an impregnation tank filled with a high-temperature modified bisphenol A epoxy resin impregnation solution with a glass transition temperature ≥220℃ for 2 seconds. This allows the epoxy resin to fully penetrate into the fiber bundle and the interface between the fiber and the varnish layer, ensuring a strong bond between the aramid fiber layer and the polyimide varnish layer. The impregnation solution is prepared as follows: Bisphenol A type epoxy resin (epoxy value 0.5 eq / 100g) and o-cresol formaldehyde type multifunctional epoxy resin (epoxy value 0.45 eq / 100g) are mixed at a mass ratio of 7:3. 4,4'-diaminodiphenyl sulfone (DDS) is added as an aromatic amine high-temperature curing agent. The amount of curing agent is calculated based on 90% of the epoxy equivalent stoichiometry. The solution is diluted with acetone to a solid content of 40% and a viscosity of 800 mPa·s. After curing, the glass transition temperature of the system is ≥220℃.

[0024] A nylon material impregnated with epoxy resin is coated onto the outer side of the aramid fiber to form a nylon layer with a thickness of 0.25 mm. High-temperature resistant nylon (PA46) powder with a melting point of 260℃ is selected and mixed with the aforementioned high-temperature resistant modified epoxy resin at a mass ratio of 7:3. An appropriate amount of N-methylpyrrolidone solvent is added to prepare a slurry with a solid content of 35%. This slurry is uniformly coated onto the outer surface of the aramid fiber layer using a scraping method. After coating, the nylon layer is baked in an oven at 200℃ for 15 minutes to allow the solvent to fully evaporate and the nylon layer to initially cure. Then, a polyamide material is coated onto the outer side of the nylon layer to form a polyamide layer with a thickness of 0.12 mm. The polyamide material is a semi-aromatic polyamide (PA6T / 6I copolymer, melting point ≥295℃). It is dissolved in m-cresol solvent to prepare a solution with a solid content of 25%. It is uniformly coated on the outer surface of the nylon layer by scraping. After coating, it is placed in a baking oven and baked at 230℃ for 15 minutes to completely remove the solvent and cure the polyamide layer into a film.

[0025] The coated wires are subjected to stepped heating sintering to fully fuse the coating layers and wrapping layers, forming an integrated high-temperature resistant insulated enameled wire. The enameled wire is then fed into a programmable sintering furnace and sintered according to the following three-stage process: First, the preheating stage involves heating from room temperature to 220°C at a rate of 2°C / min and holding for 0.5 hours to allow residual solvents in each layer to slowly evaporate and avoid rapid heating that could generate bubbles; Second, the curing stage involves heating to 300°C at a rate of 2°C / min and holding for 0.5 hours to allow the epoxy resin to fully cross-link and cure, and the chemical bonding reaction between each layer to be basically completed; Third, the fusion stage involves heating to 380°C at a rate of 3°C / min and holding for 1 hour to allow the polyimide enamel layer, aramid fiber layer, nylon layer, and polyamide layer to fully fuse and penetrate at the interface, forming a dense, microcrack-free integrated insulation layer structure. After sintering, the wire is slowly cooled to room temperature in the furnace at a rate not exceeding 5℃ / min, and then removed to obtain the finished high-temperature resistant insulated enameled wire.

[0026] Example 2 A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: Oxygen-free copper rods for electrical applications were continuously drawn into round copper wires with a diameter of 1.0 mm using multiple drawing dies. The copper wires were placed in a tubular annealing furnace, and high-purity nitrogen (≥99.99%) was introduced as a protective atmosphere. The temperature was increased to 350℃ at a rate of 5℃ / min, and held for annealing for 2 hours to fully soften the copper wires and eliminate processing stress. After annealing, the wires were cooled to room temperature in the furnace and then removed for use. γ-aminopropyltriethoxysilane (KH-550) was dissolved in a mixed solvent of water and anhydrous ethanol (water to ethanol volume ratio 1:1) to form a 2% (w / w) solution. The pH of the solution was adjusted to 4.5 with glacial acetic acid, and the solution was hydrolyzed and stirred at room temperature for 30 min to obtain the silane coupling agent working solution. The annealed copper wires were immersed in the above working solution using the dip-coating method for 10 minutes. The pulling speed was controlled at 23 mm / s. After being taken out, the wires were placed in a forced-air drying oven and dried at 100°C for 10 minutes to form a silane coupling agent interfacial bonding transition layer with a thickness of about 12 μm on the surface of the copper wires.

[0027] A modified polyimide varnish doped with nano-inorganic fillers was coated onto the surface of a copper conductor forming an interfacial bonding transition layer and then dried to form a polyimide varnish layer. A homopolymer polyimide varnish with a solid content of 20% (solvent: N-methylpyrrolidone) was selected. Nano-boron nitride powder with a particle size of 30-80 nm was added to the varnish at a ratio of 2% of the total mass of the polyimide varnish. The mixture was first pre-dispersed at 2000 r / min for 20 min using a high-speed disperser, and then ground three times using a three-roll mill to ensure that the nano-fillers were evenly distributed in the varnish without agglomeration. A vertical coating machine is used for coating, with 10 coats applied. After each coat, the coating passes through a 6m long vertical baking oven. The oven temperature is divided into three zones: 200℃ at the entrance, 250℃ in the middle, and 280℃ at the exit. The line speed is 8m / min. Each coat forms a paint film with a thickness of approximately 0.012mm. After 10 coats, the total thickness of the polyimide paint layer is approximately 0.12mm, forming a dense and uniform nano-modified polyimide paint layer.

[0028] Aramid fibers are wrapped around the outer side of the polyimide varnish layer using a double-layer reverse cross-wrapping process, with the inner and outer aramid fibers wrapped in opposite directions. Para-aramid fibers with a linear density of 22.2 dtex (heat resistance ≥427℃) are selected and wrapped on a horizontal double-head wrapping machine. The first layer is wrapped in a left-handed direction at a wrapping angle of 30°, with an overlap of 55%. The second layer is wrapped in a right-handed direction in the opposite direction to the first layer at a wrapping angle of 35°, with an overlap of 55%. The total overlap of the two layers is approximately 80%, forming a tightly interlocked mesh structure. During the wrapping process, the aramid fibers first pass through an impregnation tank filled with a high-temperature modified bisphenol A epoxy resin impregnation solution with a glass transition temperature ≥220℃ for 2 seconds. This allows the epoxy resin to fully penetrate into the fiber bundle and the interface between the fiber and the varnish layer, ensuring a strong bond between the aramid fiber layer and the polyimide varnish layer. The impregnation solution is prepared as follows: Bisphenol A type epoxy resin (epoxy value 0.5 eq / 100g) and o-cresol formaldehyde type multifunctional epoxy resin (epoxy value 0.45 eq / 100g) are mixed at a mass ratio of 7:3. 4,4'-diaminodiphenyl sulfone (DDS) is added as an aromatic amine high-temperature curing agent. The amount of curing agent is calculated based on 90% of the epoxy equivalent stoichiometry. The solution is diluted with acetone to a solid content of 40% and a viscosity of 800 mPa·s. After curing, the glass transition temperature of the system is ≥220℃.

[0029] A nylon material impregnated with epoxy resin is coated onto the outer side of the aramid fiber to form a nylon layer with a thickness of 0.15 mm. High-temperature resistant nylon (PA46) powder with a melting point of 260℃ is selected and mixed with the aforementioned high-temperature resistant modified epoxy resin at a mass ratio of 7:3. An appropriate amount of N-methylpyrrolidone solvent is added to prepare a slurry with a solid content of 35%. This slurry is uniformly coated onto the outer surface of the aramid fiber layer using a scraping method. After coating, the nylon layer is baked in an oven at 200℃ for 15 minutes to allow the solvent to fully evaporate and the nylon layer to initially cure. Then, a polyamide material is coated onto the outer side of the nylon layer to form a polyamide layer with a thickness of 0.08 mm. The polyamide material is a semi-aromatic polyamide (PA6T / 6I copolymer, melting point ≥295℃). It is dissolved in m-cresol solvent to prepare a solution with a solid content of 25%. It is uniformly coated on the outer surface of the nylon layer by scraping. After coating, it is placed in a baking oven and baked at 230℃ for 15 minutes to completely remove the solvent and cure the polyamide layer into a film.

[0030] The coated wires are subjected to stepped heating sintering to fully fuse the coating layers and wrapping layers, forming an integrated high-temperature resistant insulated enameled wire. The enameled wire is then fed into a programmable sintering furnace and sintered according to the following three-stage process: First, the preheating stage involves heating from room temperature to 220°C at a rate of 2°C / min and holding for 0.5 hours to allow residual solvents in each layer to slowly evaporate and avoid rapid heating that could generate bubbles; Second, the curing stage involves heating to 300°C at a rate of 2°C / min and holding for 0.5 hours to allow the epoxy resin to fully cross-link and cure, and the chemical bonding reaction between each layer to be basically completed; Third, the fusion stage involves heating to 380°C at a rate of 3°C / min and holding for 1 hour to allow the polyimide enamel layer, aramid fiber layer, nylon layer, and polyamide layer to fully fuse and penetrate at the interface, forming a dense, microcrack-free integrated insulation layer structure. After sintering, the wire is slowly cooled to room temperature in the furnace at a rate not exceeding 5℃ / min, and then removed to obtain the finished high-temperature resistant insulated enameled wire.

[0031] Example 3 A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: Oxygen-free copper rods for electrical applications were continuously drawn into round copper wires with a diameter of 1.0 mm using multiple drawing dies. The copper wires were placed in a tubular annealing furnace, and high-purity nitrogen (≥99.99%) was introduced as a protective atmosphere. The temperature was increased to 350℃ at a rate of 5℃ / min, and held for annealing for 2 hours to fully soften the copper wires and eliminate processing stress. After annealing, the wires were cooled to room temperature in the furnace and then removed for use. γ-aminopropyltriethoxysilane (KH-550) was dissolved in a mixed solvent of water and anhydrous ethanol (water to ethanol volume ratio 1:1) to form a 2% (w / w) solution. The pH of the solution was adjusted to 4.5 with glacial acetic acid, and the solution was hydrolyzed and stirred at room temperature for 30 min to obtain the silane coupling agent working solution. The annealed copper wires were immersed in the above working solution using the dip-coating method for 10 minutes. The pulling speed was controlled at 23 mm / s. After being taken out, the wires were placed in a forced-air drying oven and dried at 100°C for 10 minutes to form a silane coupling agent interfacial bonding transition layer with a thickness of about 12 μm on the surface of the copper wires.

[0032] A modified polyimide varnish doped with nano-inorganic fillers was coated onto the surface of a copper conductor forming an interfacial bonding transition layer and then dried to form a polyimide varnish layer. A homopolymer polyimide varnish with a solid content of 20% (solvent: N-methylpyrrolidone) was selected. Nano-boron nitride powder with a particle size of 30-80 nm was added to the varnish at a ratio of 3% of the total mass of the polyimide varnish. The mixture was first pre-dispersed at 2000 r / min for 20 min using a high-speed disperser, and then ground three times using a three-roll mill to ensure that the nano-fillers were evenly distributed in the varnish without agglomeration. A vertical coating machine is used for coating, with 10 coats applied. After each coat, the coating passes through a 6m long vertical baking oven. The oven temperature is divided into three zones: 200℃ at the entrance, 250℃ in the middle, and 280℃ at the exit. The line speed is 8m / min. Each coat forms a paint film with a thickness of approximately 0.015mm. After 10 coats, the total thickness of the polyimide paint layer is approximately 0.15mm, forming a dense and uniform nano-modified polyimide paint layer.

[0033] Aramid fibers are wrapped around the outer side of the polyimide varnish layer using a double-layer reverse cross-wrapping process, with the inner and outer aramid fibers wrapped in opposite directions. Para-aramid fibers with a linear density of 22.2 dtex (heat resistance ≥427℃) are selected and wrapped on a horizontal double-head wrapping machine. The first layer is wrapped in a left-handed direction at a wrapping angle of 30°, with an overlap of 55%. The second layer is wrapped in a right-handed direction in the opposite direction to the first layer at a wrapping angle of 35°, with an overlap of 55%. The total overlap of the two layers is approximately 80%, forming a tightly interlocked mesh structure. During the wrapping process, the aramid fibers first pass through an impregnation tank filled with a high-temperature modified bisphenol A epoxy resin impregnation solution with a glass transition temperature ≥220℃ for 2 seconds. This allows the epoxy resin to fully penetrate into the fiber bundle and the interface between the fiber and the varnish layer, ensuring a strong bond between the aramid fiber layer and the polyimide varnish layer. The impregnation solution is prepared as follows: Bisphenol A type epoxy resin (epoxy value 0.5 eq / 100g) and o-cresol formaldehyde type multifunctional epoxy resin (epoxy value 0.45 eq / 100g) are mixed at a mass ratio of 7:3. 4,4'-diaminodiphenyl sulfone (DDS) is added as an aromatic amine high-temperature curing agent. The amount of curing agent is calculated based on 90% of the epoxy equivalent stoichiometry. The solution is diluted with acetone to a solid content of 40% and a viscosity of 800 mPa·s. After curing, the glass transition temperature of the system is ≥220℃.

[0034] A nylon material impregnated with epoxy resin is coated onto the outer side of the aramid fiber to form a nylon layer with a thickness of 0.2 mm. High-temperature resistant nylon (PA46) powder with a melting point of 260℃ is selected and mixed with the aforementioned high-temperature resistant modified epoxy resin at a mass ratio of 7:3. An appropriate amount of N-methylpyrrolidone solvent is added to prepare a slurry with a solid content of 35%. This slurry is uniformly coated onto the outer surface of the aramid fiber layer using a scraping method. After coating, the nylon layer is baked in an oven at 200℃ for 15 minutes to allow the solvent to fully evaporate and the nylon layer to initially cure. Then, a polyamide material is coated onto the outer side of the nylon layer to form a polyamide layer with a thickness of 0.1 mm. The polyamide material is a semi-aromatic polyamide (PA6T / 6I copolymer, melting point ≥295℃). It is dissolved in m-cresol solvent to prepare a solution with a solid content of 25%. It is uniformly coated on the outer surface of the nylon layer by scraping. After coating, it is placed in a baking oven and baked at 230℃ for 15 minutes to completely remove the solvent and cure the polyamide layer into a film.

[0035] The coated wires are subjected to stepped heating sintering to fully fuse the coating layers and wrapping layers, forming an integrated high-temperature resistant insulated enameled wire. The enameled wire is then fed into a programmable sintering furnace and sintered according to the following three-stage process: First, the preheating stage involves heating from room temperature to 220°C at a rate of 2°C / min and holding for 0.5 hours to allow residual solvents in each layer to slowly evaporate and avoid rapid heating that could generate bubbles; Second, the curing stage involves heating to 300°C at a rate of 2°C / min and holding for 0.5 hours to allow the epoxy resin to fully cross-link and cure, and the chemical bonding reaction between each layer to be basically completed; Third, the fusion stage involves heating to 380°C at a rate of 3°C / min and holding for 1 hour to allow the polyimide enamel layer, aramid fiber layer, nylon layer, and polyamide layer to fully fuse and penetrate at the interface, forming a dense, microcrack-free integrated insulation layer structure. After sintering, the wire is slowly cooled to room temperature in the furnace at a rate not exceeding 5℃ / min, and then removed to obtain the finished high-temperature resistant insulated enameled wire.

[0036] Example 4 A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: Oxygen-free copper rods for electrical applications were continuously drawn into round copper wires with a diameter of 1.0 mm using multiple drawing dies. The copper wires were placed in a tubular annealing furnace, and high-purity nitrogen (≥99.99%) was introduced as a protective atmosphere. The temperature was increased to 350℃ at a rate of 5℃ / min, and held for annealing for 2 hours to fully soften the copper wires and eliminate processing stress. After annealing, the wires were cooled to room temperature in the furnace and then removed for use. γ-aminopropyltriethoxysilane (KH-550) was dissolved in a mixed solvent of water and anhydrous ethanol (water to ethanol volume ratio 1:1) to form a 2% (w / w) solution. The pH of the solution was adjusted to 4.5 with glacial acetic acid, and the solution was hydrolyzed and stirred at room temperature for 30 min to obtain the silane coupling agent working solution. The annealed copper wires were immersed in the above working solution using the dip-coating method for 10 minutes. The pulling speed was controlled at 23 mm / s. After being taken out, the wires were placed in a forced-air drying oven and dried at 100°C for 10 minutes to form a silane coupling agent interfacial bonding transition layer with a thickness of about 12 μm on the surface of the copper wires.

[0037] A modified polyimide varnish doped with nano-inorganic fillers was coated onto the surface of a copper conductor forming an interfacial bonding transition layer and then dried to form a polyimide varnish layer. A homopolymer polyimide varnish with a solid content of 20% (solvent: N-methylpyrrolidone) was selected. Nano-boron nitride powder with a particle size of 30-80 nm was added to the varnish at a ratio of 5% of the total mass of the polyimide varnish. The mixture was first pre-dispersed at 2000 r / min for 20 min using a high-speed disperser, and then ground three times using a three-roll mill to ensure that the nano-fillers were evenly distributed in the varnish without agglomeration. A vertical coating machine is used for coating, with 10 coats applied. After each coat, the coating passes through a 6m long vertical baking oven. The oven temperature is divided into three zones: 200℃ at the entrance, 250℃ in the middle, and 280℃ at the exit. The line speed is 8m / min. Each coat forms a paint film with a thickness of approximately 0.02mm. After 10 coats, the total thickness of the polyimide paint layer is approximately 0.2mm, forming a dense and uniform nano-modified polyimide paint layer.

[0038] Aramid fibers are wrapped around the outer side of the polyimide varnish layer using a double-layer reverse cross-wrapping process, with the inner and outer aramid fibers wrapped in opposite directions. Para-aramid fibers with a linear density of 22.2 dtex (heat resistance ≥427℃) are selected and wrapped on a horizontal double-head wrapping machine. The first layer is wrapped in a left-handed direction at a wrapping angle of 30°, with an overlap of 55%. The second layer is wrapped in a right-handed direction in the opposite direction to the first layer at a wrapping angle of 35°, with an overlap of 55%. The total overlap of the two layers is approximately 80%, forming a tightly interlocked mesh structure. During the wrapping process, the aramid fibers first pass through an impregnation tank filled with a high-temperature modified bisphenol A epoxy resin impregnation solution with a glass transition temperature ≥220℃ for 2 seconds. This allows the epoxy resin to fully penetrate into the fiber bundle and the interface between the fiber and the varnish layer, ensuring a strong bond between the aramid fiber layer and the polyimide varnish layer. The impregnation solution is prepared as follows: Bisphenol A type epoxy resin (epoxy value 0.5 eq / 100g) and o-cresol formaldehyde type multifunctional epoxy resin (epoxy value 0.45 eq / 100g) are mixed at a mass ratio of 7:3. 4,4'-diaminodiphenyl sulfone (DDS) is added as an aromatic amine high-temperature curing agent. The amount of curing agent is calculated based on 90% of the epoxy equivalent stoichiometry. The solution is diluted with acetone to a solid content of 40% and a viscosity of 800 mPa·s. After curing, the glass transition temperature of the system is ≥220℃.

[0039] A nylon material impregnated with epoxy resin is coated onto the outer side of the aramid fiber to form a nylon layer with a thickness of 0.3 mm. High-temperature resistant nylon (PA46) powder with a melting point of 260℃ is selected and mixed with the aforementioned high-temperature resistant modified epoxy resin at a mass ratio of 7:3. An appropriate amount of N-methylpyrrolidone solvent is added to prepare a slurry with a solid content of 35%. This slurry is uniformly coated onto the outer surface of the aramid fiber layer using a scraping method. After coating, the nylon layer is baked in an oven at 200℃ for 15 minutes to allow the solvent to fully evaporate and the nylon layer to initially cure. Then, a polyamide material is coated onto the outer side of the nylon layer to form a polyamide layer with a thickness of 0.15 mm. The polyamide material is a semi-aromatic polyamide (PA6T / 6I copolymer, melting point ≥295℃). It is dissolved in m-cresol solvent to prepare a solution with a solid content of 25%. It is uniformly coated on the outer surface of the nylon layer by scraping. After coating, it is placed in a baking oven and baked at 230℃ for 15 minutes to completely remove the solvent and cure the polyamide layer into a film.

[0040] The coated wires are subjected to stepped heating sintering to fully fuse the coating layers and wrapping layers, forming an integrated high-temperature resistant insulated enameled wire. The enameled wire is then fed into a programmable sintering furnace and sintered according to the following three-stage process: First, the preheating stage involves heating from room temperature to 250°C at a rate of 2°C / min and holding for 0.5 hours to allow residual solvents in each layer to slowly evaporate and avoid rapid heating that could generate bubbles; Second, the curing stage involves heating to 320°C at a rate of 2°C / min and holding for 0.5 hours to allow the epoxy resin to fully cross-link and cure, and the chemical bonding reaction between each layer to be basically completed; Third, the fusion stage involves heating to 400°C at a rate of 3°C / min and holding for 1 hour to allow the polyimide enamel layer, aramid fiber layer, nylon layer, and polyamide layer to fully fuse and penetrate at the interface, forming a dense, microcrack-free integrated insulation layer structure. After sintering, the wire is slowly cooled to room temperature in the furnace at a rate not exceeding 5℃ / min, and then removed to obtain the finished high-temperature resistant insulated enameled wire.

[0041] Example 5 A method for preparing a high-temperature resistant insulating enameled wire includes the following steps: Oxygen-free copper rods for electrical applications were continuously drawn into round copper wires with a diameter of 1.0 mm using multiple drawing dies. The copper wires were placed in a tubular annealing furnace, and high-purity nitrogen (≥99.99%) was introduced as a protective atmosphere. The temperature was increased to 350℃ at a rate of 5℃ / min, and held for annealing for 2 hours to fully soften the copper wires and eliminate processing stress. After annealing, the wires were cooled to room temperature in the furnace and then removed for use. γ-aminopropyltriethoxysilane (KH-550) was dissolved in a mixed solvent of water and anhydrous ethanol (water to ethanol volume ratio 1:1) to form a 2% (w / w) solution. The pH of the solution was adjusted to 4.5 with glacial acetic acid, and the solution was hydrolyzed and stirred at room temperature for 30 min to obtain the silane coupling agent working solution. The annealed copper wires were immersed in the above working solution using the dip-coating method for 10 minutes. The pulling speed was controlled at 23 mm / s. After being taken out, the wires were placed in a forced-air drying oven and dried at 100°C for 10 minutes to form a silane coupling agent interfacial bonding transition layer with a thickness of about 12 μm on the surface of the copper wires.

[0042] A modified polyimide varnish doped with nano-inorganic fillers was coated onto the surface of a copper conductor forming an interfacial bonding transition layer and then dried to form a polyimide varnish layer. A homopolymer polyimide varnish with a solid content of 20% (solvent: N-methylpyrrolidone) was selected. Nano-boron nitride powder with a particle size of 30-80 nm was added to the varnish at a ratio of 1% of the total mass of the polyimide varnish. The mixture was first pre-dispersed at 2000 r / min for 20 min using a high-speed disperser, and then ground three times using a three-roll mill to ensure that the nano-fillers were evenly distributed in the varnish without agglomeration. A vertical coating machine is used for coating, with 10 coats. After each coat, the coating passes through a 6m long vertical baking oven. The oven temperature is divided into three zones: 200℃ at the entrance, 250℃ in the middle, and 280℃ at the exit. The line speed is 8m / min. Each coat forms a paint film with a thickness of about 0.01mm. After 10 coats, the total thickness of the polyimide paint layer is about 0.1mm, forming a dense and uniform nano-modified polyimide paint layer.

[0043] Aramid fibers are wrapped around the outer side of the polyimide varnish layer using a double-layer reverse cross-wrapping process, with the inner and outer aramid fibers wrapped in opposite directions. Para-aramid fibers with a linear density of 22.2 dtex (heat resistance ≥427℃) are selected and wrapped on a horizontal double-head wrapping machine. The first layer is wrapped in a left-handed direction at a wrapping angle of 30°, with an overlap of 55%. The second layer is wrapped in a right-handed direction in the opposite direction to the first layer at a wrapping angle of 35°, with an overlap of 55%. The total overlap of the two layers is approximately 80%, forming a tightly interlocked mesh structure. During the wrapping process, the aramid fibers first pass through an impregnation tank filled with a high-temperature modified bisphenol A epoxy resin impregnation solution with a glass transition temperature ≥220℃ for 2 seconds. This allows the epoxy resin to fully penetrate into the fiber bundle and the interface between the fiber and the varnish layer, ensuring a strong bond between the aramid fiber layer and the polyimide varnish layer. The impregnation solution is prepared as follows: Bisphenol A type epoxy resin (epoxy value 0.5 eq / 100g) and o-cresol formaldehyde type multifunctional epoxy resin (epoxy value 0.45 eq / 100g) are mixed at a mass ratio of 7:3. 4,4'-diaminodiphenyl sulfone (DDS) is added as an aromatic amine high-temperature curing agent. The amount of curing agent is calculated based on 90% of the epoxy equivalent stoichiometry. The solution is diluted with acetone to a solid content of 40% and a viscosity of 800 mPa·s. After curing, the glass transition temperature of the system is ≥220℃.

[0044] A nylon material impregnated with epoxy resin is coated onto the outer side of the aramid fiber to form a nylon layer with a thickness of 0.1 mm. High-temperature resistant nylon (PA46) powder with a melting point of 260℃ is selected and mixed with the aforementioned high-temperature resistant modified epoxy resin at a mass ratio of 7:3. An appropriate amount of N-methylpyrrolidone solvent is added to prepare a slurry with a solid content of 35%. This slurry is uniformly coated onto the outer surface of the aramid fiber layer using a scraping method. After coating, the nylon layer is baked in an oven at 200℃ for 15 minutes to allow the solvent to fully evaporate and the nylon layer to initially cure. Then, a polyamide material is coated onto the outer side of the nylon layer to form a polyamide layer with a thickness of 0.05 mm. The polyamide material is a semi-aromatic polyamide (PA6T / 6I copolymer, melting point ≥295℃). It is dissolved in m-cresol solvent to prepare a solution with a solid content of 25%. It is uniformly coated on the outer surface of the nylon layer by scraping. After coating, it is placed in a baking oven and baked at 230℃ for 15 minutes to completely remove the solvent and cure the polyamide layer into a film.

[0045] The coated wires are subjected to stepped heating sintering to fully fuse the coating layers and wrapping layers, forming an integrated high-temperature resistant insulated enameled wire. The enameled wire is then fed into a programmable sintering furnace and sintered according to the following three-stage process: First, the preheating stage involves heating from room temperature to 200°C at a rate of 2°C / min and holding for 0.5 hours to allow residual solvents in each layer to slowly evaporate and avoid rapid heating that could generate bubbles; Second, the curing stage involves heating to 280°C at a rate of 2°C / min and holding for 0.5 hours to allow the epoxy resin to fully cross-link and cure, and the chemical bonding reaction between each layer to be basically completed; Third, the fusion stage involves heating to 350°C at a rate of 3°C / min and holding for 1 hour to allow the polyimide enamel layer, aramid fiber layer, nylon layer, and polyamide layer to fully fuse and penetrate at the interface, forming a dense, microcrack-free integrated insulation layer structure. After sintering, the wire is slowly cooled to room temperature in the furnace at a rate not exceeding 5℃ / min, and then removed to obtain the finished high-temperature resistant insulated enameled wire.

[0046] Comparative Example 1: The only difference from Example 4 is that no silane coupling agent is coated on the surface of the copper conductor, i.e. no interfacial bonding transition layer is formed. The modified polyimide varnish is directly coated on the surface of the annealed copper conductor. All other steps and parameters are the same as in Example 4.

[0047] Comparative Example 2: The only difference from Example 4 is that the polyimide paint does not contain nano boron nitride filler, and unmodified pure homophenylene polyimide paint is used for coating. All other steps and parameters are the same as in Example 4.

[0048] Comparative Example 3: The only difference from Example 4 is that the aramid fiber is wrapped using a conventional single-layer unidirectional wrapping process instead of a double-layer reverse cross-wrapping process. All other steps and parameters are the same as in Example 4.

[0049] Comparative Example 4: The only difference from Example 4 is that the step heating process is not used during high-temperature sintering. Instead, the temperature is directly raised from room temperature to 400°C in one go at a rate of 5°C / min and held for 1 hour. All other steps and parameters are the same as in Example 4.

[0050] Comparative Example 5: The only difference from Example 4 is that the nylon layer is not coated; that is, the polyamide layer is directly coated on the outside of the aramid fiber wrapping layer. All other steps and parameters are the same as in Example 4.

[0051] Comparative Example 6: The only difference from Example 4 is that the outermost polyamide layer is not coated, that is, the nylon layer is used as the outermost layer and high-temperature sintering is carried out directly. The other steps and parameters are the same as those in Example 4.

[0052] Performance testing (1) Breakdown voltage test: In accordance with the provisions of GB / T 4074.5-2024 "Test methods for winding wires - Part 5: Electrical properties", two enameled wire samples were tightly twisted into a twisted pair according to the specified method. The two ends of the twisted pair were connected to the high voltage end and the low voltage end of the withstand voltage tester, respectively. The voltage was uniformly increased at a rate of 500V / s at room temperature. The voltage value (unit: kV) when the enamel film breaks down was recorded. Five samples were tested in each group, and the arithmetic mean was taken as the breakdown voltage.

[0053] (2) Abrasion resistance test (number of reciprocating scraping): Refer to the provisions of GB / T 4074.3-2024 "Test methods for winding wires - Part 3: Mechanical properties" regarding the scraping resistance test. Fix the enameled wire sample on the reciprocating scraping test device. Use a steel needle with a diameter of 0.6 mm to reciprocate scraping the surface of the enamel film under a constant load of 450 g. The scraping stroke is 20 mm and the reciprocating speed is 60 times / min. The number of reciprocating strokes (unit: times) when the enamel film is scratched and becomes conductive with the conductor is used as the abrasion resistance index. Five samples are tested in each group, and the arithmetic mean is taken.

[0054] (3) Adhesion test (elongation at break): Refer to the provisions of GB / T 4074.3-2024 "Test methods for winding wires - Part 3: Mechanical properties" regarding the rapid break test. Take a 500mm long enameled wire sample and conduct a rapid break test on a universal tensile testing machine at a tensile speed of 50mm / min. Record the elongation at break (unit: %) and observe whether the enamel film cracks or peels off at the break and within 10mm of it. Test 5 samples in each group and take the arithmetic mean.

[0055] (4) Corona resistance life test: Two enameled wire samples are prepared into twisted pair samples according to the method specified in IEC 60851-5, placed in a constant temperature chamber, and a bipolar pulse voltage with a frequency of 1kHz and a peak value of 1.5kVp is applied at an ambient temperature of 220℃. The time from the start of voltage application to the insulation breakdown of the enamel film (unit: h) is recorded as the corona resistance life.

[0056] (5) Insulation resistance test after thermal aging: In accordance with the provisions of GB / T 4074.5-2024 "Test methods for winding wires - Part 5: Electrical properties", the enameled wire sample was placed in a constant temperature aging chamber and aged continuously at 240℃ for 500 hours. After that, the sample was taken out and the insulation resistance value (unit: MΩ·km) of the sample was measured at room temperature using a megohmmeter (with 500V DC voltage applied). Three samples were tested in each group and the arithmetic mean was taken.

[0057] (6) Observation of the density of the insulation layer cross section: The enameled wire sample was cut into a cross section perpendicular to the axis. After being potted with epoxy resin and polished, the cross section morphology of the insulation layer was observed under a scanning electron microscope (SEM) at a magnification of 500x. The number of microcracks and bubbles observed in the cross section was recorded (unit: number / mm). 2 The average value of the observation results from the three cross-sections is taken.

[0058] Table 1 Comparing the comparative examples with Example 4 reveals the following: In Comparative Example 1, after removing the silane coupling agent transition layer, the tensile elongation at break decreased significantly from 33.7% to 21.6%, a reduction of 36%, indicating that the silane coupling agent transition layer plays a crucial role in improving interlayer adhesion; In Comparative Example 2, without nano-boron nitride doping, the corona resistance lifetime plummeted from 538h to 87h, a reduction of 84%, and the breakdown voltage also decreased by approximately 30%, fully demonstrating the decisive contribution of nano-modification to corona resistance performance; In Comparative Example 3, after replacing the double-layer reverse cross-wrapping with unidirectional wrapping, the number of reciprocating paint scraping cycles decreased from 126 to 68, a reduction of 46%, indicating that the self-locking mesh structure formed by the double-layer reverse cross-wrapping is the core process for improving mechanical wear resistance; In Comparative Example 4, after one-time heating and sintering, the cross-sectional micro-defect density increased from 0 to 5.8 defects / mm². 2 After thermal aging, the insulation resistance also decreased significantly, verifying the irreplaceable role of the stepped heating sintering process in eliminating internal bubbles and microcracks. After removing the nylon layer in Comparative Example 5, the number of reciprocating paint scrapings and the elongation at break under high tension both decreased significantly, and a small number of micro-defects appeared in the cross-section, indicating that the nylon layer is indispensable for enhancing the overall mechanical strength and structural integrity. After removing the polyamide outer layer in Comparative Example 6, the number of reciprocating paint scrapings decreased significantly, and the wear resistance was obviously insufficient, indicating that the polyamide outer layer, as the outermost protective barrier, is crucial to the wear and scratch resistance of the enameled wire.

[0059] Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the essence and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A method for preparing a high-temperature resistant insulating enameled wire, characterized in that, Includes the following steps: A polyimide varnish is coated onto the surface of the conductor and dried to form a polyimide varnish layer; Aramid fibers are wrapped around the outside of the polyimide coating and impregnated with epoxy resin; A nylon material is coated on the outer side of the aramid fiber to form a nylon layer; A polyamide material is coated on the outside of the nylon layer to form a polyamide layer; The coated conductor is subjected to high-temperature sintering to fuse the coating layers and the wrapping layer, forming the high-temperature resistant insulated enameled wire.

2. The preparation method according to claim 1, characterized in that, The conductor is a copper conductor; Before coating the surface of the conductor with polyimide varnish, the method further includes an annealing and softening treatment of the conductor. After the annealing and softening treatment and before applying the polyimide varnish, the method further includes a step of coating the surface of the conductor with a silane coupling agent to form an interfacial bonding transition layer.

3. The preparation method according to claim 1, characterized in that, The polyimide paint is a modified polyimide paint doped with nano-inorganic fillers.

4. The preparation method according to claim 3, characterized in that, The nano-inorganic filler is one or more of nano-boron nitride, nano-alumina, or nano-silica, and its mass accounts for 1% to 5% of the total mass of the polyimide paint; Preferably, when forming the polyimide paint layer, the thickness of the polyimide paint layer is controlled to be 0.1 to 0.2 mm.

5. The preparation method according to claim 1, characterized in that, When wrapping aramid fibers around the outside of the polyimide coating, a double-layer reverse cross-wrapping process is adopted, with the inner aramid fibers and the outer aramid fibers wrapped in opposite directions.

6. The preparation method according to claim 1, characterized in that, When coating the outer side of the aramid fiber with nylon material, the coated nylon material is impregnated with epoxy resin; The thickness of the nylon layer is 0.1 to 0.3 mm.

7. The preparation method according to claim 1, characterized in that, The thickness of the polyamide layer is 0.05 to 0.15 mm.

8. The preparation method according to claim 1, characterized in that, During the formation of the nylon layer and the polyamide layer, each layer of material is individually baked and dried after coating.

9. The preparation method according to claim 1, characterized in that, The high-temperature sintering adopts a stepped heating sintering process, which includes the following steps: The first preheating stage involves maintaining a temperature of 200–250℃. The second curing stage involves maintaining a temperature of 280–320℃. And the third fusion stage, which involves heat preservation at 350–400°C.

10. A high-temperature resistant insulating enameled wire, characterized in that, It is prepared by the method described in any one of claims 1 to 9 above.